Cement seepage-proofing agent and application thereof in concrete
Through the cationic bridging, electrostatic attraction and hydrogen bonding of anionic polymer and bentonite, a cement anti-seepage agent is prepared, which solves the problem of cement anti-seepage agent affecting the mechanical properties and environmental friendliness in the existing technology, and achieves efficient Impermeable properties and low cost for mass production.
Patent Information
- Application Number
- CN202410845508.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
AI Technical Summary
When existing cement anti-seepage agents improve the impermeability of concrete, they usually affect the mechanical properties or have environmentally unfriendly problems, and there is a lack of low-cost, excellent-performance modifiers that can be mass-produced.
An anionic polymer and bentonite are combined through cationic bridging, electrostatic attraction and hydrogen bonding to prepare a cement anti-seepage agent. The intercalation reaction efficiency is improved through extrusion and standing processes to form a product with better anti-seepage properties.
Significantly reduced the permeability coefficient of concrete from 10-5 to 10-8, improved density and tolerance to high-salt pollutants, shortened curing time, reduced project costs, extended project progress, and improved improve the quality of concrete.
Smart Images

Figure BDA0004915574800000131 
Figure BDA0004915574800000132 
Figure BDA0004915574800000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete additives, in particular to a cement anti-seepage agent and application thereof in concrete. Background Art
[0002] At present, the research on cement anti-seepage agent technology shows a diversified trend. Traditional cement modifiers include various inorganic salts, organosilicon, polymers, silicates and nanomaterials, which improve the density and impermeability of concrete by filling the microscopic pores in cement-based materials or reacting chemically with the surface of cement particles. However, while these traditional modifiers improve the impermeability of concrete, they often have a negative impact on the mechanical properties of concrete or are environmentally unfriendly. For example, inorganic iron and aluminum salt modifiers are prone to passivation and easy to corrode steel materials in buildings; silicon-based modifiers affect the mechanical properties of cement and are environmentally unfriendly; organic polymer modifiers are often expensive and not conducive to large-scale use.
[0003] In recent years, researchers have begun to explore more environmentally friendly and efficient cement anti-seepage agents, such as using natural organic matter or biomass-derived ingredients for modification, so as to improve the impermeability of concrete while maintaining its mechanical properties and environmental friendliness. In addition, another research focus is on the development of cement anti-seepage agents with dual or multiple modification mechanisms, through the synergistic effect between different components, to achieve more comprehensive and effective concrete modification. However, new modifiers are often expensive and remain in the laboratory stage. The feasibility of large-scale mass production and product stability remain to be demonstrated. There is still a lack of low-cost, high-performance cement anti-seepage modifiers on the market that can be mass-produced.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] One of the purposes of the present invention is to provide a cement impermeable agent, aiming to solve at least one of the above-mentioned technical problems in the prior art.
[0006] A second object of the present invention is to provide an application of a cement anti-seepage agent.
[0007] In order to solve the above technical problems, the present invention particularly adopts the following technical solutions:
[0008] The first aspect of the present invention provides a cement impermeable agent, which is mainly obtained by reacting bentonite, anionic polymer, initiator and cross-linking agent;
[0009] The anionic polymer is an anionic water-soluble polymer;
[0010] The anionic water-soluble polymer includes at least one of polyacrylic acid, polyacrylic acid salt, polyacrylamide, polypropylene sulfonic acid, polypropylene sulfonate, carboxymethyl cellulose, carboxymethyl starch and xanthan gum;
[0011] The aqueous solution of the anionic polymer is added to the bentonite, and then an initiator and a cross-linking agent are added and mixed evenly to obtain a mixture; the mixture is continuously extruded, allowed to stand, and dried to obtain the cement anti-seepage agent.
[0012] Furthermore, the bentonite includes sodium-based bentonite or calcium-based bentonite.
[0013] Preferably, the polyacrylate comprises sodium polyacrylate.
[0014] Preferably, the initiator comprises at least one of potassium persulfate, hydrogen peroxide, 1,1-diphenyl-2-trinitrophenylhydrazine, dibenzoyl peroxide and dicumyl peroxide.
