Positive polarity infrared LED epitaxial structure and preparation method thereof

By using the superlattice structure of C-doped AlGaAs and Mg-doped AlGaAs layers alternately laminated in the epitaxial structure of positive polar infrared LEDs, and combined with cyclic annealing treatment, the problems of light absorption and electrical uniformity of the P-type layer are solved, and the Luminous efficiency and yield.

CN118919623AActive Publication Date: 2024-11-08JIANGXI YAOCHI TECH CO LTD +1

Patent Information

Application Number
CN202411183507.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

In the existing epitaxial structure of positive polar infrared LEDs, the P-type layer material has a large light absorption, which is prone to epitaxial defects and electrical properties, which affects the luminous efficiency and uniformity.

Method used

The P-AlGaAs current expansion layer is used to form a superlattice structure formed by periodically alternately laminaring of C-doped AlGaAs layer and Mg-doped AlGaAs layer. Through cyclic annealing treatment, the Mg element is diffused in the C-doped AlGaAs layer to increase the holes. Solubility and electrical uniformity.

Benefits of technology

The light absorption of the P-type layer is reduced, the crystal quality and luminous efficiency of the epitaxial layer are improved, the electrical uniformity on the chip is enhanced, and the luminous intensity and yield of the LED are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919623A_ABST
    Figure CN118919623A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor materials, and discloses an epitaxial structure of a positive polarity infrared LED and a preparation method of the epitaxial structure, and the epitaxial structure comprises a buffer layer, an N-AlGaAs current expansion layer, an N-AlGaAs limiting layer, a multi-quantum well layer, a P-AlGaAs limiting layer, a P-AlGaAs current expansion layer and a P-type GaAs ohmic contact layer which are sequentially stacked. The P-AlGaAs current expansion layer is a superlattice formed by periodically and alternately laminating the C-doped AlGaAs layer and the Mg-doped AlGaAs layer, so that the hole distribution of the epitaxial layer is more uniform, the epitaxial layer with high quality and high uniformity is grown, the yield of the LED chip is improved, the light absorption is reduced, and the luminous efficiency and the luminous intensity are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor materials, and in particular to an epitaxial structure of a positive-polarity infrared LED and a preparation method thereof. Background Art

[0002] Infrared LED is a near-infrared light-emitting device that converts electrical energy into light energy. Its wavelength is concentrated in the range of 1μm-3μm. It has a series of advantages such as small size, low power consumption, long life, high stability, good directionality, etc. At present, infrared LED is widely used in remote control, telemetry, optical isolation, optical switch, photoelectric control, target tracking and other systems.

[0003] In the prior art, in the epitaxial structure of the positive polarity infrared LED, the P-type layer material is AlGaAs, and the doping element is Mg or C, but the following defects still exist: when Mg is used for doping, the window of epitaxial growth is small, epitaxial defects caused by Mg are more likely to occur, and light absorption is serious; when C is used for doping, the requirements for the temperature and airflow of the reaction chamber are relatively high. For example, when growing a C-doped epitaxial layer in the Aixtron-G4-15 chip machine device, due to the large size of the small disk and the water cooling of the edge side wall, it is very easy for the C doping amount of the flat edge to be 1 to 2 times higher than that of the round edge, resulting in a large difference in electrical properties within the chip. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an epitaxial structure of a positive infrared LED and a preparation method thereof, which can reduce the light absorption of the P-type layer, make the hole concentration in the epitaxial wafer uniform, and improve the crystal quality of the epitaxial layer.

[0005] In order to solve the above technical problems, the first aspect of the present invention provides an epitaxial structure of a positive polarity infrared LED, characterized in that it includes a buffer layer, an N-AlGaAs current spreading layer, an N-AlGaAs limiting layer, a multi-quantum well layer, a P-AlGaAs limiting layer, a P-AlGaAs current spreading layer, and a P-type GaAs ohmic contact layer stacked in sequence;

[0006] The P-AlGaAs current spreading layer is a superlattice formed by periodically alternating stacking of C-doped AlGaAs layers and Mg-doped AlGaAs layers, with the number of periods being 33 to 150. In each period, the C-doped AlGaAs layer is located below the Mg-doped AlGaAs layer.

[0007] As an improvement of the above solution, the total thickness of the P-AlGaAs current spreading layer is 4 μm to 9 μm.

[0008] As an improvement of the above solution, the thickness of the C-doped AlGaAs layer is 30 nm to 60 nm, and the thickness of the Mg-doped AlGaAs layer is 30 nm to 60 nm.

