High-efficiency flame-retardant photovoltaic backboard base film and preparation method thereof

By using a combination of ester compounds, halogen-free flame retardants and anti-aging agents in the base film of the photovoltaic backsheet, combined with the melt polycondensation process and γ-aminopropyltriethoxysilane modification technology, the resistance of traditional photovoltaic backsheets is solved. It solves the problems of insufficient flame retardancy and insufficient weather resistance, and achieves both efficient flame retardancy and weather resistance.

CN118769655APending Publication Date: 2024-10-15ZHEJIANG JIANXING TECH CO LTD

Patent Information

Application Number
CN202410782398.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The flame retardant level of traditional photovoltaic backsheets is insufficient, especially when used outdoors, they are easily affected by water vapor, resulting in reduced flame retardant performance. They also require high aging and weather resistance, but commonly used flame retardant materials cannot take both into account.

Method used

Using a combination of ester compounds, halogen-free flame retardants and anti-aging agents, a high-efficiency flame-retardant photovoltaic backsheet base film is prepared through catalytic esterification and melt polycondensation processes. The addition of inorganic particles and halogen-free flame retardants is increased to improve the base film. Flame retardant and weather-resistant properties, and the metal oxide is modified with γ-aminopropyltriethoxysilane to enhance dispersion properties.

Benefits of technology

It achieves both high-efficiency flame retardant performance and weather resistance, avoids the impact of moisture on flame retardant materials, and improves the reliability and high temperature resistance of the base film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004897534320000091
    Figure BDA0004897534320000091
Patent Text Reader

Abstract

The invention relates to the technical field of photovoltaic backboard base films, and particularly discloses an efficient flame-retardant photovoltaic backboard base film and a preparation method thereof. An efficient flame-retardant photovoltaic backboard base film comprises two surface layers and a core layer arranged between the two surface layers, and the surface layers are prepared from, by weight, 90-110 parts of ester, 0.2-1.0 part of inorganic particles, 1-10 parts of a halogen-free flame retardant, 0.2-3 parts of a tackifier and 0.1-1.0 part of an anti-aging agent; the core layer is prepared from the following raw material components in parts by weight: 90 to 110 parts of ester, 0.2 to 5.0 parts of inorganic particles, 5 to 25 parts of halogen-free flame retardant, 0.2 to 3 parts of tackifier and 0.1 to 1.0 part of anti-aging agent; the ester comprises the following raw materials: acid, alcohol ester, a catalyst and a solvent. The base film provided by the invention not only has better flame retardant property, but also has better aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of photovoltaic backplane base films, and in particular to a high-efficiency flame-retardant photovoltaic backplane base film and a preparation method thereof. Background Art

[0002] Traditional photovoltaic backsheets are made of fluorine-containing materials, which have excellent flame retardant properties. Therefore, the flame retardant grade of the base film in the middle layer is not required to be high. Generally, V-2 or VTM-2 is sufficient to meet the use requirements. However, as the requirements for limiting and prohibiting fluorine become increasingly stringent, and in specific application scenarios, such as rooftop distributed power generation, low flame retardant grades can easily cause irreparable losses. Therefore, in this scenario, it is necessary to use materials with higher flame retardancy, such as V-0 or VTM-0. Since most flame retardants are sensitive to water vapor, their flame retardant properties will decrease when used outdoors for a long time. In addition, PET used in photovoltaic backsheets has high requirements for aging and weather resistance. General flame retardant materials will have a greater impact on its mechanical and aging properties. Therefore, it is urgent to develop a base film for photovoltaic backsheets that can meet both flame retardant and weather resistance requirements. Summary of the invention

[0003] In order to obtain a photovoltaic backplane base film that can meet both flame retardancy and weather resistance requirements, the present application provides a high-efficiency flame retardant photovoltaic backplane base film and a preparation method thereof.

[0004] In the first aspect, the present application provides a highly efficient flame-retardant photovoltaic backplane base film, which adopts the following technical solution: A high-efficiency flame-retardant photovoltaic backplane base film comprises two surface layers and a core layer arranged between the two surface layers, wherein the raw materials of the surface layers comprise the following components in parts by weight: 90-110 parts of esterified product, 0.2-1.0 parts of inorganic particles, 1-10 parts of halogen-free flame retardant, 0.2-3 parts of tackifier, and 0.1-1.0 parts of anti-aging agent; the raw materials of the core layer comprise the following components in parts by weight: 90-110 parts of esterified product, 0.2-5.0 parts of inorganic particles, 5-25 parts of halogen-free flame retardant, 0.2-3 parts of tackifier, and 0.1-1.0 parts of anti-aging agent; the raw materials of the esterified product comprise acid, alcohol ester, catalyst, and solvent.