[0015] Preferably, the cross-linking agent comprises iron salt, aluminum salt or methylenebisacrylamide and derivatives thereof.
[0016] Furthermore, the anionic water-soluble polymer is sodium polyacrylate and carboxymethyl cellulose.
[0017] Preferably, the molar ratio of the sodium polyacrylate to the carboxymethyl cellulose is 2 to 7:1.
[0018] Furthermore, the amount of the anionic polymer used is 1% to 40% of the mass of the bentonite.
[0019] Preferably, the amount of the initiator is 0.1% to 1% of the mass of the bentonite, preferably 0.4%.
[0020] Preferably, the amount of the cross-linking agent is 0.01% to 0.2% of the mass of the bentonite, preferably 0.125%.
[0021] Furthermore, the mass of water in the aqueous solution of the anionic polymer is 80% to 150% of the mass of the bentonite.
[0022] Furthermore, the bentonite is sodium-based bentonite, and the mass of water in the aqueous solution of the anionic polymer is 100% to 150% of the mass of the sodium-based bentonite.
[0023] Preferably, the bentonite is calcium-based bentonite, and the mass of water in the aqueous solution of the anionic polymer is 80% to 120% of the mass of the calcium-based bentonite.
[0024] Furthermore, the mixture is extruded using a roller press for 1 h to 6 h.
[0025] Preferably, the standing time is 6 h to 72 h.
[0026] Preferably, the drying temperature is 50° C. to 100° C., and the drying time is 8 h to 16 h.
[0027] Furthermore, the preparation method also includes a crushing and screening process after drying.
[0028] Preferably, the particle size of the cement anti-seepage agent after crushing and screening is less than 200 meshes.
[0029] Preferably, the preparation method of the cement impermeable agent comprises the following steps:
[0030] A. Mix acrylic acid and sodium carbonate and dissolve them in deionized water for reaction, then add carboxymethyl cellulose and deionized water, and mix them evenly until no bubbles are formed;
[0031] B. Add the substance obtained in step A to bentonite, and then add potassium persulfate and methylenebisacrylamide in sequence, mix each substance evenly and then add the next substance to obtain a mixture;
[0032] C. Extruding the mixture using a double-roll extruder, and then letting the extruded mixture stand, drying the standing mixture in an oven, and finally crushing the mixture to obtain the cement anti-seepage agent product.
[0033] The second aspect of the present invention provides application of the cement impermeable agent in concrete.
[0034] Furthermore, the addition amount of the cement anti-seepage agent is 1% to 5%.
[0035] Compared with the prior art, the present invention has at least the following beneficial effects:
[0036] The cement impermeable agent provided by the present invention uses anionic polymers to establish cationic bridging, electrostatic attraction and hydrogen bonding with bentonite, wherein cationic bridging refers to that the exchangeable cations in the double electric layer are connected to the anionic groups of the polymer through electrostatic interaction. The cations are fixed by the anionic polymers and montmorillonite, and the obtained cement impermeable agent is not easily replaced by heavy metal ions, which weakens the negative impact of heavy metal ion pollutants and protects the expansion capacity of bentonite. Electrostatic action refers to that the edge positive charge of the montmorillonite layer attracts the anionic groups in the anionic polymer through electrostatic attraction, so that the anionic polymer is combined with the montmorillonite sheet. Certain functional groups such as carboxyl groups are connected to the oxygen atoms in montmorillonite through hydrogen bonds. The above-mentioned cationic bridging, electrostatic attraction and hydrogen bonding work together to improve the performance of bentonite. At the same time, the extrusion and static setting of the preparation method improves the intercalation reaction of the anionic polymer in montmorillonite, promotes the efficiency of the intercalation reaction, and the obtained cement impermeable agent has better anti-seepage performance.
