Solid-phase welding forming method for T-shaped structure
The bottom plate and vertical plate are assembled into a diffusion blank through solid-state welding technology, and welded in hot isostatic pressing equipment to form a T-shaped structure. This solves the problems of low material utilization and high equipment loss in the existing technology, and achieves efficient production. and cost reduction.
Patent Information
- Application Number
- CN202410964408.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-15
AI Technical Summary
The existing T-shaped structure preparation method has low material utilization rate and causes high losses to tools and equipment.
The bottom plate, vertical plate, first side plate and second side plate are assembled to form a diffusion blank. The T-shaped structure is formed by heating and applying air pressure in a hot isostatic pressing equipment through solid-phase welding technology, and the preset dimensions are obtained through machining. products.
It improves material utilization, reduces the loss of tools and equipment, improves production efficiency, and reduces production costs.
Smart Images

Figure CN118768706A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal forming, and more particularly to a T-shaped structure solid phase welding forming method. Background Art
[0002] A certain type of titanium alloy aviation component is shown in the figure. Its shape is long and narrow, and its cross section is "T" shaped. Figure 1 At present, the manufacturing of this component mainly adopts CNC machining of titanium alloy thick plates, that is, using a plate with a thickness of not less than L (unit: mm), using a high-pressure water machine or a sawing machine to cut it into a rectangle of L×h, and then using a CNC machining center to process it into a T-shaped cross-section component. The material utilization rate of the mechanical processing process is low. At the same time, because titanium alloy is a material that is difficult to process, a large amount of mechanical processing consumes a lot of tools and equipment. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] The technical problem to be solved by the present invention is that the existing method for preparing a T-shaped structure has a low material utilization rate and causes great loss to cutting tools and equipment.
[0005] (II) Technical solution
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] The present invention provides a T-shaped structure solid phase welding forming method, which is used for diffusion welding a vertically arranged bottom plate and a vertical plate to form a T-shaped structure. The T-shaped structure solid phase welding forming method comprises the following steps:
[0008] S1. Prepare a bottom plate, a vertical plate, a first side plate, and a second side plate, and assemble the first side plate, the second side plate, the bottom plate, and the vertical plate to form a blank with a rectangular outer contour, wherein the contact surface between the bottom plate and the vertical plate is set as a welding area, the contact surface between the first side plate and the bottom plate and the vertical plate, and the contact surface between the second side plate and the bottom plate and the vertical plate are set as non-welding areas, and solder stopper is coated on the surface of the non-welding area;
[0009] S2, sealing and welding the peripheral gap of the blank and evacuating the blank to form at least one diffusion blank;
[0010] S3, placing the at least one diffusion blank into a hot isostatic pressing device, heating it to a preset temperature, and applying equal gas pressure to the diffusion blank in a circumferential direction, so that the bottom plate and the vertical plate are diffusion welded to form a T-shaped structure;
[0011] S4. After cooling to room temperature, removing the first side panel and the second side panel to obtain the T-shaped structure.
[0012] Preferably, there are a plurality of diffusion blanks, and the plurality of diffusion blanks are stacked and assembled to form a diffusion blank group with a rectangular outer contour, and a release agent is coated on the contact surfaces of two adjacent diffusion blanks;
[0013] The diffusion blank group is placed in a hot isostatic pressing device, heated to a preset temperature, and an equal gas pressure is applied to the diffusion blank group in a circumferential direction, so that the bottom plate and the vertical plate are diffusion welded to form a T-shaped structure.
[0014] Preferably, the diffusion blank group is placed on a graphite plate with a flat surface, and then the diffusion blank group and the graphite plate are placed together in a hot isostatic pressing device.
[0015] Preferably, the method further comprises the following steps:
[0016] S5. Machining the T-shaped structure to obtain a T-shaped structure with a preset size.
[0017] Preferably, the material of the first side panel, the material of the second side panel, the material of the bottom panel, and the material of the vertical panel are the same.
[0018] Preferably, the material of the first side plate, the material of the second side plate, the material of the bottom plate and the material of the vertical plate are all titanium alloy.
[0019] Preferably, the first side plate and the second side plate are made of a first material, the bottom plate and the vertical plate are made of a second material, and the first material and the second material are heterogeneous materials having the same thermal expansion coefficient.
[0020] Preferably, the method further comprises the following steps:
[0021] S6, assembling the removed first side panel and the second side panel with another bottom panel and another vertical panel to form a blank with a rectangular outer contour, and then repeating steps S2 to S4.
[0022] Preferably, before step S1, the first side panel, the second side panel, the bottom panel and the vertical panel are pickled using an acid solution, and after the pickling is completed, the first side panel, the second side panel, the bottom panel and the vertical panel are cleaned and dried.