[0005] By adopting the above technical scheme, the acid and alcohol ester are first esterified with a catalyst to obtain an esterified product, and then the flame retardant properties of the base film are improved by combining inorganic particles and halogen-free flame retardants. The addition of an anti-aging agent can make the base film have certain weather resistance. The thickener can make the surface layer and the core layer better composite, and the amount of inorganic particles and halogen-free flame retardants added in the core layer is increased, so that the formed composite base film has both good flame retardant properties and good aging resistance.

[0006] In a specific embodiment, the acid includes terephthalic acid, isophthalic acid or a mixture of the two.

[0007] In a specific embodiment, the alcohol ester includes one or more of ethylene terephthalate, ethylene isophthalate, and ethylene naphthalate.

[0008] In a specific embodiment, the solvent includes one or more of ethylene glycol, neopentyl glycol, propylene glycol, butylene glycol, and 1,4-cyclohexanedimethanol.

[0009] In a specific embodiment, the inorganic particles include one or more of mica, barium sulfate, kaolin, titanium dioxide, calcium carbonate, silicon dioxide, talc, and montmorillonite; the halogen-free flame retardant includes one or more of phosphorus compounds, metal oxides, hydroxides, silicon-based flame retardants, and nitrogen-based flame retardants.

[0010] By adopting the above technical solution, the addition of mica, barium sulfate, kaolin, titanium dioxide, calcium carbonate, silicon dioxide, talc and montmorillonite can improve the high temperature resistance of the base film, and talc can also improve the dispersion performance between the raw materials.

[0011] In a specific embodiment, the preparation method of the halogen-free flame retardant comprises the following steps: γ-aminopropyltriethoxysilane, ethanol and water are stirred and mixed to obtain a spraying liquid; The metal oxide and the hydroxide are stirred and mixed uniformly to obtain a mixture, and then during the stirring process, the spraying liquid is slowly sprayed into the mixture. After the spraying is completed, the mixture is continuously stirred and dried to obtain a modified material; The polyethylene terephthalate and the modified material are stirred and mixed uniformly, melt-blended, and extruded into granules to obtain a halogen-free flame retardant; wherein the weight ratio of the polyethylene terephthalate to the modified material is 1:(1.5-2.5).

[0012] By adopting the above technical scheme, γ-aminopropyltriethoxysilane is first dissolved in ethanol to obtain a spray liquid, and then sprayed and dried while stirring metal oxides and hydroxides, so that the γ-aminopropyltriethoxysilane first modifies the metal oxides and hydroxides to improve the dispersion performance, which is convenient for mixing with polyethylene terephthalate. Under the action of γ-aminopropyltriethoxysilane, coupling is carried out and the metal oxides and hydroxides are wrapped on the surface, so that the metal oxides and hydroxides can be more evenly dispersed in the esterification product. Polyethylene terephthalate has good high temperature resistance and processing performance, thereby further improving the flame retardancy and weather resistance of the base film.

[0013] In a specific embodiment, the tackifier includes one or more of oxazoline, isocyanate, pyromellitic anhydride, trimellitic anhydride, and glycidyl ether epoxy compounds.

[0014] In a specific embodiment, the anti-aging agent includes one or more of 4-methoxybenzylidenemalonate, N,N'-bis(4-ethoxyformylphenyl)-N-benzylformamidine, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol, 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-octyloxyphenol, 2,2'-(1,4-benzenedimethylene)dimalonate, and N-(2-ethoxyphenyl)-N-(2-ethylphenyl)-oxamide.

[0015] In the second aspect, the present application provides a method for preparing a highly efficient flame-retardant photovoltaic backplane base film, which adopts the following technical solution: A method for preparing a high-efficiency flame-retardant photovoltaic backsheet base film comprises the following steps: Esterification: adding acid to solvent, stirring and mixing evenly to obtain acid solution; adding alcohol ester to solvent, stirring and mixing evenly to obtain alcohol ester solution; adding catalyst to solvent, stirring and mixing evenly to obtain catalyst solution; mixing acid solution and alcohol ester solution first, then adding catalyst solution, and carrying out esterification reaction at 250-265°C and 100-200kPa for 4-5h to obtain esterified product; wherein the molar ratio of acid to solvent is 1:(1.15-1.7); the molar ratio of alcohol ester to solvent is 1:(1.8-2.4); the weight ratio of catalyst to solvent is 1:(20-100); the weight ratio of the mixed solution of acid solution and alcohol ester solution to catalyst solution is (97.9-99.63):(0.37-2.1); Polycondensation: first add inorganic particles, halogen-free flame retardant and anti-aging agent to the esterified product, then add it to the pre-polycondensation kettle, evacuate, and pre-polycondense for 2-4 hours at 270-280°C and 1-10kPa to obtain a pre-polycondensation product; then pump the pre-polycondensation product into the final polycondensation kettle, perform final polycondensation at 280-285°C and 100-200kPa for 2-3 hours to obtain a final polycondensation product, and finally add a tackifier to obtain a polymer melt A; use the above method again to obtain a melt B; Compounding: Melt A and melt B are transported from different pipes, merged by a distributor, and formed into a three-layer structure before the extrusion die, and then cast, longitudinally stretched, transversely stretched, heat-set, corona-treated, and cooled to obtain a photovoltaic backplane base film.