[0009] As an improvement of the above solution, the hole solubility in the P-AlGaAs current spreading layer is greater than 3.5×10 18 cm -3 , the doping amount of the C-doped AlGaAs layer is less than the doping amount of the Mg-doped AlGaAs layer.

[0010] As an improvement of the above solution, the C doping amount in the C-doped AlGaAs layer is 3×10 18 cm -3 ~4×10 18 cm -3 ;

[0011] The doping amount of Mg in the Mg-doped AlGaAs layer is 3.5×10 18 cm -3 ~4.5×10 18 cm -3 .

[0012] As an improvement of the above solution, the Al component in the C-doped AlGaAs layer is 0.1-0.4;

[0013] The Al content in the Mg-doped AlGaAs layer is 0.1-0.4.

[0014] As an improvement of the above solution, the growth temperature of the C-doped AlGaAs layer is 650° C. to 720° C., and the growth pressure is 30 to 80 mbar;

[0015] The growth temperature of the Mg-doped AlGaAs layer is 650° C. to 720° C., and the growth pressure is 30 to 80 mbar.

[0016] As an improvement of the above solution, the Mg-doped AlGaAs layer is annealed after growth, and then the next period of C-doped AlGaAs layer is grown. The annealing treatment is: maintaining the temperature at 650° C. to 720° C. for 5s to 10s.

[0017] The second aspect of the present invention further provides a method for preparing the epitaxial structure of the positive polarity infrared LED, comprising:

[0018] growing a buffer layer on the substrate;

[0019] Growing an N-AlGaAs current spreading layer on the buffer layer;

[0020] Growing an N-AlGaAs confinement layer on the N-AlGaAs current spreading layer;

[0021] Growing a multi-quantum well layer on the N-AlGaAs confinement layer;

[0022] Growing a P-AlGaAs confinement layer on the multi-quantum well layer;

[0023] growing a P-AlGaAs current spreading layer on the P-AlGaAs confinement layer;

[0024] Growing a P-type GaAs ohmic contact layer on the P-AlGaAs current spreading layer;

[0025] The P-AlGaAs current spreading layer is a superlattice formed by periodically alternating stacking of a C-doped AlGaAs layer and a Mg-doped AlGaAs layer, wherein in each period, the C-doped AlGaAs layer is located below the Mg-doped AlGaAs layer;

[0026] As an improvement of the above scheme, growing a P-AlGaAs current extension layer on the P-AlGaAs confinement layer comprises:

[0027] (1) controlling the temperature of the reaction chamber to be maintained at 650° C. to 720° C., and growing a C-doped AlGaAs layer using a C source, an Al source, a Ga source, and an As source;

[0028] (2) Turn off the C source, introduce the Mg source, Al source, Ga source, and As source to grow the Mg-doped AlGaAs layer, and complete one cycle of growth;

[0029] (3) Turn off the Group III source and Mg source, maintain the temperature and perform annealing for 5s to 10s;

[0030] (4) Repeat steps (1) to (3) until the thickness or the number of cycles reaches a preset value.

[0031] The implementation of the present invention has the following beneficial effects:

[0032] In the present invention, a P-AlGaAs current spreading layer is arranged on a P-AlGaAs confinement layer and a P-type GaAs ohmic contact layer, and the P-AlGaAs current spreading layer is a superlattice formed by periodically and alternately stacking a C-doped AlGaAs layer and a Mg-doped AlGaAs layer. Compared with a traditional Mg-doped structure, it is easier to grow a high-quality epitaxial layer, the epitaxial defects are less, the light absorption of C-doping is less than that of Mg-doping, and the epitaxial luminescence efficiency can be effectively improved. Compared with a traditional C-doped structure, it is easier to grow a P-AlGaAs with high uniformity, the electrical uniformity within the chip is greatly improved compared with single C-doping, and the luminescence intensity is improved.

[0033] The present invention adopts a cyclic annealing method to diffuse Mg doping in the C-doped AlGaAs layer, so that the C-doped AlGaAs layer, which is very sensitive to temperature, has better hole solubility uniformity in the wafer due to the diffusion of Mg doping, and the electrical yield in the wafer is greatly improved, further improving the yield of the epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 : A schematic diagram of the structure of an epitaxial structure of a positive polarity infrared LED in the present invention;

[0035] Figure 2 : A method for preparing an epitaxial structure of a positive polarity infrared LED in the present invention;

[0036] Figure 3 : Schematic diagram of the flow rates of Al source, Ga source, C source and Mg source in steps (1) to (3) of Example 1 of the present invention (source amount of MO source).

