Zinc nitride and preparation method thereof

By heating zinc into zinc vapor and reacting with preheated ammonia gas in an inert atmosphere, the problem of limited contact with zinc in the molten state is solved, the reaction efficiency and raw material utilization are improved, and it is suitable for mass production of zinc nitride.

CN118771318APending Publication Date: 2024-10-15XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048315.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the prior art, when zinc reacts with ammonia in the molten state, internal contact is limited, resulting in low raw material utilization, low reaction efficiency, and difficulty in mass production.

Method used

Zinc is heated to 800~900°C to form zinc vapor, which reacts with preheated ammonia in an inert atmosphere to deposit zinc nitride powder. By controlling the heating rate and ammonia flow, the reaction area and efficiency are increased.

Benefits of technology

Through the reaction of zinc vapor and ammonia gas, the reaction area and efficiency of the raw material are significantly improved, which is suitable for mass production, avoids the rapid cooling or solidification of zinc vapor, and improves the purity and utilization of zinc nitride powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the field of semiconductor materials, and discloses a preparation method of zinc nitride, which comprises the following steps: heating a zinc elementary substance in an inert atmosphere to vaporize the zinc elementary substance into zinc steam; preheating the ammonia gas; and when the zinc elementary substance is heated to 800-900 DEG C, ammonia gas is introduced into the reaction system, so that the zinc steam and the ammonia gas react in an inert atmosphere, and powder deposited at the bottom of the reaction system is zinc nitride powder. Compared with the prior art in which the molten zinc reacts with the ammonia gas, the preparation method provided by the invention has the advantages that the reaction area of the raw materials is greatly increased, the reaction efficiency is higher, and the preparation method is suitable for batch production. In addition, the invention also discloses the zinc nitride prepared by the preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor materials and relates to the preparation of a nitride, in particular to zinc nitride and its preparation. Background Art

[0002] In the field of wide-gap semiconductors, zinc compounds have been widely studied. Zn3N2 is a gray-black crystal with an inverse helium-manganese structure, a molecular weight of 224.12, and a relative density of 6.2 g / m 3 . Zinc nitride (Zn3N2) has unique electrical and optical properties, which makes it widely used in light-emitting diodes, solar cells, sensors and other fields. In the existing technology, zinc nitride can be prepared by magnetron sputtering, chemical vapor deposition, electrostatic electrolysis, molecular beam epitaxy and other methods. Zinc nitride is widely used in fuel cells, solar cells and other fields, and is a new functional material with potential.

[0003] CN116750730A discloses a method for preparing zinc nitride, wherein zinc is heated to 550-600°C, ammonia is introduced into the reaction system to react with the zinc, and zinc powder is placed in layers, ammonia can flow between the multi-layer quartz boats, so that ammonia has more opportunities to contact with zinc powder, and the reaction rate of zinc is improved by controlling the reaction temperature and the laying thickness of zinc powder. In this method, when zinc powder is heated to 550-600°C, zinc is in a molten state and reacts with ammonia, and the contact between the inside of the molten zinc and ammonia is limited, which affects the utilization rate of the raw materials to a certain extent. Summary of the invention

[0004] In view of the defects and shortcomings of the prior art, in a first aspect, the present invention provides a method for preparing zinc nitride; in a second aspect, the present invention provides zinc nitride prepared by the above preparation method.

[0005] In a first aspect, the present invention provides a method for preparing zinc nitride, comprising: heating zinc element under an inert atmosphere to vaporize it into zinc vapor; preheating ammonia; when the zinc element is heated to 800-900° C., introducing ammonia into a reaction system to allow the zinc vapor and ammonia to react under the inert atmosphere, and the powder deposited at the bottom of the reaction system is zinc nitride powder.

[0006] Preferably, the heating of zinc comprises the following steps: Step 101, heating zinc to 800-900° C. and keeping the temperature for 30-60 minutes; Step 102, then raise the temperature to 950-1050°C and keep it for 15-30 minutes.

[0007] More preferably, in step 101, the heating rate is 3-10°C / min.

[0008] More preferably, in step 102, the heating rate is 0.2-1°C / min.

[0009] Preferably, the temperature of the preheated ammonia is 200-300°C.

[0010] Preferably, the ammonia flow rate is 2 to 5 L / min.

[0011] In a second aspect, a zinc nitride is prepared by the above preparation method.

[0012] Compared with the prior art, the present invention has the following obvious beneficial effects: Zinc is sublimated into gaseous state and then reacted with ammonia to prepare zinc nitride. Compared with the prior art in which zinc is in molten state and reacts with ammonia, the reaction area of ​​the raw materials is greatly increased, the reaction efficiency is also faster, and it is suitable for mass production. DETAILED DESCRIPTION

[0013] The present invention provides the following specific technical solutions.

[0014] In a first aspect, the present invention provides a method for preparing zinc nitride, comprising: heating zinc in an inert atmosphere to vaporize it into zinc vapor; preheating ammonia; when the zinc is heated to 800-900° C., introducing ammonia to react the zinc vapor and ammonia in the inert atmosphere, and the powder deposited at the bottom of the reaction system is zinc nitride powder.