[0037] The present invention provides an application of cement anti-seepage agent in concrete, providing an anti-seepage agent with better performance for the concrete field. After adding the cement anti-seepage agent, the permeability coefficient of the concrete increases from 10 -5 Reduced to 10 -8 , greatly improving the density of concrete; in addition, the tolerance of concrete to high-salt pollutants has also been improved; the curing time of concrete has been shortened from 28 days to 7 days, which has accelerated the progress of the project, reduced the total cost of the project, and saved water resources. The cement impermeable agent provided by the present invention improves the quality of concrete, expands the application field of concrete, and promotes the development of downstream industries. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. The components of the embodiments of the present invention described and shown herein can be arranged and designed in various different configurations.
[0039] The first aspect of the present invention provides a cement impermeable agent, which is mainly obtained by reacting bentonite, anionic polymer, initiator and cross-linking agent;
[0040] The anionic polymer is an anionic water-soluble polymer;
[0041] The anionic water-soluble polymer includes at least one of polyacrylic acid, polyacrylic acid salt, polyacrylamide, polypropylene sulfonic acid, polypropylene sulfonate, carboxymethyl cellulose, carboxymethyl starch and xanthan gum;
[0042] The aqueous solution of the anionic polymer is added to the bentonite, and then an initiator and a cross-linking agent are added and mixed evenly to obtain a mixture; the mixture is continuously extruded, allowed to stand, and dried to obtain the cement anti-seepage agent.
[0043] The cement impermeable agent provided by the present invention uses anionic polymers to establish cationic bridging, electrostatic attraction and hydrogen bonding with bentonite, wherein cationic bridging refers to that the exchangeable cations in the double electric layer are connected to the anionic groups of the polymer through electrostatic interaction. The cations are fixed by the anionic polymers and montmorillonite, and the obtained cement impermeable agent is not easily replaced by heavy metal ions, which weakens the negative impact of heavy metal ion pollutants and protects the expansion capacity of bentonite. Electrostatic action refers to that the edge positive charge of the montmorillonite layer attracts the anionic groups in the anionic polymer through electrostatic attraction, so that the anionic polymer is combined with the montmorillonite sheet. Certain functional groups such as carboxyl groups are connected to the oxygen atoms in montmorillonite through hydrogen bonds. The above-mentioned cationic bridging, electrostatic attraction and hydrogen bonding work together to improve the performance of bentonite. At the same time, the extrusion and static setting of the preparation method improves the intercalation reaction of the anionic polymer in montmorillonite, promotes the efficiency of the intercalation reaction, and the obtained cement impermeable agent has better anti-seepage performance.
[0044] Bentonite is a non-metallic mineral with montmorillonite as the main mineral component. The montmorillonite structure is a 2:1 type crystal structure composed of two silicon-oxygen tetrahedra sandwiching a layer of aluminum-oxygen octahedron. Since the layered structure formed by the montmorillonite unit cell contains certain cations, such as Cu, Mg, Na, K, etc., and these cations are very unstable in their interaction with the montmorillonite unit cell and are easily exchanged by other cations, it has good ion exchangeability. The present invention uses anionic polymers to modify bentonite, which also utilizes the characteristics of cations in montmorillonite.
[0045] Furthermore, the bentonite includes sodium-based bentonite or calcium-based bentonite.
[0046] Sodium bentonite is classified according to the type and content of exchangeable cations between montmorillonite layers: those with an alkalinity coefficient greater than or equal to 1 are sodium bentonite, and those with an alkalinity coefficient less than 1 are calcium bentonite.
[0047] Preferably, the polyacrylate comprises sodium polyacrylate.
[0048] Preferably, the initiator comprises at least one of potassium persulfate, hydrogen peroxide, 1,1-diphenyl-2-trinitrophenylhydrazine (DPPH), dibenzoyl peroxide (BPO) and dicumyl peroxide (DCP).
[0049] Preferably, the cross-linking agent comprises iron salt, aluminum salt or methylenebisacrylamide and derivatives thereof.
[0050] Preferably, the iron salt comprises ferric nitrate.
[0051] Preferably, the aluminum salt comprises aluminum chloride.
[0052] Furthermore, the anionic water-soluble polymer is sodium polyacrylate and carboxymethyl cellulose.