[0037] Reference numerals:

[0038] 1-buffer layer; 2-N-AlGaAs current spreading layer; 3-N-AlGaAs confinement layer; 4-multiple quantum well layer; 5-P-AlGaAs confinement layer; 6-P-AlGaAs current spreading layer; 61-C-doped AlGaAs layer; 62-Mg-doped AlGaAs layer; 7-P-type GaAs ohmic contact layer. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail with specific embodiments below.

[0040] In order to solve the above problems, the present invention provides a positive polarity infrared LED epitaxial structure in the first aspect, see Figure 1 , including a buffer layer 1, an N-AlGaAs current spreading layer 2, an N-AlGaAs confinement layer 3, a multi-quantum well layer 4, a P-AlGaAs confinement layer 5, a P-AlGaAs current spreading layer 6, and a P-type GaAs ohmic contact layer 7 which are stacked in sequence;

[0041] The P-AlGaAs current spreading layer 6 is a superlattice formed by periodically alternating stacking of a C-doped AlGaAs layer 61 and a Mg-doped AlGaAs layer 62 , with the number of periods being 33 to 150. In each period, the C-doped AlGaAs layer 61 is located below the Mg-doped AlGaAs layer 62 .

[0042] In 3×10 18 cm -3Among the above high-solubility impurity semiconductors, the Mg-doped AlGaAs material epitaxial layer has more defects when the thickness is relatively large. In the present invention, a structure in which C-doped AlGaAs layers 61 and Mg-doped AlGaAs layers 62 are periodically alternately stacked is adopted. Through periodic annealing, the Mg element can be uniformly diffused in the AlGaAs epitaxial layer, which can increase the hole concentration and achieve the ideal high doping. At the same time, a higher quality AlGaAs epitaxial layer is obtained, so that the surface defects of the epitaxial layer are fewer and the light extraction efficiency of the LED is higher.

[0043] Preferably, the hole solubility in the P-AlGaAs current spreading layer 6 is greater than 3.5×10 18 cm -3 The doping amount of the C-doped AlGaAs layer 61 is less than that of the Mg-doped AlGaAs layer 62, which is beneficial to the diffusion of the Mg element, can effectively reduce the ionization energy of the Mg impurities, and can regulate the defect state in the material and increase the hole concentration of the doping layer, thereby improving the efficiency of p-type doping.

[0044] Furthermore, the Al content in the C-doped AlGaAs layer 61 is 0.1-0.4, and the C doping amount is 3×10 18 cm -3 ~4×10 18 cm -3 , an exemplary doping level is 3×10 18 cm -3 , 3.2×10 18 cm -3 , 3.4×10 18 cm -3 , 3.6×10 18 cm -3 , 3.8×10 19 cm -3 , 4×10 18 cm -3 , but not limited thereto; the Al component in the Mg-doped AlGaAs layer 62 is 0.1 to 0.4, and the Mg doping amount is 3.5×10 18 cm -3 ~4.5×10 18 cm -3 , an exemplary doping level is 3.5×10 18 cm -3 , 3.7×10 18 cm -3 , 3.9×10 18 cm -3 , 4.1×10 18 cm -3 , 4.3×10 18 cm-3 , 4.5×10 18 cm -3 , but not limited to this.

[0045] Preferably, the exemplary number of periods in the present invention is 33, 35, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, but not limited thereto. The total thickness of the P-AlGaAs current spreading layer 6 is 4 μm to 9 μm, and exemplary ones are 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, but not limited thereto. Controlling the thickness of the P-AlGaAs current spreading layer 6 to be 4 μm to 9 μm can evenly distribute the injected carriers to the active area, reduce the carrier crowding effect, and thus improve the luminous efficiency and uniformity of the LED. If the thickness is too high, the crystal quality of the Mg-doped AlGaAs layer 62 will be reduced, and the carriers will be extended too far, affecting the luminous efficiency.

[0046] Further, the thickness of the C-doped AlGaAs layer 61 is 30nm to 60nm, and exemplary thicknesses are 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, and 60nm, but not limited thereto; the thickness of the Mg-doped AlGaAs layer 62 is 30nm to 60nm, and exemplary thicknesses are 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, and 60nm, but not limited thereto.

[0047] Furthermore, after the growth of the Mg-doped AlGaAs layer 62 is completed, an annealing treatment is performed, and then the next cycle of C-doped AlGaAs layer 61 is grown. The annealing treatment is: maintaining the temperature at 650°C to 720°C for 5s to 10s. By using the cyclic annealing method, the Mg doped in the Mg-doped AlGaAs layer 62 is diffused in the C-doped AlGaAs layer 61, so that the C-doped AlGaAs layer 61, which is very sensitive to temperature, has a better hole solubility uniformity in the chip due to the diffusion of Mg doping, and the electrical yield in the chip is greatly improved.