[0016] By adopting the above technical scheme and utilizing the above method, a base film with good flame retardancy and weather resistance can be obtained. After melt polycondensation, the melt A and melt B obtained can meet the raw material requirements for the film drawing process, and the melt A and melt B are directly drawn into film. Under the premise of ensuring the quality of the base film, the influence of moisture on the flame retardant material due to melt cooling and pelletizing is avoided, thereby improving the reliability of the flame retardant performance.

[0017] In a specific embodiment, the viscosity of melt A is 0.70dl / g-0.90dl / g, the terminal carboxyl content is ≤20mmol / kg, the melting point is 250℃-272℃, the ash content is 0.2%-1.0%, and the oxygen index is 25-30%; the viscosity of melt B is 0.70dl / g-0.90dl / g, the terminal carboxyl content is ≤20mmol / kg, the melting point is 250℃-272℃, the ash content is 0.2%-5.0%, and the oxygen index is 27-40%.

[0018] In summary, the present application includes at least one of the following beneficial technical effects: 1. In the present application, a catalyst is first used to esterify the acid and alcohol ester to obtain an esterified product, and then inorganic particles and halogen-free flame retardants are used to improve the flame retardant properties of the base film. The addition of an anti-aging agent can make the base film have certain weather resistance. The tackifier can make the surface layer and the core layer better composite, and the addition amount of inorganic particles and halogen-free flame retardants in the core layer is increased, so that the formed composite base film has both good flame retardant properties and good aging resistance. 2. In the present application, γ-aminopropyltriethoxysilane is first dissolved in ethanol to obtain a spraying liquid, and then sprayed and dried while stirring metal oxides and hydroxides, so that γ-aminopropyltriethoxysilane first modifies the metal oxides and hydroxides to improve the dispersion performance, which is convenient for mixing with polyethylene terephthalate. Under the action of γ-aminopropyltriethoxysilane, coupling is carried out and the metal oxides and hydroxides are wrapped on the surface, so that the metal oxides and hydroxides can be more evenly dispersed in the esterification product. Polyethylene terephthalate has good high temperature resistance and processing performance, thereby further improving the flame retardancy and weather resistance of the base film; 3. The method in the present application, after melt polycondensation, obtains Melt A and Melt B which can meet the raw material requirements of the film drawing process, and Melt A and Melt B are directly drawn into film. Under the premise of ensuring the quality of the base film, it avoids the influence of melt cooling and pelletizing and moisture on the flame retardant material, thereby improving the reliability of the flame retardant performance. DETAILED DESCRIPTION

[0019] The present application is further described in detail below with reference to the embodiments.

[0020] All raw materials in the embodiment can be obtained commercially. Acids include but are not limited to terephthalic acid, isophthalic acid, or a mixture of one or both; alcohol esters include but are not limited to a mixture of one or more of ethylene terephthalate, ethylene isophthalate, and ethylene naphthalate; solvents include but are not limited to a mixture of one or more of ethylene glycol, neopentyl glycol, propylene glycol, butanediol, and 1,4-cyclohexanedimethanol; inorganic particles include but are not limited to a mixture of one or more of mica, barium sulfate, kaolin, titanium dioxide, calcium carbonate, silicon dioxide, talc, and montmorillonite, preferably a mixture of silicon dioxide and talc in this application; halogen-free flame retardants include but are not limited to a mixture of one or more of phosphorus compounds, metal oxides, hydroxides, silicon flame retardants, and nitrogen flame retardants, preferably metal oxides, hydroxides, a mixture of the composition; a tackifier including but not limited to a mixture of one or more of oxazoline, isocyanate, pyromellitic anhydride, trimellitic anhydride, and glycidyl ether epoxy compounds, preferably isocyanate in the present application; an anti-aging agent including but not limited to a mixture of one or more of 4-methoxybenzylidenemalonate, N,N'-bis(4-ethoxyformylphenyl)-N-benzylformamidine, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol, 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-octyloxyphenol, 2,2'-(1,4-benzenedimethylene)dimalonate tetraethyl ester, and N-(2-ethoxyphenyl)-N-(2-ethylphenyl)-oxamide, preferably 4-methoxybenzylidenemalonate in the present application.