[0053] Sodium polyacrylate is a lower-cost anionic polymer and acts as a filler and binder in cement impermeability to enhance impermeability. Sodium polyacrylate has strong water swelling and viscosity, and can form fibrous or network hydrogels when in contact with water, which can block continuous pores and extend the permeation path. When different bentonite particles / clusters are connected with anionic polymer functional groups with long-chain structures, they are combined together and the change in pore volume can be limited.
[0054] Preferably, the molar ratio of the sodium polyacrylate to the carboxymethyl cellulose is 2 to 7:1.
[0055] The molar ratio of sodium polyacrylate to carboxymethyl cellulose is controlled at 2 to 7:1, so that more sodium polyacrylate can establish cationic bridges with bentonite, and cationic bridges dominate the bonding mode, thereby making the organic group more firmly bonded to the Si-O group in the montmorillonite bilayer. When the molar ratio of sodium polyacrylate to carboxymethyl cellulose is less than 2:1, the bonding mode is mainly that the carboxyl group can be connected to the oxygen atom in montmorillonite through hydrogen bonds, the hydrophilicity is strong, and the organic group is easy to elute; when the molar ratio of sodium polyacrylate to carboxymethyl cellulose is greater than 7:1, sodium polyacrylate is not easy to directly bond with bentonite.
[0056] Typically but not limiting, the molar ratio of sodium polyacrylate to carboxymethyl cellulose can be, for example, 2:1, 3:1, 4:1, 5:1 or 7:1, or any value within the range of 2 to 7:1.
[0057] Furthermore, the amount of the anionic polymer used is 1% to 40% of the mass of the bentonite.
[0058] When the amount of anionic polymer is less than 1% of the bentonite mass, the bentonite modification effect is poor and the permeability coefficient is higher than 10 -7 cm / s; when the amount of anionic polymer is higher than 40% of the mass of bentonite, it will lead to excessive modifier and no obvious improvement on the permeability coefficient.
[0059] Typically but not limiting, the amount of anionic polymer used is 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35% or 40% of the mass of bentonite, and can be any value within the range of 1% to 40%.
[0060] Preferably, the amount of the initiator is 0.1% to 1% of the mass of the bentonite, preferably 0.4%.
[0061] When the amount of initiator used is less than 0.1% of the mass of bentonite, the activation degree of the reaction monomers will be insufficient and the polymerization reaction efficiency will be reduced; when the amount of initiator used is higher than 1% of the mass of bentonite, after the reaction monomers are fully activated, the additional addition of initiator will lead to an unnecessary increase in production costs.
[0062] Typically but not limiting, the amount of initiator used is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1% of the mass of bentonite, and can also be any value within the range of 0.1% to 1%.
[0063] Preferably, the amount of the cross-linking agent is 0.01% to 0.2% of the mass of the bentonite, preferably 0.125%.
[0064] When the amount of the cross-linking agent is less than 0.01% of the mass of bentonite, a stable structure cannot be formed between the polymer monomer and the bentonite, and the generated product is unstable; when the amount of the cross-linking agent is higher than 0.2% of the mass of the bentonite, the polymer monomer will be over-cross-linked, or the production cost may be increased unnecessarily.
[0065] Typically but not limiting, the amount of crosslinking agent used is 0.01%, 0.05%, 0.08%, 0.1%, 0.12%, 0.14%, 0.16%, 0.18%, 0.19% or 0.2% of the mass of bentonite, and can be any value within the range of 0.01% to 0.2%.
[0066] Furthermore, the mass of water in the aqueous solution of the anionic polymer is 80% to 150% of the mass of the bentonite.
[0067] The present invention ensures that the reaction is synthesized according to a semi-dry process by controlling the water content, so the amount of water added to the aqueous solution of the anionic polymer is controlled.
[0068] When the mass of water in the anionic polymer aqueous solution is lower than 80% of the mass of bentonite, the functional groups on the surface of the bentonite will not be fully hydrolyzed, and will not be activated and fully contact and react with the polymer; when the mass of water in the anionic polymer aqueous solution is higher than 150% of the mass of bentonite, the energy consumption and time cost in the subsequent drying process will increase.