[0015] In the prior art, zinc is usually heated to a molten state and reacted with ammonia to produce zinc nitride. The contact between the inside of the molten zinc and the ammonia is limited, and the reaction is incomplete, resulting in limited utilization of the raw materials. After research, the inventors found that heating zinc to sublimate into zinc vapor can greatly increase the reaction area, and the reaction efficiency is also faster, which is suitable for batch production. And preheating ammonia before the reaction of ammonia and zinc vapor, on the one hand, preheating ammonia can accelerate the reaction and shorten the reaction time; on the other hand, preheating ammonia can prevent the zinc vapor from rapidly cooling and liquefying or solidifying when the two are in contact, resulting in zinc powder impurities in the zinc nitride powder, reducing the utilization of the raw materials.

[0016] Preferably, the heating of zinc comprises the following steps: Step 101, heating zinc to 800-900° C. and keeping the temperature for 30-60 minutes; Step 102, then raise the temperature to 950-1050°C and keep it for 15-30 minutes.

[0017] The inventors have found that when heating zinc, first heating it to 800-900°C to melt it, and then raising the temperature to sublime it, zinc vapor can be stably generated, allowing the reaction to proceed continuously.

[0018] More preferably, in step 101, the heating rate is 3-10°C / min.

[0019] More preferably, in step 102, the heating rate is 0.2-1°C / min.

[0020] In the actual production process, the heating rates in step 101 and step 102 can be adjusted according to the actual situation, and the above heating rates are only the preferred ranges given by the inventors. The inventors have found through research that controlling the heating rate in step 102 to be low can make the zinc vapor overflow slowly, so that the zinc vapor and ammonia react fully, thereby improving the utilization rate of the raw materials.

[0021] Preferably, the temperature of the preheated ammonia is 200-300°C.

[0022] In the actual production process, the preheating temperature of ammonia can be adjusted according to the production situation and should be considered together with the ambient temperature during production. The temperature of preheating ammonia is 200-300°C, which is the preferred range proposed by the inventor. If the preheating temperature is too low or not heated, it is easy to cause the zinc vapor to cool down rapidly and liquefy or solidify, reducing the utilization rate of the raw materials; if the preheating temperature is too high, it is easy to cause the ammonia to decompose, resulting in a waste of raw materials.

[0023] Preferably, in step 2, the ammonia flow rate is 2 to 5 L / min.

[0024] In a second aspect, a zinc nitride is prepared by the above preparation method.

[0025] Preferably, the purity of the zinc nitride is ≥4N.

[0026] In order to make the technical problems, technical solutions and technical advantages to be solved by the present invention more clear, they will be described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the following specific embodiments.

[0027] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0029] Embodiment 1: A method for preparing zinc nitride comprises the following steps: Step 1: Load zinc into the heating zone of the reactor, and introduce argon to replace the gas in the reactor.

[0030] Step 2, heating the zinc element, first from room temperature to 800°C at 3°C / min, keeping warm for 60 minutes, then heating to 1050°C at 0.2°C / min, keeping warm for 30 minutes. At the same time, ammonia is introduced into another heating zone of the reactor and heated to 300°C, so that the temperature of the ammonia entering the reaction system is 300°C. When the zinc is heated to 850°C, the heated ammonia is introduced at a flow rate of 3L / min, so that the heated ammonia and zinc vapor react.

[0031] Step 3: After the raw materials react, the reactor is cooled naturally to room temperature, and the powder collected from the bottom of the reactor is zinc nitride.

[0032] Embodiment 2: A method for preparing zinc nitride comprises the following steps: Step 1: Load zinc into the heating zone of the reactor, and introduce argon to replace the gas in the reactor.

[0033] Step 2, heating the zinc element, first from room temperature to 900°C at 10°C / min, keeping warm for 30 minutes, then heating to 1000°C at 0.5°C / min, keeping warm for 20 minutes. At the same time, ammonia is introduced into another heating zone of the reactor and heated to 200°C, so that the temperature of the ammonia entering the reaction system is 200°C. When the zinc is heated to 800°C, the heated ammonia is introduced at a flow rate of 2L / min, so that the heated ammonia and zinc vapor react.

[0034] Step 3: After the raw materials react, the reactor is cooled naturally to room temperature, and the powder collected from the bottom of the reactor is zinc nitride.

[0035] Embodiment 3: A method for preparing zinc nitride comprises the following steps: Step 1: Load zinc into the heating zone of the reactor, and introduce argon to replace the gas in the reactor.

[0036] Step 2, heating the zinc element, first from room temperature to 850°C at 5°C / min, keeping warm for 30 minutes, then heating to 950°C at 1°C / min, keeping warm for 15 minutes. At the same time, ammonia is introduced into another heating zone of the reactor and heated to 250°C, so that the temperature of the ammonia entering the reaction system is 250°C. When the zinc is heated to 900°C, the heated ammonia is introduced at a flow rate of 5L / min, so that the heated ammonia and zinc vapor react.

[0037] Step 3: After the raw materials react, the reactor is cooled naturally to room temperature, and the powder collected from the bottom of the reactor is zinc nitride.