[0021] Preparation Example Preparation Example 1 Preparation Example 1 provides a method for preparing a halogen-free flame retardant, comprising the following steps: Stir and mix γ-aminopropyltriethoxysilane, ethanol and water to obtain a spraying liquid; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol and water is 5:18:2; The metal oxide and the hydroxide are stirred and mixed evenly to obtain a mixture, and then during the stirring process, the spraying liquid is slowly sprayed into the mixture. After the spraying is completed, the stirring is continued for 0.5 hours, and finally the mixture is dried at 100°C for 1.5 hours to obtain a modified material; wherein the weight ratio of the metal oxide to the hydroxide is 1:1.5, and the metal oxide is aluminum oxide, and the hydroxide is aluminum hydroxide; polyethylene terephthalate and the modified material are stirred and mixed evenly, melt-blended, and extruded into granules to obtain a halogen-free flame retardant; wherein the weight ratio of the polyethylene terephthalate to the modified material is 1:1.5.

[0022] Preparation Example 2 The difference between Preparation Example 2 and Preparation Example 1 is that the weight ratio of polyethylene terephthalate to the modified material is 1:2, and the remaining steps are consistent with Preparation Example 1.

[0023] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that the weight ratio of polyethylene terephthalate to modified material is 1:2.5, and the remaining steps are consistent with Preparation Example 1. Example

[0024] Example 1 Embodiment 1 provides a method for preparing a high-efficiency flame-retardant photovoltaic backsheet base film, comprising the following steps: Esterification: add the acid to the solvent, stir and mix evenly to obtain an acid solution; add the alcohol ester to the solvent, stir and mix evenly to obtain an alcohol ester liquid; add the catalyst to the solvent, stir and mix evenly to obtain a catalyst liquid; first mix the acid solution and the alcohol ester liquid, add them to the esterification kettle, then add the catalyst liquid, and carry out esterification reaction at 250°C and 100kPa for 5 hours to obtain an esterified product; wherein the molar ratio of the acid to the solvent is 1:1.15; the molar ratio of the alcohol ester to the solvent is 1:1.8; the weight ratio of the catalyst to the solvent is 1:20; the weight ratio of the mixed solution of the acid solution and the alcohol ester liquid to the catalyst liquid is 97.9:2.1; the acid is terephthalic acid; the alcohol ester is ethylene glycol terephthalate; the catalyst is antimony trioxide; and the solvent is ethylene glycol; Polycondensation: first add 0.2kg of inorganic particles, 1kg of halogen-free flame retardant, and 0.1kg of anti-aging agent to 90kg of esterification product, then add to the pre-polycondensation kettle, evacuate, discharge excess solvent, and pre-polycondense for 4h at 270℃ and 1kPa to obtain a pre-polycondensation product; then pump the pre-polycondensation product into the final polycondensation kettle, perform final polycondensation at 280℃ and 100kPa for 3h to obtain a final polycondensation product, and finally add 0.2kg of tackifier to obtain polymer melt A; and melt A has a viscosity of 0.70dl / g, a terminal carboxyl content of 15mmol / kg, a melting point of 250℃, an ash content of 0.2%, and an oxygen index of 25%; First, 0.2 kg of inorganic particles, 5 kg of halogen-free flame retardant, and 0.1 kg of anti-aging agent were added to 90 kg of esterification product, and then added to a pre-condensation kettle, vacuumed, and excess solvent was discharged, and pre-condensation was performed at 270 ° C., 1 kPa for 4 hours to obtain a pre-condensation product; then the pre-condensation product was pumped into a final condensation kettle, and final condensation was performed at 280 ° C., 100 kPa for 3 hours to obtain a final condensation product, and finally 0.2 kg of tackifier was added to obtain a polymer melt B; and the viscosity of melt B was 0.70 dl / g, The terminal carboxyl content is 15mmol / kg, the melting point is 250℃, the ash content is 0.2%, and the oxygen index is 27%; the inorganic particles are a mixture of silicon dioxide and talc, and the weight ratio of silicon dioxide to talc is 1:1; the halogen-free flame retardant is a mixture of metal oxides and hydroxides, and the weight ratio of metal oxides and hydroxides is 1:1.5, the metal oxide is aluminum oxide, and the hydroxide is aluminum hydroxide; the anti-aging agent is 4-methoxybenzylidenemalonic acid dimethyl ester; the tackifier is isocyanate; Compounding: Melt A and Melt B are transported by different pipes, merged by a distributor, and form a three-layer structure in front of the extrusion die, then cast into sheets, longitudinally stretched, transversely stretched, heat-set, corona-treated, and cooled to form. Melt B forms a core layer with a thickness of 235 microns, and melt A forms surface layers on both sides of the core layer with a thickness of 7.5 microns to obtain a photovoltaic backplane base film.