[0023] Preferably, a cone-head milling cutter is used to perform milling along the centers of the welds of the diffusion blank to remove the first side plate and the second side plate to obtain the T-shaped structure.
[0024] (III) Beneficial effects
[0025] The above technical solution of the present invention has at least the following advantages:
[0026] ① The present invention uses a bottom plate, a vertical plate, a first side plate and a second side plate to form a diffusion blank. The first side plate and the second side plate are used to compensate for the T-shaped structure to form a rectangular diffusion blank, so that the rectangular diffusion blank can be uniformly pressed for solid phase welding, which greatly improves the material utilization rate compared with the mechanical processing technology in the prior art;
[0027] ② The welding connection area of the present invention is set as the thickness area of the vertical edge, which is conducive to the bottom edge bearing pressure. At the same time, the welding area is small, and the welding quality of the welding area is easy to ensure;
[0028] ③ The rectangular packaging batching method of the present invention can weld dozens to hundreds of blanks at one time on the platform in the gas pressure furnace, with high production efficiency;
[0029] ④ The first side panel and the second side panel can be reused, further reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 It is a schematic diagram of the structural assembly of a diffusion blank provided in an embodiment of the present invention.
[0032] Figure 2 It is a process flow chart of a T-shaped structure solid phase welding forming method provided by an embodiment of the present invention.
[0033] Figure 3 It is a schematic structural diagram of a diffusion blank group provided in an embodiment of the present invention.
[0034] Figure 4 It is a schematic diagram of the dimensions of the T-shaped structure provided in an embodiment of the present invention.
[0035] Figure 5 It is a schematic diagram of the dimensions of the vertical plate provided in an embodiment of the present invention.
[0036] Figure 6 It is a schematic diagram of the dimensions of the base plate provided in an embodiment of the present invention.
[0037] Figure 7 It is a schematic diagram of the dimensions of the first side panel and the second side panel provided in an embodiment of the present invention.
[0038] The reference numerals in the figures are:
[0039] 10. T-shaped structure; 1. bottom plate; 2. vertical plate; 3. first side plate; 4. second side plate; 5. diffusion blank; 6. graphite plate. DETAILED DESCRIPTION
[0040] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0041] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly located on the other element or indirectly located on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element.
[0042] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention, and do not indicate that a device or element must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0043] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating relative importance or indicating the number of technical features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The specific implementation of the present invention is described in more detail below in conjunction with specific embodiments:
[0044] like Figure 1 and Figure 2 As shown, an embodiment of the present invention provides a T-shaped structure solid phase welding forming method, which is used to diffusely weld a vertically arranged bottom plate 1 and a vertical plate 2 to form a T-shaped structure 10. The T-shaped structure solid phase welding forming method includes the following steps:
[0045] S1, prepare the bottom plate 1, the vertical plate 2, the first side plate 3 and the second side plate 4 (such as Figure 2 a), and assemble the first side panel 3, the second side panel 4, the bottom panel 1 and the vertical panel 2 to form a blank with a rectangular outer contour (as shown in FIG. Figure 2b, c), wherein the contact surface between the bottom plate 1 and the vertical plate 2 is set as a welding area, the contact surface between the first side plate 3 and the bottom plate 1 and the vertical plate 2, and the contact surface between the second side plate 4 and the bottom plate 1 and the vertical plate 2 are set as non-welding areas, and a solder stopper (preferably a boron nitride solution) is coated on the surface of the non-welding area; the first side plate 3 and the second side plate 4 can compensate the outer contour of the T-shaped structure formed by the assembly of the bottom plate 1 and the vertical plate 2 into a rectangle to prevent the bottom plate 1 from being compressed and unstable at high temperatures. Specifically, the thickness of the bottom plate 1 is b, the thickness of the vertical plate 2 is a, the thickness of the first side plate 3 and the thickness of the second side plate 4 are both c, and the height is d. The height of the rectangular blank formed after assembly is b+d, and the width is 2c+a.
[0046] S2. Seal the gap around the blank and evacuate it (such as Figure 2 d), forming at least one diffusion blank 5;
[0047] S3, placing at least one diffusion blank 5 in a hot isostatic pressing device, heating it to a preset temperature, and applying equal gas pressure to the diffusion blank 5 in a circumferential direction, so that the bottom plate 2 and the vertical plate 3 are diffusion welded to form a T-shaped structure 10 (such as Figure 2 e); applying equal air pressure to the diffusion blank 5 in the circumferential direction to prevent the component from being deformed due to uneven pressure.
[0048] S4, after cooling to room temperature, the first side plate 3 and the second side plate 4 are removed to obtain a T-shaped structure 10 (such as Figure 2 f).