[0048] Accordingly, the present invention also provides a method for preparing an epitaxial structure of a positive polarity infrared LED, see Figure 2 ,include:

[0049] S01, growing a buffer layer 1 on a substrate;

[0050] In the present invention, the epitaxial structure of the positive polarity infrared LED is deposited and grown in the MOCVD equipment. Before growing the buffer layer 1, pretreatment is required. The pretreatment includes: adjusting the pressure of the reaction chamber, introducing hydrogen and arsine, adjusting the temperature in the reaction chamber and performing baking treatment; the introduction of hydrogen and arsine can clean the surface of the substrate and remove oxides and other contaminants on the surface of the substrate. The pressure in the reaction chamber is kept low, and the pressure is 30mbar to 70mbar, preferably 50mbar.

[0051] Furthermore, the temperature of the reaction chamber is adjusted to 730°C to 78°C for a baking treatment with a baking time of 3min to 8min. The baking treatment can reduce defects in the material, promote the migration and reaction of atoms on the substrate surface, thereby increasing the growth rate and improving the interface quality between the epitaxial structure and the substrate.

[0052] The type of substrate in the present invention is not limited, and may be a silicon substrate, a GaAs substrate, etc., which are not marked in the figure.

[0053] Preferably, the buffer layer 1 is a GaAs buffer layer 1, and the thickness of the buffer layer 1 is 100 nm to 400 nm.

[0054] Furthermore, the buffer layer 1 is a Si-doped GaAs buffer layer 1, and the Si doping amount is 1×10 18 cm -3 ~2×10 18 cm -3 .

[0055] Furthermore, the growth temperature of the buffer layer 1 is 650° C. to 720° C., and the growth pressure is 30 mbar to 70 mbar.

[0056] S02, growing an N-AlGaAs current spreading layer 2 on the buffer layer 1;

[0057] Preferably, the doping element of the N-AlGaAs current spreading layer 2 is Si, and the doping amount of Si is 1×10 18 cm -3 ~4×10 18 cm -3 The thickness of the N-AlGaAs current spreading layer 2 is 0.2 μm to 3 μm.

[0058] Furthermore, the growth temperature of the N-AlGaAs current spreading layer 2 is 650° C. to 720° C., and the growth pressure is 30 mbar to 70 mbar.

[0059] S03, growing an N-AlGaAs confinement layer 3 on the N-AlGaAs current spreading layer 2;

[0060] Preferably, the doping element of the N-AlGaAs confinement layer 3 is Si, and the doping amount of Si is 1×10 18 cm -3 ~4×10 18 cm -3 The thickness of the N-AlGaAs current spreading layer 2 is 100nm to 500nm.

[0061] Furthermore, the growth temperature of the N-AlGaAs confinement layer 3 is 650° C. to 720° C., and the growth pressure is 30 mbar to 70 mbar.

[0062] S04, growing a multi-quantum well layer 4 on the N-AlGaAs confinement layer 3;

[0063] Preferably, the multi-quantum well layer 4 is a periodic structure of alternately stacked InGaAs quantum well layers and AlGaAs quantum barrier layers, with a period number of 4 to 30, the In component of the InGaAs quantum well layer is 0.1 to 0.15, and the thickness is 5 nm to 10 nm; the Al component of the AlGaAs quantum barrier layer is 0.02 to 0.1, and the thickness is 10 nm to 30 nm.

[0064] Furthermore, the growth temperature of the InGaAs quantum well layer and the AlGaAs quantum barrier layer are both 650° C. to 680° C., and the growth pressure is 30 mbar to 70 mbar.

[0065] S05, growing a P-AlGaAs confinement layer 5 on the multi-quantum well layer 4;

[0066] Preferably, the doping element of the P-AlGaAs confinement layer 5 is C, and the doping amount of C is 2×10 18 cm -3 ~4×10 18 cm -3 The thickness of the P-AlGaAs confinement layer 5 is 100nm to 500nm.

[0067] Furthermore, the growth temperature of the N-AlGaAs current spreading layer 2 is 650° C. to 720° C., and the growth pressure is 30 mbar to 70 mbar.