[0025] Example 2 The difference between Example 2 and Example 1 is that, polycondensation: first add 0.6 kg of inorganic particles, 5.5 kg of halogen-free flame retardant, and 0.55 kg of anti-aging agent to 100 kg of esterification product, then add them to a pre-polycondensation kettle, evacuate, discharge excess solvent, and pre-polycondense for 4 hours at 270° C. and 1 kPa to obtain a pre-polycondensation product; then pump the pre-polycondensation product into a final polycondensation kettle, perform final polycondensation at 280° C. and 100 kPa for 3 hours to obtain a final polycondensation product, and finally add 1.6 kg of tackifier to obtain a polymer melt A; and the viscosity of melt A is 0.80 dl / g, the terminal carboxyl content is 18 mmol / kg, the melting point is 261° C., the ash content is 0.6%, and the oxygen index is 28%; First, 2.6 kg of inorganic particles, 15 kg of halogen-free flame retardant, and 0.55 kg of anti-aging agent are added to 100 kg of esterification product, and then added to a pre-condensation kettle, vacuumed, and excess solvent is discharged, and pre-condensation is carried out at 270° C. and 1 kPa for 4 hours to obtain a pre-condensation product; then the pre-condensation product is pumped into a final condensation kettle, and final condensation is carried out at 280° C. and 100 kPa for 3 hours to obtain a final condensation product, and finally 1.6 kg of tackifier is added to obtain a polymer melt B; and the viscosity of melt B is 0.80 dl / g, the terminal carboxyl content is 18 mmol / kg, the melting point is 261° C., the ash content is 2.6%, and the oxygen index is 34%; Compounding: Melt A and Melt B are transported by different pipes, merged by a distributor, and form a three-layer structure in front of the extrusion die, then cast into sheets, longitudinally stretched, transversely stretched, heat-set, corona-treated, and cooled to form, where melt B forms a core layer with a thickness of 217 microns, and melt A forms surface layers on both sides of the core layer with a thickness of 16 microns to obtain a photovoltaic backplane base film; the remaining steps are consistent with Example 1.

[0026] Example 3 The difference between Example 3 and Example 1 is that, polycondensation: first add 1 kg of inorganic particles, 10 kg of halogen-free flame retardant, and 1 kg of anti-aging agent to 110 kg of esterification product, then add to the pre-polycondensation kettle, evacuate, discharge excess solvent, and pre-polycondense for 4 hours at 270° C. and 1 kPa to obtain a pre-polycondensation product; then pump the pre-polycondensation product into the final polycondensation kettle, perform final polycondensation at 280° C. and 100 kPa for 3 hours to obtain a final polycondensation product, and finally add 3 kg of tackifier to obtain a polymer melt A; and the viscosity of melt A is 0.90 dl / g, the terminal carboxyl content is 20 mmol / kg, the melting point is 272° C., the ash content is 1%, and the oxygen index is 30%; First, 5 kg of inorganic particles, 25 kg of halogen-free flame retardant, and 1 kg of anti-aging agent are added to 110 kg of esterified product, and then added to a pre-condensation kettle, vacuumed, and excess solvent is discharged, and pre-condensation is performed at 270° C. and 1 kPa for 4 hours to obtain a pre-condensation product; then the pre-condensation product is pumped into a final condensation kettle, and final condensation is performed at 280° C. and 100 kPa for 3 hours to obtain a final condensation product, and finally 3 kg of tackifier is added to obtain a polymer melt B; and the viscosity of melt A is 0.90 dl / g, the terminal carboxyl content is 20 mmol / kg, the melting point is 272° C., the ash content is 5%, and the oxygen index is 40%; Compounding: Melt A and Melt B are transported by different pipes, merged by a distributor, and form a three-layer structure in front of the extrusion die, then cast into sheets, longitudinally stretched, transversely stretched, heat-set, corona-treated, and cooled to form, where melt B forms a core layer with a thickness of 200 microns, and melt A forms surface layers on both sides of the core layer with a thickness of 25 microns to obtain a photovoltaic backplane base film; the remaining steps are consistent with Example 1.