[0069] Typically but not limiting, the mass of water in the aqueous solution can be 80%, 90%, 100%, 110%, 120%, 130%, 140% or 150% of the mass of bentonite, or any value within the range of 80% to 150%.
[0070] Furthermore, the bentonite is sodium-based bentonite, and the mass of water in the aqueous solution of the anionic polymer is 100% to 150% of the mass of the sodium-based bentonite.
[0071] Since sodium bentonite has a larger polarity and stronger water absorption and expansion properties, the amount of water added is slightly higher. In specific implementation, the amount of water added can be 100%, 110%, 120%, 130%, 140% or 150% of the mass of bentonite, or any value within the range of 100% to 150%.
[0072] Preferably, the bentonite is calcium-based bentonite, and the mass of water in the aqueous solution of the anionic polymer is 80% to 120% of the mass of the calcium-based bentonite.
[0073] Calcium-based bentonite has lower polarity and weaker water swelling than sodium-based bentonite, so the amount of water added is slightly lower. In specific implementation, the amount of water added can be 80%, 90%, 100%, 110% or 120% of the mass of bentonite, or any value within the range of 80% to 120%.
[0074] The present invention controls the amount of water added to the system and uses a semi-dry process to pre-synthesize organic modified bentonite. During the modification process, external force extrusion promotes the intercalation reaction of anionic polymers in montmorillonite minerals in bentonite. The key to the semi-dry synthesis process is to control the water content to the plastic limit of the mixture to induce dissociation and intercalation reactions of the polymer.
[0075] The key to the semi-dry synthesis process is to control the moisture content to the plastic limit of the mixture to induce dissociation and intercalation reactions of the polymer.
[0076] Furthermore, the mixture is extruded using a roller press for 1 h to 6 h.
[0077] The purpose of extrusion is to ensure that the cross-linking reaction between the polymer and bentonite is promoted by external force, so as to ensure the smooth progress of the polymerization reaction and the performance of the product.
[0078] Typically but not limiting, the extrusion time may be, for example, 1 h, 2 h, 3 h, 4 h, 5 h or 6 h, or any value within the time range of 1 h to 6 h.
[0079] Preferably, the standing time is 6 h to 72 h.
[0080] The purpose of standing is to allow the solid to settle and separate the modified soil after the reaction from the excess unreacted monomers.
[0081] Typically but not limiting, the standing time may be, for example, 6 h, 18 h, 30 h, 42 h, 54 h or 72 h, or any value within the time range of 6 h to 72 h.
[0082] Preferably, the drying temperature is 50° C. to 100° C., and the drying time is 8 h to 16 h.
[0083] The drying temperature is controlled at 50°C to 100°C in order to ensure the drying efficiency and prevent the cellulose anionic polymer from being degraded under high temperature conditions.
[0084] Furthermore, the preparation method also includes a crushing and screening process after drying.
[0085] Preferably, the particle size of the cement anti-seepage agent after crushing and screening is less than 200 meshes.
[0086] In some embodiments of the present invention, the preparation method of the cement impermeable agent comprises the following steps:
[0087] A. Mix acrylic acid and sodium carbonate and dissolve them in deionized water for reaction, then add carboxymethyl cellulose and deionized water, and mix them evenly until no bubbles are formed;
[0088] B. Add the substance obtained in step A to bentonite, and then add potassium persulfate and methylenebisacrylamide in sequence, mix each substance evenly and then add the next substance to obtain a mixture;
[0089] C. Extruding the mixture using a double-roll extruder, and then letting the extruded mixture stand, drying the standing mixture in an oven, and finally crushing the mixture to obtain the cement anti-seepage agent product.
[0090] In the above preparation method, acrylic acid and sodium carbonate are added to synthesize sodium polyacrylate. Potassium persulfate and methylenebisacrylamide are initiators and crosslinkers, respectively. Sodium polyacrylate is not used directly because sodium polyacrylate has a large molecular weight and is relatively stable, which will affect the effect of inserting into the molecular layer of montmorillonite minerals; and the cost of sodium polyacrylate is much higher than that of sodium acrylate and sodium carbonate. Using acrylic acid and sodium carbonate to synthesize sodium polyacrylate in the preparation process can improve the effect of anionic polymer intercalation and reduce costs.