[0038] Embodiment 4: A method for preparing zinc nitride comprises the following steps: Step 1: Load zinc into the heating zone of the reactor, and introduce argon to replace the gas in the reactor.

[0039] Step 2, heating the zinc element, first from room temperature to 800°C at 3°C / min, keeping warm for 60min, then heating to 1050°C at 5°C / min, keeping warm for 30min. At the same time, ammonia is introduced into another heating zone of the reactor and heated to 300°C, so that the temperature of the ammonia entering the reaction system is 300°C. When the zinc is heated to 850°C, the heated ammonia is introduced at a flow rate of 3L / min, so that the heated ammonia and zinc vapor react.

[0040] Step 3: After the raw materials react, the reactor is cooled naturally to room temperature, and the powder collected from the bottom of the reactor is zinc nitride.

[0041] Embodiment 5: A method for preparing zinc nitride comprises the following steps: Step 1: Load zinc into the heating zone of the reactor, and introduce argon to replace the gas in the reactor.

[0042] Step 2, heating zinc element, first from room temperature to 900°C at 10°C / min, keeping the temperature for 30 minutes, then heating to 1000°C at 0.5°C / min, keeping the temperature for 20 minutes. When zinc is heated to 800°C, ammonia is introduced at a flow rate of 2L / min to react ammonia and zinc vapor.

[0043] Step 3: After the raw materials react, the reactor is cooled naturally to room temperature, and the powder collected from the bottom of the reactor is zinc nitride.

[0044] Comparative Example 1: A method for preparing zinc nitride comprises the following steps: Step 1: Fill zinc into the heating zone of the reactor with a filling thickness of 1 mm, and introduce argon to replace the gas in the reactor.

[0045] Step 2, heating the zinc element, first from room temperature to 600°C at 10°C / min, and keeping warm; at the same time, introducing ammonia into another heating zone of the reactor and raising the temperature to 300°C, so that the temperature of the ammonia entering the reaction system is 300°C; then introducing ammonia into the reactor at a flow rate of 2L / min, so that the ammonia and the zinc element heated to 600°C react.

[0046] Step 3: After the raw materials have reacted, the reactor is cooled naturally to room temperature to obtain zinc nitride.

[0047] The nitrogen content in the powder collected in Test Examples 1 to 5 was measured, and the amount of zinc in the zinc nitride product was calculated based on the nitrogen content. The amount of zinc in the zinc nitride product divided by the amount of zinc elemental raw material was the reaction rate of the raw zinc elemental raw material. The test parameters are shown in Table 1.

[0048] Table 1 Reaction rate of zinc in preparing zinc nitride in Examples 1 to 5 By comparing the reaction rates of zinc in Example 1 and Example 4, it can be seen that in the second heating process of zinc, a too fast heating rate of zinc will lead to a decrease in the reaction rate of zinc.

[0049] By comparing the reaction rates of zinc in Example 2 and Example 5, it can be seen that if the ammonia is not heated, the reaction rate of zinc will also decrease. The inventors explored the reason and found that the temperature difference between ammonia and zinc vapor is too large. When the two come into contact, part of the zinc vapor quickly cools down and liquefies or solidifies, turning into zinc powder and depositing at the bottom of the reactor, resulting in a decrease in the utilization rate of the zinc raw material and affecting the purity of the product.

[0050] By comparing the reaction rates of zinc in Example 1 and Comparative Example 1, it can be seen that if the zinc is only heated to 600°C, the zinc is in a molten state and reacts with ammonia, and the reaction rate of the zinc is low. The inventors explored the reason and found that the surface of the zinc in the molten state restricts the entry of ammonia into the interior to a certain extent, and the contact between the internal zinc and ammonia is limited, and the reaction is incomplete, thereby affecting the reaction rate.

[0051] The embodiments described above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the technical scope of the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing zinc nitride, It is characterized in that include: Heat zinc in an inert atmosphere to vaporize it into zinc vapor; preheat ammonia; when the zinc is heated to 800-900°C, introduce ammonia into the reaction system to allow the zinc vapor and ammonia to react in an inert atmosphere, and the powder deposited at the bottom of the reaction system is zinc nitride powder.

2. A method for preparing zinc nitride according to claim 1, It is characterized in that The heating of zinc element includes the following steps: Step 101, heating zinc to 800-900° C. and keeping the temperature for 30-60 minutes; Step 102, then raise the temperature to 950-1050°C and keep it for 15-30 minutes.

3. A method for preparing zinc nitride as claimed in claim 2, It is characterized in that In step 101, the heating rate is 3-10°C / min.

4. A method for preparing zinc nitride according to claim 2 or 3, It is characterized in that In step 102, the heating rate is 0.2-1°C / min.

5. A method for preparing zinc nitride according to claim 1, It is characterized in that The temperature of the preheated ammonia is 200-300°C.

6. A method for preparing zinc nitride according to claim 1 or 5, It is characterized in that The flow rate of ammonia is 2-5 L / min.

7. A zinc nitride, It is characterized in that Prepared by the preparation method described in any one of claims 1 to 6.