[0027] Example 4 The difference between Example 4 and Example 2 is that, in esterification, an acid is added to a solvent, and the mixture is stirred and mixed to obtain an acid solution; an alcohol ester is added to a solvent, and the mixture is stirred and mixed to obtain an alcohol ester solution; a catalyst is added to a solvent, and the mixture is stirred and mixed to obtain a catalyst solution; the acid solution and the alcohol ester solution are first mixed, and added to an esterification kettle, and then the catalyst solution is added, and the esterification reaction is carried out at 257° C. and 150 kPa for 4.5 hours to obtain an esterified product; wherein the molar ratio of the acid to the solvent is 1:1.42; the molar ratio of the alcohol ester to the solvent is 1:2.1; the weight ratio of the catalyst to the solvent is 1:60; the weight ratio of the mixed solution of the acid solution and the alcohol ester solution to the catalyst solution is 98.76:1.23; and the remaining steps are consistent with Example 2.

[0028] Example 5 The difference between Example 5 and Example 2 is that, in esterification, an acid is added to a solvent, and the mixture is stirred and mixed to obtain an acid solution; an alcohol ester is added to a solvent, and the mixture is stirred and mixed to obtain an alcohol ester solution; a catalyst is added to a solvent, and the mixture is stirred and mixed to obtain a catalyst solution; the acid solution and the alcohol ester solution are first mixed, and the mixture is added to an esterification kettle, and then the catalyst solution is added, and the esterification reaction is carried out at 265° C. and 200 kPa for 4 hours to obtain an esterified product; wherein the molar ratio of the acid to the solvent is 1:1.7; the molar ratio of the alcohol ester to the solvent is 1:2.4; the weight ratio of the catalyst to the solvent is 1:100; the weight ratio of the mixed solution of the acid solution and the alcohol ester solution to the catalyst solution is 99.63:0.37; and the remaining steps are consistent with Example 2.

[0029] Example 6 The difference between Example 6 and Example 4 is that, polycondensation: first, 0.6 kg of inorganic particles, 5.5 kg of halogen-free flame retardant, and 0.55 kg of anti-aging agent are added to 100 kg of esterification product, and then added to a pre-polycondensation kettle, vacuumed, excess solvent is discharged, and pre-polycondensation is carried out at 275 ° C., 5 kPa for 3 hours to obtain a pre-polycondensation product; then the pre-polycondensation product is pumped into a final polycondensation kettle, and final polycondensation is carried out at 283 ° C., 150 kPa for 2.5 hours to obtain a final polycondensation product, and finally 1.6 kg of tackifier is added to obtain polymer melt A; First, 2.6 kg of inorganic particles, 15 kg of halogen-free flame retardant, and 0.55 kg of anti-aging agent were added to 100 kg of esterification product, and then added to the pre-condensation kettle, vacuumed, and excess solvent was discharged, and pre-condensed at 275 ° C, 5 kPa for 3 hours to obtain a pre-condensation product; then the pre-condensation product was pumped into the final condensation kettle, and the final condensation was carried out at 283 ° C, 150 kPa for 2.5 hours to obtain a final condensation product, and finally 1.6 kg of tackifier was added to obtain polymer melt B; the remaining steps were consistent with Example 4.

[0030] Example 7 The difference between Example 7 and Example 4 is that, polycondensation: first, 0.6 kg of inorganic particles, 5.5 kg of halogen-free flame retardant, and 0.55 kg of anti-aging agent are added to 100 kg of esterification, and then added to a pre-polycondensation kettle, vacuumed, excess solvent is discharged, and pre-polycondensation is carried out at 280 ° C. and 10 kPa for 2 hours to obtain a pre-polycondensation product; then the pre-polycondensation product is pumped into a final polycondensation kettle, and final polycondensation is carried out at 285 ° C. and 200 kPa for 2 hours to obtain a final polycondensation product, and finally 1.6 kg of tackifier is added to obtain polymer melt A; First, 2.6 kg of inorganic particles, 15 kg of halogen-free flame retardant, and 0.55 kg of anti-aging agent were added to 100 kg of esterification product, and then added to the pre-condensation kettle, vacuumed, and excess solvent was discharged, and pre-condensed at 280 ° C, 10 kPa for 2 hours to obtain a pre-condensation product; then the pre-condensation product was pumped into the final condensation kettle, and the final condensation was carried out at 285 ° C, 200 kPa for 2 hours to obtain a final condensation product, and finally 1.6 kg of tackifier was added to obtain polymer melt B; the remaining steps were consistent with Example 4.