[0091] The second aspect of the present invention provides application of the cement impermeable agent in concrete.
[0092] The present invention provides an application of cement anti-seepage agent in concrete, providing an anti-seepage agent with better performance for the concrete field. After adding the cement anti-seepage agent, the permeability coefficient of the concrete increases from 10 -5 Reduced to 10 -8, greatly improving the density of concrete; in addition, the tolerance of concrete to high-salt pollutants has also been improved; the curing time of concrete has been shortened from 28 days to 7 days, which has accelerated the progress of the project, reduced the total cost of the project, and saved water resources. The cement impermeable agent provided by the present invention improves the quality of concrete, expands the application field of concrete, and promotes the development of downstream industries.
[0093] Furthermore, the addition amount of the cement anti-seepage agent is 1% to 5%.
[0094] When used, the amount of cement impermeable agent added to concrete can be, for example, 1%, 2%, 3%, 4% or 5%, or any value within the range of 1% to 5%. During the implementation of the present invention, it was found that an addition amount of 2% can reduce the cement permeability coefficient by one order of magnitude, and at an addition amount of 4%, the permeability coefficient can be reduced by 3 orders of magnitude.
[0095] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. The raw materials used in the present invention can be obtained by commercial purchase unless otherwise specified.
[0096] Example 1
[0097] This embodiment provides a cement anti-seepage agent, and the specific preparation method is as follows:
[0098] 1. Weigh 1 kg of sodium bentonite and place it in a reaction container.
[0099] 2. Weigh 201.6 g of acrylic acid and 148.4 g of sodium carbonate, mix and evenly dissolve in deionized water. After the reaction, add 50 g of sodium carboxymethyl cellulose, then add deionized water and stir until no bubbles are formed. The total amount of water added is 120 g, and pour into the reaction container filled with bentonite.
[0100] 3. Continue to add 5.6g potassium persulfate and 1.75g methylenebisacrylamide into the reaction vessel. Each time you add the reagent, stir evenly to obtain a bentonite mixture.
[0101] 4. Extrude the bentonite mixture for 2 hours using a double-roll extruder. Allow the extruded bentonite to stand for 48 hours. Heat and dry it in an oven at 85°C for 12 hours. Put the dried cement impermeable agent into a high-power pulverizer, crush it, pass it through a 200-mesh sieve and store it in a sealed bag.
[0102] Example 2
[0103] This embodiment provides a cement anti-seepage agent, and the specific preparation method is as follows:
[0104] 1. Weigh 1 kg of sodium bentonite and place it in a reaction container.
[0105] 2. Same as the step in Example 1.
[0106] 3. Continue to add 4g potassium persulfate and 1.25g methylenebisacrylamide to the reaction vessel. Each time you add the reagent, stir evenly to obtain a bentonite mixture.
[0107] 4. Extrude the bentonite mixture for 2 hours using a double-roll extruder. Allow the extruded bentonite to stand for 24 hours. Heat and dry it in an oven at 85°C for 16 hours. Put the dried cement impermeable agent into a high-power pulverizer, crush it, pass it through a 200-mesh sieve and store it in a sealed bag.
[0108] Example 3
[0109] This embodiment provides a cement anti-seepage agent. The difference from Embodiment 1 is that 198.8 g of acrylamide (solid content>90%, Songya Chemical (Shanghai) Co., Ltd.) is used in step 2 to replace sodium acrylate, and the remaining raw materials and steps are the same as those in Embodiment 1 and are not repeated here.
[0110] Example 4
[0111] This embodiment provides a cement anti-seepage agent. The difference from Embodiment 1 is that 300 g of acrylamide (solid content>90%, Songya Chemical (Shanghai) Co., Ltd.) is used in step 2 instead of sodium acrylate, and carboxymethyl starch is used instead of sodium carboxymethyl cellulose. The remaining raw materials and steps are the same as those in Embodiment 1 and are not described again.