[0068] S06, growing a P-AlGaAs current spreading layer 6 on the P-AlGaAs confinement layer 5;

[0069] Preferably, the growth temperature of the C-doped AlGaAs layer 61 is 650°C to 720°C, exemplarily 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, but not limited thereto; the growth pressure is 30 to 80 mbar, exemplarily 30 mbar, 40 mbar, 50 mbar, 60 mbar, 70 mbar, 80 mbar, but not limited thereto. The growth temperature of the Mg-doped AlGaAs layer 62 is 650°C to 720°C, exemplarily 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, but not limited thereto; the growth pressure is 30 to 80 mbar, exemplarily 30 mbar, 40 mbar, 50 mbar, 60 mbar, 70 mbar, 80 mbar, but not limited thereto.

[0070] Further, when growing the C-doped AlGaAs layer 61, the ratio of the flow rate of the Al source to the C source in the C-doped AlGaAs layer 61 is 1:(0.23-0.28), exemplarily 1:0.23, 1:0.24, 1:0.25, 1:0.26, 1:0.27, 1:0.28, but not limited thereto. When growing the Mg-doped AlGaAs layer 62, the ratio of the flow rate of the Al source to the C source is 1:(0.3-0.35), exemplarily 1:0.3, 1:0.31, 1:0.32, 1:0.33, 1:0.34, 1:0.35, but not limited thereto. Controlling the Al source and the doping element C source or Mg source when growing the C-doped AlGaAs layer 61 or the Mg-doped AlGaAs layer 62 is beneficial to promoting the uniformity of the P-AlGaAs current spreading layer 6, ensuring the addition of a sufficient amount of doping elements, and increasing the hole concentration as much as possible.

[0071] Furthermore, after the growth of the Mg-doped AlGaAs layer 62 is completed, an annealing treatment is performed, and then the next cycle of C-doped AlGaAs layer 61 is grown. The annealing treatment is: maintaining the temperature at 650°C to 720°C for 5s to 10s. By using the cyclic annealing method, the Mg doped in the Mg-doped AlGaAs layer 62 is diffused in the C-doped AlGaAs layer 61, so that the C-doped AlGaAs layer 61, which is very sensitive to temperature, has a better hole solubility uniformity in the chip due to the diffusion of Mg doping, and the electrical yield in the chip is greatly improved.

[0072] In some specific and preferred embodiments, step S06 includes:

[0073] (1) controlling the temperature of the reaction chamber to be maintained at 650° C. to 720° C., and growing a C-doped AlGaAs layer 61 through a C source, an Al source, a Ga source, and an As source;

[0074] (2) Turn off the C source, and introduce the Mg source, Al source, Ga source, and As source to grow the Mg-doped AlGaAs layer 62, completing one cycle of growth;

[0075] (3) Turn off the Group III source and Mg source, maintain the temperature and perform annealing for 5s to 10s;

[0076] (4) Repeat steps (1) to (3) until the thickness or the number of cycles reaches a preset value.

[0077] S07 . Growing a P-type GaAs ohmic contact layer 7 on the P-AlGaAs current spreading layer 6 .

[0078] Preferably, the doping element of the P-type GaAs ohmic contact layer 7 is C, and the doping amount of C is 7×10 19 cm -3 ~2×10 20 cm -3 The thickness of the P-type GaAs ohmic contact layer 7 is 30 nm to 150 nm.

[0079] Furthermore, the growth temperature of the P-type GaAs ohmic contact layer 7 is 580° C. to 630° C., and the growth pressure is 30 mbar to 70 mbar.

[0080] It should be noted that the use of high-purity H 2 (hydrogen) as carrier gas, As source is AsH (arsine), N source is high purity NH 3 , the Al source is TMAl (trimethylaluminum), the Ga source is TMGa (trimethylgallium), the In source is TMIn (trimethylindium), and the Si source is SiH 4 , the Mg source is CP2Mg.

[0081] The present invention will be further described below with specific embodiments:

[0082] Example 1

[0083] This embodiment provides an epitaxial structure of a positive polarity infrared LED, comprising a buffer layer, an N-AlGaAs current spreading layer, an N-AlGaAs limiting layer, a multi-quantum well layer, a P-AlGaAs limiting layer, a P-AlGaAs current spreading layer, and a P-type GaAs ohmic contact layer stacked in sequence.

[0084] The P-AlGaAs current spreading layer is a superlattice formed by periodically alternating stacking of C-doped AlGaAs layers and Mg-doped AlGaAs layers, and in each period, the C-doped AlGaAs layer is located below the Mg-doped AlGaAs layer.

[0085] The Al component of the C-doped AlGaAs layer is 0.25, and the C doping amount is 3.0×10 18 cm -3 , with a thickness of 45 nm; the Al composition of the Mg-doped AlGaAs layer is 0.25, and the Mg doping amount is 4.0×10 18 cm -3 , thickness is 50nm, number of periods is 53, and total thickness is 5.035μm.