[0031] Example 8 The difference between Example 8 and Example 6 is that the acid is a mixture of terephthalic acid and isophthalic acid, and the weight ratio of terephthalic acid to isophthalic acid is 1:1; the alcohol ester is a mixture of ethylene terephthalate and ethylene isophthalate, and the weight ratio of ethylene terephthalate to ethylene isophthalate is 1:1; the solvent is a mixture of ethylene glycol and propylene glycol, and the weight ratio of ethylene glycol to propylene glycol is 1:1; and the remaining steps are consistent with Example 6.

[0032] Example 9 The difference between Example 9 and Example 6 is that the halogen-free flame retardant is the halogen-free flame retardant in Preparation Example 1; the remaining steps are consistent with Example 6.

[0033] Example 10 The difference between Example 10 and Example 6 is that the halogen-free flame retardant is the halogen-free flame retardant in Preparation Example 2; the remaining steps are consistent with Example 6.

[0034] Embodiment 11 The difference between Example 11 and Example 6 is that the halogen-free flame retardant is the halogen-free flame retardant in Preparation Example 3; the remaining steps are consistent with Example 6.

[0035] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that melt A is directly pumped into the die head, then cast into a sheet, longitudinally stretched, transversely stretched, heat-set, corona-treated, and cooled to form a photovoltaic backplane base film with a thickness of 250 microns.

[0036] Performance test Flame retardant performance: According to GB / T2408-2008 "Determination of combustion performance of plastics", the flame retardant grade is obtained; and the oxygen index of the base film is detected.

[0037] Aging resistance: The aging resistance of the base film was tested at 121° C., 100% humidity, and 0.2 MPa pressure to obtain the aging time.

[0038] Table 1 Test results of photovoltaic backsheet base film In combination with Example 1 and Comparative Example 1, the flame retardant properties and aging resistance of the base film in Example 1 are both good. It can be seen that by using the method in the present application, a composite film composed of a surface layer and a core layer arranged between two surface layers, and inorganic particles and halogen-free flame retardants are added to the raw materials, the obtained base film has both good flame retardant properties and good aging resistance.

[0039] Combining Examples 1-3, the flame retardant properties of the base film in Example 3 are the best, but the aging resistance of the base film in Example 2 is the best. It can be seen that when preparing the melt, increasing the amount of raw materials used can improve the flame retardant properties of the base film, but will reduce the aging resistance.

[0040] Combining Example 2, Example 4 and Example 5, the base film in Example 4 has the best aging resistance, which shows that when preparing the ester, the reaction conditions in Example 4 are the best.

[0041] Combining Example 4, Example 6 and Example 7, the base film in Example 6 has the best flame retardant properties and the best aging resistance. It can be seen that when performing the polycondensation reaction, the reaction conditions in Example 6 are the best.

[0042] Combining Example 6 and Example 8, the flame retardant properties of the base film in Example 8 are better, and the aging resistance is also better. It can be seen that when preparing the ester, the acid is a mixed acid composed of terephthalic acid and isophthalic acid, and the alcohol ester is a mixture of ethylene terephthalate and ethylene isophthalate, and then combined with a mixed solvent composed of ethylene glycol and propylene glycol, the performance of the obtained base film is also better.

[0043] Combining Example 6 with Examples 9-11, the base film in Examples 9-11 has better flame retardant properties and better aging resistance. It can be seen that modifying the flame retardant using polyethylene terephthalate and γ-aminopropyltriethoxysilane not only improves the dispersion properties of the flame retardant, thereby further improving the flame retardant properties of the base film, but polyethylene terephthalate can also further improve the aging resistance of the base film.

[0044] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A highly efficient flame-retardant photovoltaic backsheet base film, comprising two surface layers and a core layer disposed between the two surface layers, characterized in that: The raw materials of the surface layer include the following components in parts by weight: 90-110 parts of esterified product, 0.2-1.0 parts of inorganic particles, 1-10 parts of halogen-free flame retardant, 0.2-3 parts of tackifier, and 0.1-1.0 parts of anti-aging agent; the raw materials of the core layer include the following components in parts by weight: 90-110 parts of esterified product, 0.2-5.0 parts of inorganic particles, 5-25 parts of halogen-free flame retardant, 0.2-3 parts of tackifier, and 0.1-1.0 parts of anti-aging agent; the raw materials of the esterified product include acid, alcohol ester, catalyst, and solvent.

2. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 1, characterized in that: The acid includes terephthalic acid, isophthalic acid or a mixture of the two.

3. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 2, characterized in that: The alcohol ester includes one or more of ethylene terephthalate, ethylene isophthalate, and ethylene naphthalate.

4. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 3, characterized in that: The solvent includes one or more of ethylene glycol, neopentyl glycol, propylene glycol, butylene glycol, and 1,4-cyclohexanedimethanol.

5. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 1, characterized in that: The inorganic particles include one or more of mica, barium sulfate, kaolin, titanium dioxide, calcium carbonate, silicon dioxide, talc, and montmorillonite; the halogen-free flame retardant includes one or more of phosphorus compounds, metal oxides, hydroxides, silicon-based flame retardants, and nitrogen-based flame retardants.

6. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 5, characterized in that: The preparation method of the halogen-free flame retardant comprises the following steps: γ-aminopropyltriethoxysilane, ethanol and water are stirred and mixed to obtain a spraying liquid; The metal oxide and the hydroxide are stirred and mixed uniformly to obtain a mixture, and then during the stirring process, the spraying liquid is slowly sprayed into the mixture. After the spraying is completed, the mixture is continuously stirred and dried to obtain a modified material; The polyethylene terephthalate and the modified material are stirred and mixed evenly, melt-blended, and extruded into granules to obtain a halogen-free flame retardant; wherein the weight ratio of the polyethylene terephthalate to the modified material is 1: (1.5-2.5).

7. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 1, characterized in that: The tackifier includes one or more of oxazoline, isocyanate, pyromellitic anhydride, trimellitic anhydride, and glycidyl ether epoxy compounds.

8. The high-efficiency flame-retardant photovoltaic backsheet base film according to claim 1, characterized in that: The anti-aging agent includes one or more of 4-methoxybenzylidenemalonate, N,N'-bis(4-ethoxyformylphenyl)-N-benzylformamidine, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol, 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-octyloxyphenol, 2,2'-(1,4-benzenedimethylene)dimalonate tetraethyl, and N-(2-ethoxyphenyl)-N-(2-ethylphenyl)-oxamide.

9. A method for preparing a high-efficiency flame-retardant photovoltaic backsheet base film as claimed in claims 1 to 8, characterized in that: The following steps are involved: Esterification: add the acid to the solvent, stir and mix evenly to obtain an acid solution; add the alcohol ester to the solvent, stir and mix evenly to obtain an alcohol ester liquid; add the catalyst to the solvent, stir and mix evenly to obtain a catalyst liquid; first mix the acid solution and the alcohol ester liquid, then add the catalyst liquid, and carry out esterification reaction at 250-265°C and 100-200kPa for 4-5 hours to obtain an esterified product; wherein the molar ratio of the acid to the solvent is 1:(1.15-1.7); the molar ratio of the alcohol ester to the solvent is 1:(1.8-2.4); the weight ratio of the catalyst to the solvent is 1:(20-100); the weight ratio of the mixed solution of the acid solution and the alcohol ester liquid to the catalyst liquid is (97.9-99.63):(0.37-2.1); Polycondensation: first add inorganic particles, halogen-free flame retardant and anti-aging agent to the esterified product, then add it to the pre-polycondensation kettle, evacuate, and pre-polycondense for 2-4 hours at 270-280°C and 1-10kPa to obtain a pre-polycondensation product; then pump the pre-polycondensation product into the final polycondensation kettle, perform final polycondensation at 280-285°C and 100-200kPa for 2-3 hours to obtain a final polycondensation product, and finally add a tackifier to obtain a polymer melt A; use the above method again to obtain a melt B; Compounding: Melt A and melt B are transported from different pipes, merged by a distributor, and formed into a three-layer structure before the extrusion die, and then cast, longitudinally stretched, transversely stretched, heat-set, corona-treated, and cooled to obtain a photovoltaic backplane base film.

10. The method for preparing a high-efficiency flame-retardant photovoltaic backsheet base film according to claim 9, characterized in that: The viscosity of melt A is 0.70dl / g-0.90dl / g, the terminal carboxyl content is ≤20mmol / kg, the melting point is 250℃-272℃, the ash content is 0.2%-1.0%, and the oxygen index is 25-30%; the viscosity of melt B is 0.70dl / g-0.90dl / g, the terminal carboxyl content is ≤20mmol / kg, the melting point is 250℃-272℃, the ash content is 0.2%-5.0%, and the oxygen index is 27-40%.

Citation Information

Patent Citations

  • Preparation method of polyether material, polyether film and preparation method thereof

    CN103627150A

  • Ultraviolet-resistant thin film for isolation clothes and preparation method thereof

    CN104608453A

  • Solar battery backplane, and preparation method of film polyester used for backplane

    CN106008940A

  • Optical polyester film

    CN108556441A

  • Medical super-tough puncture-resistant high-barrier composite film and preparation method thereof

    CN109968777A

Cited By