[0112] Example 5
[0113] This embodiment provides a cement anti-seepage agent. The difference from Embodiment 1 is that in step 2, 50.4 g of acrylic acid, 37.1 g of sodium carbonate, and 12.5 g of sodium carboxymethyl cellulose are weighed. The remaining raw materials and steps are the same as those in Embodiment 1 and are not described again.
[0114] Example 6
[0115] This embodiment provides a cement anti-seepage agent. The difference from Embodiment 1 is that in step 2, the amount of acrylic acid weighed is 172.8 g, the amount of sodium carbonate weighed is 127.2 g, and the amount of sodium carboxymethyl cellulose weighed is 100 g. The remaining raw materials and steps are the same as those in Embodiment 1 and are not repeated here.
[0116] Example 7
[0117] This embodiment provides a cement anti-seepage agent. The difference from Embodiment 1 is that sodium carboxymethyl cellulose is not added in step 2, and the remaining raw materials and methods are the same as those in Embodiment 1, which will not be described again.
[0118] Example 8
[0119] This embodiment provides a cement anti-seepage agent. The difference from Embodiment 1 is that acrylic acid and sodium carbonate are not added in step 2. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.
[0120] Example 9
[0121] This embodiment provides a cement impermeable agent. The difference from Embodiment 1 is that in step 2, a 0.2% aqueous solution of sodium polyacrylate is directly used to replace acrylic acid and sodium carbonate. The manufacturer of sodium polyacrylate is Shandong Muheng Biotechnology Co., Ltd. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be repeated here.
[0122] Comparative Example 1
[0123] This comparative example provides a bentonite having the same specifications and batches as those of the bentonite in Examples 1-10.
[0124] Comparative Example 2
[0125] This comparative example provides a cement anti-seepage agent, the specification is HEA anti-cracking waterproof agent, the manufacturer is Zhejiang Sanshi Group Special Cement Co., Ltd. Its main components are calcium sulfoaluminate, high aluminum clinker, anhydrite and other inorganic materials.
[0126] Test Example 1
[0127] The substances obtained in the examples and comparative examples were used as cement anti-seepage agents to carry out concrete performance tests.
[0128] 1. Preparation of cement soil
[0129] Take 10g of cement anti-seepage agent, add 100g of deionized water, stir with an automatic stirrer for 15 minutes to make mud, pour the prepared mud into a beaker, seal it and let it stand for 24 hours.
[0130] Take 200g of cement, add the cement anti-seepage agent slurry prepared above, mix evenly with an automatic stirrer, and then add the prepared in-situ soil to continue stirring. After stirring, pour the slurry into the mold, pour about 1cm each time, and vibrate manually until there are no bubbles on the surface, continue to pour the remaining slurry, and repeat the above operation until the mold is filled. After pouring, put it in a standard curing room for curing (temperature 20℃, humidity above 95%RH). According to the strength development of the sample, demold it after 1-2 days (push the sample out with a pusher), cut the sample height to 30mm (determined according to the requirements of the flexible wall penetration test), and flatten the upper and lower bottom surfaces of the sample, then put the sample in a sealed bag and continue to cure until the age of 7d, 14d and 28d, measure the diameter and height of the sample with a vernier caliper, and record them.
[0131] 2. Determination of permeability coefficient of cement soil specimen
[0132] The permeability coefficient at each consolidation pressure was measured according to ASTM D5084-16a. The permeability coefficient after curing for 7 days is shown in Table 1.
[0133] Table 1
[0134]
[0135] The permeability coefficient after curing for 28 days is shown in Table 2.
[0136] Table 2
[0137]
[0138] Test Example 2
[0139] The addition amount of cement anti-seepage agent was adjusted to 4 g, and the permeability coefficient was tested in the same manner as in Test Example 1. The obtained data are shown below.
[0140] The permeability coefficient after curing for 7 days is shown in Table 3.
[0141] Table 3
[0142]
[0143] The permeability coefficient after curing for 28 days is shown in Table 4.