[0086] The hole solubility in the P-AlGaAs current spreading layer is 3.5×10 18 cm -3 .

[0087] It is prepared by the following preparation method:

[0088] S01. In the MOCVD equipment, maintain a low pressure of 50 mbar, introduce hydrogen and arsine, increase the temperature to 750°C, bake at high temperature for 5 minutes, and then grow a buffer layer on the substrate;

[0089] The buffer layer is a Si-doped GaAs buffer layer, and the Si doping amount is 1.5×10 18 cm -3 .

[0090] Specifically, the temperature was lowered to 690° C., and Ga source, As source and Si source were introduced to grow a Si-doped GaAs buffer layer with a thickness of 250 nm.

[0091] S02. Growing N-AlGaAs current spreading layer on the buffer layer

[0092] The doping element of the N-AlGaAs current spreading layer is Si, and the doping amount of Si is 2.5×10 18 cm -3 .

[0093] Specifically, the temperature was maintained at 690° C., and Ga source, Al source, As source and Si source were introduced to grow an N—AlGaAs current spreading layer with a thickness of 1.5 μm.

[0094] S03, growing an N-AlGaAs confinement layer on the N-AlGaAs current spreading layer

[0095] The doping element of the N-AlGaAs confinement layer is Si, and the doping amount of Si is 3×10 18 cm -3 .

[0096] Specifically, the temperature was maintained at 690° C., and Ga source, Al source, As source and Si source were introduced to grow an N—AlGaAs confinement layer with a thickness of 300 nm.

[0097] S04. Growing a multi-quantum well layer on the N-AlGaAs confinement layer

[0098] The multi-quantum well layer is a periodic structure of alternately stacked InGaAs quantum well layers and AlGaAs quantum barrier layers, with a period number of 15. The In component of the InGaAs quantum well layer is 0.12 and the thickness is 7nm; the Al component of the AlGaAs quantum barrier layer is 0.05 and the thickness is 20nm.

[0099] Specifically, the temperature is lowered to 665°C, and Ga source, In source, and As source are introduced to grow an InGaAs quantum well layer. Subsequently, the In source is turned off, and Ga source, Al source, and As source are introduced to grow an AlGaAs quantum barrier layer to complete one cycle of growth. Subsequently, the quantum well layer and quantum barrier layer are repeatedly stacked and grown for 14 cycles.

[0100] S05. Growing a P-AlGaAs confinement layer on the multi-quantum well layer

[0101] The doping element of the P-AlGaAs confinement layer is C, and the doping amount of C is 3×10 18 cm -3 , with a thickness of 300nm.

[0102] Specifically, the temperature was raised to 690° C., and Ga source, Al source, As source, and C source were introduced to grow a P-AlGaAs confinement layer.

[0103] S06, growing a P-AlGaAs current spreading layer on the P-AlGaAs confinement layer;

[0104] The P-AlGaAs current spreading layer is a superlattice formed by periodically and alternately stacking a C-doped AlGaAs layer and a Mg-doped AlGaAs layer. In each period, the C-doped AlGaAs layer is located below the Mg-doped AlGaAs layer.

[0105] Specifically:

[0106] (1) The temperature is maintained at 690° C. and a C-doped AlGaAs layer is grown using a C source, an Al source, a Ga source, and an As source;

[0107] (2) Turn off the C source, introduce the Mg source, Al source, Ga source, and As source to grow the Mg-doped AlGaAs layer, and complete one cycle of growth;

[0108] (3) Turn off the Group III source and Mg source, maintain the temperature and perform annealing for 8 seconds;

[0109] (4) Repeat steps (1) to (3) 52 times to complete the growth of the P-AlGaAs current spreading layer.

[0110] The flow rates of Al source, Ga source, C source and Mg source in steps (1) to (3) are as follows: Figure 3 As shown (since the saturated vapor pressure of Al is lower than that of Ga, the source flow rate must be much larger to be consistent with the mol amount of the Ga source).

[0111] S07. Growing a P-type GaAs ohmic contact layer on the P-AlGaAs current spreading layer.

[0112] The doping element of the P-type GaAs ohmic contact layer is C, and the doping amount of C is 7×10 19 cm -3 ~2×10 20 cm -3 The thickness of the P-type GaAs ohmic contact layer is 30nm to 150nm.

[0113] Specifically, the temperature was lowered to 600° C., and a C source, a Ga source, and an As source were introduced to grow a P-type GaAs ohmic contact layer with a thickness of 90 nm.

