Reaction method for preparing maleic anhydride through oxidation of n-butane

By using 2,5-dihydrofuran, furan and 2(5H)-furanone as promoters under the catalyst, the overall conversion rate and maleic anhydride selection of n-butane oxidation to maleic anhydride were improved. property, solves the problems of insufficient conversion rate and selectivity in the existing technology, and achieves an efficient increase in maleic anhydride yield.

CN118772086AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310377598.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

The total conversion rate and maleic anhydride selectivity in the existing n-butane oxidation reaction to prepare maleic anhydride need to be further improved.

Method used

Under the action of a catalyst, 2,5-dihydrofuran, furan and 2(5H)-furanone are used as promoters, which are contacted with n-butane and oxidants, and the molar ratio and dosage are optimized to improve reaction efficiency.

Benefits of technology

Significantly improve the total conversion rate of the reaction and the selectivity of maleic anhydride, greatly improving the yield of maleic anhydride, and the accelerator is completely reacted in the reactor, no new impurities are introduced, the operation is simple, and no large-scale equipment is required Transformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004171104670000071
    Figure BDA0004171104670000071
  • Figure BDA0004171104670000101
    Figure BDA0004171104670000101
  • Figure BDA0004171104670000111
    Figure BDA0004171104670000111
Patent Text Reader

Abstract

The invention relates to the field of maleic anhydride production, and discloses a reaction method for preparing maleic anhydride through n-butane oxidation. The invention relates to a reaction method for preparing maleic anhydride by oxidizing n-butane, which comprises the following step: under the action of a catalyst, enabling an accelerant, n-butane and an oxidant to be in contact, wherein the accelerant is selected from at least one of 2, 5-dihydrofuran, furan and 2 (5H)-furanone. The method can effectively improve the total conversion rate of the reaction and the maleic anhydride selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of maleic anhydride production, and in particular to a method for preparing maleic anhydride by oxidation of n-butane. Background Art

[0002] Maleic anhydride (maleic anhydride) is an important organic chemical raw material and fine chemical product. It is the third largest anhydride in the world after phthalic anhydride and acetic anhydride. It is mainly used in the production of thermosetting resins, unsaturated polyester resins, pesticides, medicines, coatings, inks, lubricant additives, paper chemicals, textile chemicals, textile finishing agents, food additives and surfactants. In addition, maleic anhydride can also be used as a raw material to produce a series of widely used fine chemical products such as 1,4-butanediol (GBL), tetrahydrofuran (THF), maleic acid, fumaric acid and tetrahydroanhydride. The development and utilization prospects are very broad, and its application range is still expanding.

[0003] The production process of maleic anhydride is mainly divided into benzene catalytic oxidation method, n-butane catalytic oxidation method, C4 olefin catalytic oxidation method and phthalic anhydride by-product method according to raw materials. In recent years, the process of producing maleic anhydride with low-cost carbon four fraction (n-butane) as raw material has become the absolute mainstream of maleic anhydride production worldwide. Since 2011, the trend of converting the benzene oxidation method to the n-butane oxidation method to produce maleic anhydride has become increasingly obvious in China. The production capacity and operating rate of domestic n-butane oxidation maleic anhydride production units have exceeded those of the benzene oxidation method. These factors have greatly stimulated the demand of domestic enterprises for vanadium phosphorus oxygen catalysts for butane-based maleic anhydride production.

[0004] In the typical process of producing maleic anhydride by the n-butane method, n-butane and air are preheated and passed through a tube-in-tube fixed bed reactor equipped with a vanadium phosphorus oxygen catalyst to generate maleic anhydride. After passing through a post-processing unit, relatively pure maleic anhydride is obtained.

[0005] In addition to n-butane and air, the raw gas has long been reported in patent literature that adding water vapor alone to the reaction system is beneficial to the reaction. For example, US20070249848A1 adopts carbon monoxide to be added to the raw gas, which can appropriately improve the selectivity and yield of maleic anhydride and reduce the hot spot temperature. CN202415420U reports a process for seasonal water vapor supplementation, that is, adding steam to the reaction air in the spring and winter when the weather is dry, so that the catalytic oxidation environment is improved and the catalyst weakening rate is slowed down. The activity of the catalytic thorn is improved, while the maleic anhydride conversion rate is increased, and the raw material consumption is reduced. US4950769A reports a method of replenishing water with hydrogen peroxide, which decomposes into water and oxygen at high temperature.

[0006] US511707A, US3474041A, US4701433A, US4515899A and the like mention that adding compounds containing phosphorus, such as trimethyl phosphate, to the raw gas can slow down the problem of phosphorus loss in the late stage of the catalyst life cycle and extend the life of the catalyst.

[0007] These technologies have made great contributions to the industry and provided many valuable inspirations for later researchers. How to further improve the conversion rate of n-butane and the selectivity of maleic anhydride has always been an important research direction. Summary of the invention

[0008] The purpose of the present invention is to overcome the problem that the total conversion rate and maleic anhydride selectivity in the reaction of preparing maleic anhydride by oxidation of n-butane in the prior art need to be further improved, and to provide a method for preparing maleic anhydride by oxidation of n-butane. The method effectively improves the total conversion rate and maleic anhydride selectivity of the reaction.