[0144] Table 4
[0145]
[0146] Test Example 3
[0147] The compressive strength of the cement-soil specimens of Test Example 1 was tested at 7, 14, and 28 days of curing age. The compressive strength test was carried out in accordance with the provisions of GB / T 50081-2019. The obtained data are shown in Table 5 below.
[0148] Table 5
[0149]
[0150] Test Example 4
[0151] The cement soil specimens prepared by the method of Test Example 1 were subjected to flexible wall test tolerance tests using 500 mM CaCl2 and 1000 mM NaCl and deionized water, respectively. The test scheme was carried out in accordance with ASTM D5084-16a. After stabilization under an effective consolidation stress of 200 kPa, the permeability coefficients were obtained and are shown in Table 6 below.
[0152] Table 6
[0153]
[0154]
[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A cement anti-seepage agent, characterized in that: It is mainly obtained by the reaction of bentonite, anionic polymer, initiator and cross-linking agent; The anionic polymer is an anionic water-soluble polymer; The anionic water-soluble polymer includes at least one of polyacrylic acid, polyacrylic acid salt, polyacrylamide, polypropylene sulfonic acid, polypropylene sulfonate, carboxymethyl cellulose, carboxymethyl starch and xanthan gum; The aqueous solution of the anionic polymer is added to the bentonite, and then an initiator and a cross-linking agent are added and mixed evenly to obtain a mixture; the mixture is continuously extruded, allowed to stand, and dried to obtain the cement anti-seepage agent.
2. The cement anti-seepage agent according to claim 1, characterized in that: The bentonite includes sodium-based bentonite or calcium-based bentonite; Preferably, the polyacrylate comprises sodium polyacrylate; Preferably, the initiator comprises at least one of potassium persulfate, hydrogen peroxide, 1,1-diphenyl-2-trinitrophenylhydrazine, dibenzoyl peroxide and diisopropylbenzene peroxide; Preferably, the cross-linking agent comprises iron salt, aluminum salt or methylenebisacrylamide and derivatives thereof.
3. The cement anti-seepage agent according to claim 1, characterized in that: The anionic water-soluble polymer is sodium polyacrylate and carboxymethyl cellulose; Preferably, the molar ratio of the sodium polyacrylate to the carboxymethyl cellulose is 2 to 7:
1.
4. The cement anti-seepage agent according to any one of claims 1 to 3, characterized in that: The amount of the anionic polymer is 1% to 40% of the mass of the bentonite; Preferably, the amount of the initiator is 0.1% to 1% of the mass of the bentonite, preferably 0.4%; Preferably, the amount of the cross-linking agent is 0.01% to 0.2% of the mass of the bentonite, preferably 0.125%.
5. The cement anti-seepage agent according to any one of claims 1 to 3, characterized in that: In the aqueous solution of the anionic polymer, the mass of water is 80% to 150% of the mass of the bentonite.
6. The cement anti-seepage agent according to claim 5, characterized in that: The bentonite is sodium bentonite, and the mass of water in the aqueous solution of the anionic polymer is 100% to 150% of the mass of the sodium bentonite; Preferably, the bentonite is calcium-based bentonite, and in the aqueous solution of the anionic polymer, the mass of water is 80% to 120% of the mass of the calcium-based bentonite.
7. The cement anti-seepage agent according to any one of claims 1 to 3, characterized in that: The mixture is extruded using a roller press for 1 h to 6 h; Preferably, the standing time is 6h to 72h; Preferably, the drying temperature is 50° C. to 100° C., and the drying time is 8 h to 16 h.
8. The cement anti-seepage agent according to any one of claims 1 to 3, characterized in that: It also includes the crushing and screening process after drying; Preferably, the particle size of the cement anti-seepage agent after crushing and screening is less than 200 meshes.
9. Use of the cement anti-seepage agent according to any one of claims 1 to 8 in concrete.
10. The use according to claim 9, characterized in that: The addition amount of the cement anti-seepage agent is 1% to 5%.
Citation Information
Patent Citations
Water-inflated polymer-mineral composite and its preparation
CN1071180A
Method for preparing organic improved bentonite on basis of seepage prevention
CN107778423A
Preparation method of polymer modified bentonite
CN112744823A