[0114] Example 2

[0115] This embodiment provides an epitaxial structure of a positive polarity infrared LED, which is basically the same as that of Embodiment 1, except that:

[0116] The Al component of the C-doped AlGaAs layer is 0.25, and the C doping amount is 3.5×10 18 cm -3 ; The Al composition of the Mg-doped AlGaAs layer is 0.25, and the Mg doping amount is 4.5×10 18 cm -3 .

[0117] Example 3

[0118] This embodiment provides an epitaxial structure of a positive polarity infrared LED, which is basically the same as that of Embodiment 1, except that:

[0119] The thickness of the C-doped AlGaAs layer is 30 nm; the thickness of the Mg-doped AlGaAs layer is 60 nm.

[0120] Example 4

[0121] This embodiment provides an epitaxial structure of a positive polarity infrared LED, which is basically the same as that of Embodiment 1, except that:

[0122] In S06 of the preparation method, the next cycle of growth is carried out without undergoing cyclic annealing treatment.

[0123] Specifically:

[0124] (1) The temperature is maintained at 690° C. and a C-doped AlGaAs layer is grown using a C source, an Al source, a Ga source, and an As source;

[0125] (2) Turn off the C source, introduce the Mg source, Al source, Ga source, and As source to grow the Mg-doped AlGaAs layer, and complete one cycle of growth;

[0126] (3) Repeat steps (1) to (2) 52 times to complete the growth of the P-AlGaAs current spreading layer.

[0127] Comparative Example 1

[0128] This comparative example provides an epitaxial structure of a positive polarity infrared LED, which is basically the same as that of Example 1, except that:

[0129] The P-AlGaAs current spreading layer is a C-doped AlGaAs layer with a thickness of 5.035 μm and a C doping amount of 3.5×10 18 cm -3 , the hole solubility is 3.5×10 18 cm -3 .

[0130] Comparative Example 2

[0131] This comparative example provides an epitaxial structure of a positive polarity infrared LED, which is basically the same as that of Example 1, except that:

[0132] The P-AlGaAs current spreading layer is a Mg-doped AlGaAs layer with a thickness of 5.035 μm and a Mg doping amount of 3.5×10 18 cm -3 , the hole solubility is 3.5×10 18 cm -3 .

[0133] Comparative Example 3

[0134] This comparative example provides an epitaxial structure of a positive polarity infrared LED, which is basically the same as that of Example 1, except that:

[0135] The epitaxial structure of the positive polarity infrared LED comprises a buffer layer, an N-AlGaAs current spreading layer, an N-AlGaAs limiting layer, a multi-quantum well layer, a P-AlGaAs limiting layer, and a P-type GaAs ohmic contact layer which are stacked in sequence.

[0136] Performance Testing

[0137] The epitaxial wafers obtained in the embodiment and the comparative example were made into 8*8μm chips for photoelectric performance testing. The specific chip testing method is: when a current of 20mA is passed, the light efficiency improvement rate, luminous intensity and yield of the obtained chip are tested; wherein the light efficiency improvement rate is calculated based on comparative example 3 which does not contain a P-AlGaAs current extension layer.

[0138] The test results are shown in Table 1 below.

[0139] Table 1 Test results of LED chips obtained in the embodiments and comparative examples

[0140] Light efficiency improvement rate (%) Luminous intensity (mW) Yield (%) Example 1 82.9 7.5 96.2 Example 2 78.0 7.3 95.5 Example 3 68.3 6.9 95.7 Example 4 53.7 6.3 85.9 Comparative Example 1 48.8 6.1 87.5 Comparative Example 2 53.7 6.3 84.3 Comparative Example 3 0 4.1 55.5

[0141] From the above results, it can be seen that a P-AlGaAs current spreading layer is arranged on the P-AlGaAs confinement layer and the P-type GaAs ohmic contact layer, and the P-AlGaAs current spreading layer is a superlattice formed by periodically alternating stacking of C-doped AlGaAs layers and Mg-doped AlGaAs layers, and combined with a cyclic annealing process, it is beneficial to distribute the holes in the epitaxial layer more evenly, grow a high-quality, high-uniformity epitaxial layer, improve the yield of the LED chip, reduce light absorption, and effectively improve the luminous efficiency and luminous intensity.