[0049] like Figure 3 As shown, preferably, there are multiple diffusion blanks, and the multiple diffusion blanks 5 are stacked and assembled to form a diffusion blank group with a rectangular outer contour, and a release agent is coated on the contact surfaces of two adjacent diffusion blanks 5;
[0050] The diffusion blank group is placed in a hot isostatic pressing device, heated to a preset temperature, and an equal gas pressure is applied to the diffusion blank group in a circumferential direction, so that the bottom plate 1 and the vertical plate 2 are diffusion welded to form a T-shaped structure 10.
[0051] Diffusion welding technology is a type of solid phase welding technology. Solid phase welding technology is a solid phase welding technology that places closely contacted welded parts in a vacuum or protective gas atmosphere and maintains them at a certain temperature and pressure for a period of time, so that the atoms between the contact surfaces are welded to each other to achieve a reliable connection. This welding technology avoids the change in metal properties at the joint caused by metal melting and the adverse effects of the external environment on the connection interface. The joints obtained using solid phase welding technology have high reliability, good static strength, dynamic strength, thermal stability, etc.
[0052] Preferably, the diffusion blank group is placed on a graphite plate 6 with a flat surface, and then the diffusion blank group and the graphite plate 6 are placed together in a hot isostatic pressing device.
[0053] Preferably, the method further comprises the following steps:
[0054] S5. Machining the T-shaped structure 10 to obtain a T-shaped structure with a preset size.
[0055] Preferably, the material of the first side plate 3 , the material of the second side plate 4 , the material of the bottom plate 1 , and the material of the vertical plate 2 are the same.
[0056] Preferably, the material of the first side plate 3 , the material of the second side plate 4 , the material of the bottom plate 1 , and the material of the vertical plate 2 are all titanium alloy.
[0057] Preferably, the first side plate 3 and the second side plate 4 are made of a first material, the bottom plate 1 and the vertical plate 2 are made of a second material, and the first material and the second material are heterogeneous materials having the same thermal expansion coefficient.
[0058] Preferably, the method further comprises the following steps:
[0059] S6, assemble the disassembled first side panel 3 and second side panel 4 with another bottom panel 1 and another vertical panel 2 to form a blank with a rectangular outer contour, and then repeat steps S2 to S4. It should be noted that the edges of the first side panel 3 and the second side panel 4 with welding-processing are still used as the welding-processing edges of the next batch, and the edges of the first side panel 3 and the second side panel 4 disassembled by machining may have some material loss, and the material of the sealing welding can supplement the loss material during disassembly when the next sealing welding is performed.
[0060] Preferably, before step S1, the first side plate, the second side plate, the bottom plate and the vertical plate are pickled with an acid solution. After the pickling is completed, the first side plate 3, the second side plate 4, the bottom plate 1 and the vertical plate 2 are cleaned and dried.
[0061] Preferably, a cone-head milling cutter is used to perform milling along the centers of the welds of the diffusion blank to remove the first side plate 3 and the second side plate 4 to obtain the T-shaped structure 10 .
[0062] The following are specific embodiments provided by the present invention:
[0063] A solid phase welding test was conducted on a T-shaped structure 10 of an aviation product. The vertical edge thickness of the T-shaped structure 10 was 4 mm, the minimum envelope thickness of the bottom edge was 5 mm, the minimum envelope width of the bottom edge was 36 mm, and the minimum envelope total height of the T-shaped structure 10 was 46 mm. A titanium alloy plate of a bottom plate 1 with a thickness of 6 mm, a first side plate 3 with a thickness of 15 mm, a vertical plate 2 with a thickness of 6 mm, and a second side plate 4 with a thickness of 15 mm was selected for combination. Figure 4 The welding process is as follows:
[0064] 1) Press Figure 5 , Figure 6 , Figure 7 The dimensions shown are respectively processed for the bottom plate 1, the vertical plate 2, the first side plate 3 and the second side plate 4, wherein: Figure 5 is the size of the vertical plate 2, Figure 6 is the size of the base plate 1, Figure 7 is the size of the first side plate 3 and the second side plate 4.
[0065] 2) The processed bottom plate 1, the vertical plate 2, the first side plate 3 and the second side plate 4 are placed in a 1% HF + 2% HNO3 mixed acid solution for cleaning for 10 minutes, and then the surfaces of the bottom plate 1, the vertical plate 2, the first side plate 3 and the second side plate 4 are rinsed with tap water and dried;
[0066] 3) Press Figure 2 The batching method in the invention is to batch the bottom plate 1, the vertical plate 2, the first side plate 3 and the second side plate 4, clamp them with a bow clamp, seal the butt edges with automatic argon arc welding, and weld a titanium alloy ventilation pipe 51 (see FIG. Figure 2 (d));
[0067] 4) Connect the vent pipe 51 to the vacuum pump and start the vacuum pump to evacuate to 1.6×10 -3 Pa, observe the vacuum pump pressure gauge. After a certain period of time (1min), if the vacuum pump pressure gauge pointer does not change significantly, it is considered that the blank cavity has been evacuated to a vacuum state and there is no air leakage in the cavity. Then, the titanium alloy vent pipe is sealed and welded, and the blank making is completed.