[0009] In order to achieve the above object, the present invention provides a method for preparing maleic anhydride by oxidation of n-butane, which method comprises: contacting a promoter, n-butane and an oxidant under the action of a catalyst;

[0010] Wherein, the promoter is selected from at least one of 2,5-dihydrofuran, furan and 2(5H)-furanone.

[0011] Preferably, the promoter is selected from at least two of 2,5-dihydrofuran, furan and 2(5H)-furanone.

[0012] Preferably, the molar ratio of furan, 2,5-dihydrofuran and 2(5H)-furanone is 5-60:0-15:35-95, preferably 8-55:0-15:45-95.

[0013] Preferably, the amount of the promoter is 0.01-5%, preferably 0.1-1%, based on the amount of n-butane.

[0014] Through the above technical solution, the beneficial effects of the present invention include:

[0015] The method provided by the present invention introduces a promoter, which can promote the reaction of preparing maleic anhydride by oxidation of n-butane, thereby effectively improving the total conversion rate of the reaction and the selectivity of maleic anhydride, so that the yield of maleic anhydride is greatly improved. At the same time, the promoter is completely reacted in the reactor without introducing new impurities.

[0016] The method provided by the invention is easy to operate and does not require major modifications to existing devices. DETAILED DESCRIPTION

[0017] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0018] In one aspect, the present invention provides a method for preparing maleic anhydride by oxidation of n-butane, the method comprising: contacting a promoter, n-butane and an oxidant under the action of a catalyst;

[0019] Wherein, the promoter is selected from at least one of 2,5-dihydrofuran, furan and 2(5H)-furanone.

[0020] Preferably, the promoter is selected from at least two of 2,5-dihydrofuran, furan and 2(5H)-furanone. In this preferred embodiment, the two promoters work synergistically, which is more conducive to improving the yield of maleic anhydride.

[0021] In order to further improve the yield of maleic anhydride, preferably, the molar ratio of furan, 2,5-dihydrofuran and 2(5H)-furanone is 5-60:0-15:35-95, preferably 8-55:0-15:45-95.

[0022] According to the present invention, preferably, the amount of the promoter is 0.01-5% of the amount of n-butane substance, preferably 0.1-1%, such as 0.01%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, and any value in the range formed by any two of these numerical values. Adopting this preferred embodiment is more conducive to the improvement of maleic anhydride yield.

[0023] According to the present invention, preferably, based on the total volume of n-butane and the oxidant, the volume fraction of n-butane is 1.5-2%.

[0024] In the present invention, the volume fraction of n-butane is obtained by the following formula:

[0025] Volume fraction of n-butane = volume of n-butane introduced / (volume of n-butane introduced + volume of oxidant introduced) × 100%.

[0026] The reaction of preparing maleic anhydride by oxidation of n-butane described in the present invention can be a continuous reaction or a batch reaction.

[0027] When the n-butane oxidation reaction to prepare maleic anhydride is a continuous reaction, preferably, the method comprises: adding a mixture of a promoter, an oxidant and n-butane into a reactor containing a catalyst for contact.

[0028] When the n-butane oxidation reaction to prepare maleic anhydride is a batch reaction, the promoter can be added alone or mixed with other materials before being added, and the present invention has no particular limitation on this.

[0029] When the promoter is added separately, preferably, the method comprises: adding the promoter into a reactor containing a catalyst to contact with n-butane and an oxidant.

[0030] When the accelerator is mixed with other materials and added, there are mainly three situations:

[0031] Preferably, the method comprises: adding a mixture of the promoter and n-butane into a reactor containing a catalyst to contact the mixture with an oxidant.

[0032] Preferably, the method comprises: adding a mixture of a promoter and an oxidant into a reactor containing a catalyst to contact with n-butane.

[0033] Preferably, the method comprises: adding a mixture of a promoter, an oxidant and n-butane into a reactor containing a catalyst for contact.

[0034] When the n-butane oxidation reaction to prepare maleic anhydride is a batch reaction, the amount of the catalyst used is 0.001-4% of the volume of n-butane.

[0035] Water vapor can reduce hot spots, and water vapor can be added to the reaction of the present invention as needed. Preferably, the reaction raw materials of the method also contain water vapor.

[0036] Preferably, the amount of water vapor used is 0-1%, preferably 0-0.5%, of the amount of n-butane.

[0037] The present invention has no particular limitation on the manner of adding the water vapor, which can be added alone or together with other substances.

[0038] According to a specific embodiment of the present invention, a mixture of water vapor, a promoter, an oxidant and n-butane is added into a reactor containing a catalyst for contact.