[0142] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. An epitaxial structure of a positive polarity infrared LED, characterized in that: It includes a buffer layer, an N-AlGaAs current expansion layer, an N-AlGaAs limiting layer, a multi-quantum well layer, a P-AlGaAs limiting layer, a P-AlGaAs current expansion layer, and a P-type GaAs ohmic contact layer which are stacked in sequence; The P-AlGaAs current spreading layer is a superlattice formed by periodically alternating stacking of C-doped AlGaAs layers and Mg-doped AlGaAs layers, with the number of periods being 33 to 150. In each period, the C-doped AlGaAs layer is located below the Mg-doped AlGaAs layer.

2. The epitaxial structure of the positive polarity infrared LED according to claim 1, characterized in that: The total thickness of the P-AlGaAs current spreading layer is 4 μm to 9 μm.

3. The epitaxial structure of a positive polarity infrared LED as claimed in claim 1 or 2, characterized in that: The thickness of the C-doped AlGaAs layer is 30nm-60nm, and the thickness of the Mg-doped AlGaAs layer is 30nm-60nm.

4. The epitaxial structure of the positive polarity infrared LED according to claim 1, characterized in that: The hole solubility in the P-AlGaAs current spreading layer is greater than 3.5×10 18 cm -3 , the doping amount of the C-doped AlGaAs layer is less than the doping amount of the Mg-doped AlGaAs layer.

5. The epitaxial structure of the positive polarity infrared LED according to claim 4, characterized in that: The doping amount of C in the C-doped AlGaAs layer is 3×10 18 cm -3 ~4×10 18 cm -3 ; The doping amount of Mg in the Mg-doped AlGaAs layer is 3.5×10 18 cm -3 ~4.5×10 18 cm -3 .

6. The epitaxial structure of the positive polarity infrared LED according to claim 1, characterized in that: The Al content in the C-doped AlGaAs layer is 0.1-0.4; The Al content in the Mg-doped AlGaAs layer is 0.1-0.

4.

7. The epitaxial structure of the positive polarity infrared LED according to claim 1, characterized in that: The growth temperature of the C-doped AlGaAs layer is 650° C. to 720° C., and the growth pressure is 30 to 80 mbar; The growth temperature of the Mg-doped AlGaAs layer is 650° C. to 720° C., and the growth pressure is 30 to 80 mbar.

8. The epitaxial structure of the positive polarity infrared LED according to claim 7, characterized in that: After the growth of the Mg-doped AlGaAs layer is completed, an annealing treatment is performed, and then a C-doped AlGaAs layer of the next cycle is grown. The annealing treatment is: maintaining the temperature at 650° C. to 720° C. for 5 seconds to 10 seconds.

9. A method for preparing an epitaxial structure of a positive polarity infrared LED as claimed in any one of claims 1 to 8, characterized in that: include: growing a buffer layer on the substrate; Growing an N-AlGaAs current spreading layer on the buffer layer; Growing an N-AlGaAs confinement layer on the N-AlGaAs current spreading layer; Growing a multi-quantum well layer on the N-AlGaAs confinement layer; Growing a P-AlGaAs confinement layer on the multi-quantum well layer; growing a P-AlGaAs current spreading layer on the P-AlGaAs confinement layer; Growing a P-type GaAs ohmic contact layer on the P-AlGaAs current spreading layer; The P-AlGaAs current spreading layer is a superlattice formed by periodically alternating stacking of C-doped AlGaAs layers and Mg-doped AlGaAs layers, and in each period, the C-doped AlGaAs layer is located below the Mg-doped AlGaAs layer.

10. The method for preparing the epitaxial structure of a positive polarity infrared LED according to claim 9, characterized in that: Growing a P-AlGaAs current spreading layer on a P-AlGaAs confinement layer includes: (1) controlling the temperature of the reaction chamber to be maintained at 650° C. to 720° C., and growing a C-doped AlGaAs layer using a C source, an Al source, a Ga source, and an As source; (2) Turn off the C source, introduce the Mg source, Al source, Ga source, and As source to grow the Mg-doped AlGaAs layer, and complete one cycle of growth; (3) Turn off the Group III source and Mg source, maintain the temperature and perform annealing for 5s to 10s; Repeat steps (1) to (3) until the thickness or number of cycles reaches a preset value.

Citation Information

Patent Citations

  • Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode

    CN115832138A

  • Infrared LED chip and preparation method thereof

    CN116978993A

  • Light emitting diode epitaxial structure and forming method thereof

    CN118099306A

  • Nitride semiconductor LED and fabrication method thereof

    KR100580752B1

Cited By

  • Red light LED epitaxial wafer and preparation method thereof

    CN119403314A

  • A red light LED epitaxial wafer and preparation method thereof

    CN119403314B

  • Method for improving epitaxial growth quality of tunnel junction cascade semiconductor laser