[0068] 5) Use a graphite plate 6, the upper surface of which should be smooth and flat, and press 60 groups of diffusion blanks 5 Figure 3 The placement method is to arrange them on the graphite plate 6, apply an isolating agent between two adjacent diffusion blanks, and then place the diffusion blank group and the graphite plate 6 together in a hot isostatic pressing device;
[0069] 6) Start vacuuming and the vacuum degree reaches 1.6×10 -3 Pa, turn on heating, set the target temperature to 980℃, and the heating rate to 60~100℃ / h;
[0070] 7) When the furnace chamber temperature reaches 980°C, turn on the pressurization button, fill with argon gas and pressurize to 150MPa, and keep warm for 1.0h;
[0071] 8) After the holding time is up, the furnace chamber pressure is unloaded to 1 atmosphere, the heating is turned off, and the workpiece is cooled down along with the furnace;
[0072] 9) When the equipment temperature drops below 100°C, open the furnace door to take out the parts;
[0073] 10) Clamp each welded diffusion blank 5 on a milling machine, use a cone-head milling cutter to perform milling along the center of each weld, separate the diffusion blank 5, disassemble the first side plate 3 and the second side plate 4, and obtain a T-shaped test piece;
[0074] 11) The separated first side plate 3 and the second side plate 4 are repeatedly pickled, batched, welded, and placed into the furnace for pressure welding (repeat the above steps) with another bottom plate 1 and another vertical plate 2 to obtain a T-shaped test piece;
[0075] 12) Process the T-shaped component to the final size according to the digital modeling machine.
[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A T-shaped structure solid phase welding forming method, It is characterized in that The method for solid phase welding of a vertically arranged bottom plate and a vertical plate to form a T-shaped structure comprises the following steps: S1. Prepare a bottom plate, a vertical plate, a first side plate, and a second side plate, and assemble the first side plate, the second side plate, the bottom plate, and the vertical plate to form a blank with a rectangular outer contour, wherein the contact surface between the bottom plate and the vertical plate is set as a welding area, the contact surface between the first side plate and the bottom plate and the vertical plate, and the contact surface between the second side plate and the bottom plate and the vertical plate are set as non-welding areas, and solder stopper is coated on the surface of the non-welding area; S2, sealing and welding the peripheral gap of the blank and evacuating the blank to form at least one diffusion blank; S3, placing the at least one diffusion blank into a hot isostatic pressing device, heating it to a preset temperature, and applying equal gas pressure to the diffusion blank in a circumferential direction, so that the bottom plate and the vertical plate are diffusion welded to form a T-shaped structure; S4. After cooling to room temperature, removing the first side panel and the second side panel to obtain the T-shaped structure.
2. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that There are a plurality of diffusion blanks, and the plurality of diffusion blanks are stacked and assembled to form a diffusion blank group with a rectangular outer contour, and a release agent is coated on the contact surfaces of two adjacent diffusion blanks; The diffusion blank group is placed in a hot isostatic pressing device, heated to a preset temperature, and an equal gas pressure is applied to the diffusion blank group in a circumferential direction, so that the bottom plate and the vertical plate are diffusion welded to form a T-shaped structure.
3. The T-shaped structure solid phase welding forming method according to claim 2, It is characterized in that The diffusion blank group is placed on a graphite plate with a flat surface, and then the diffusion blank group and the graphite plate are placed together in a hot isostatic pressing device.
4. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that The following steps are also included: S5. Machining the T-shaped structure to obtain a T-shaped structure with a preset size.
5. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that The material of the first side panel, the material of the second side panel, the material of the bottom panel, and the material of the vertical panel are the same.
6. The T-shaped structure solid phase welding forming method according to claim 5, It is characterized in that The material of the first side plate, the material of the second side plate, the material of the bottom plate and the material of the vertical plate are all titanium alloy.
7. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that The first side plate and the second side plate are made of a first material, the bottom plate and the vertical plate are made of a second material, and the first material and the second material are heterogeneous materials having the same thermal expansion coefficient.
8. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that The following steps are also included: S6, assembling the removed first side panel and the second side panel with another bottom panel and another vertical panel to form a blank with a rectangular outer contour, and then repeating steps S2 to S4.
9. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that Before step S1, the first side panel, the second side panel, the bottom panel and the vertical panel are pickled with an acid solution. After the pickling is completed, the first side panel, the second side panel, the bottom panel and the vertical panel are cleaned and dried.
10. The T-shaped structure solid phase welding forming method according to claim 1, It is characterized in that A cone-head milling cutter is used to perform milling along the centers of the welds of the diffusion blank to remove the first side plate and the second side plate to obtain the T-shaped structure.