[0039] In the reaction of preparing maleic anhydride by oxidation of n-butane in the art, a vanadium phosphorus oxygen catalyst is usually used. During the use of the vanadium phosphorus oxygen catalyst, phosphorus will be lost in large quantities, resulting in reduced catalyst activity. The addition of a phosphorus supplementing agent can make up for the lack of phosphorus. Therefore, the reaction of the present invention can also add a phosphorus supplementing agent as needed. Preferably, the reaction raw materials of the method also contain a phosphorus supplementing agent.

[0040] The present invention has no particular limitation on the type of the phosphorus supplement agent, and it can be a conventional choice in the art. Preferably, the phosphorus supplement agent is trimethyl phosphate.

[0041] Preferably, the amount of the phosphorus supplement agent is 0-1%, preferably 0-0.5%, of the amount of n-butane substance.

[0042] The present invention has no particular limitation on the manner of adding the phosphorus supplement agent, which can be added alone or together with other substances.

[0043] According to a specific embodiment of the present invention, a mixture of a phosphorus supplement, a promoter, an oxidant and n-butane is added into a reactor containing a catalyst for contact.

[0044] Carbon monoxide can reduce hot spots, and carbon monoxide can be added to the reaction of the present invention as needed. Preferably, the reaction raw materials of the method also contain carbon monoxide.

[0045] Preferably, the amount of carbon monoxide used is 0-1%, preferably 0-0.5%, of the amount of n-butane substance.

[0046] The present invention has no particular limitation on the manner of adding the carbon monoxide, which can be added alone or together with other substances.

[0047] According to a specific embodiment of the present invention, a mixture of carbon monoxide, a promoter, an oxidant and n-butane is added into a reactor containing a catalyst for contact.

[0048] According to the present invention, preferably, the reaction conditions include: temperature of 370-440°C, preferably 400-440°C; volume space velocity of 1000-2200h -1 , preferably 1500-2100h -1 ; The pressure is 0.01-0.09MPa, preferably 0.02-0.08MPa.

[0049] In the present invention, when n-butane is added to the reactor alone, the volume space velocity is the volume space velocity of n-butane.

[0050] When a mixture of n-butane and other substances (such as oxidants, promoters, etc.) is added to the reactor, the volume space velocity is the volume space velocity of the mixture.

[0051] The present invention has no particular limitation on the type of the oxidant, which can be selected conventionally in the art. Preferably, the oxidant is an oxygen-containing gas, preferably air.

[0052] There is no particular limitation on the catalyst used in the method for preparing maleic anhydride by oxidation of n-butane of the present invention, and various catalysts commonly used in the art can be used. Preferably, the catalyst is a vanadium phosphorus oxygen catalyst.

[0053] According to the present invention, preferably, based on the total mass of the catalyst, the mass content of vanadium is 28-35%, preferably 30-34%; the mass content of phosphorus is 15-25%, preferably 18-22%.

[0054] According to the present invention, preferably, the bulk density of the catalyst is 0.6-0.85 g / cm 3 , preferably 0.7-0.8 g / cm 3 .

[0055] The present invention has no particular limitation on the preparation method of the above-mentioned catalyst, as long as the catalyst with the above-mentioned composition and characteristics can be prepared. In order to better illustrate the method of the present invention, the present invention provides a catalyst disclosed in CN108339558A as an example.

[0056] The present invention will be described in detail below through examples.

[0057] In the following embodiments,

[0058] n-Butane volume fraction = n-Butane input volume / (n-Butane input volume + air input volume) × 100%

[0059]

[0060]

[0061] Yield = total conversion × maleic anhydride selectivity

[0062] The furan, 2,5-dihydrofuran and 2(5H)-furanone used in the following examples are all commercially available products of analytical grade.

[0063] Preparation Example 1

[0064] The catalyst was prepared according to the method of Example 1 of CN108339558A.

[0065] Example 1

[0066] The catalyst was loaded into a fixed bed reactor with a single tube specification of Φ25×2×4000mm (outer diameter 25mm, wall thickness 2mm, height 4000mm). A mixture of promoter, air and n-butane was added to the fixed bed reactor, with a volume fraction of n-butane of 1.81%, a promoter of furan, and a promoter amount of 1% of the amount of n-butane. At a molten salt temperature of 425°C, a pressure of 0.02MPa, and a volume space velocity of 2000h -1 The real-time evaluation results are shown in Table 1.

[0067] Example 2

[0068] The catalyst was loaded into a fixed bed reactor with a single tube specification of Φ25×2×4000mm (outer diameter 25mm, wall thickness 2mm, height 4000mm). A mixture of promoter, air and n-butane was added into the fixed bed reactor, the volume fraction of n-butane was 1.79%, the promoter was 2,5-dihydrofuran, the amount of promoter added was 0.8% of the amount of n-butane, at a molten salt temperature of 425°C, a pressure of 0.02MPa, and a volume space velocity of 2000h -1 The real-time evaluation results are shown in Table 1.

[0069] Example 3

[0070] The catalyst was loaded into a fixed bed reactor with a single tube specification of Φ25×2×4000mm (outer diameter 25mm, wall thickness 2mm, height 4000mm). A mixture of promoter, air and n-butane was added into the fixed bed reactor, the volume fraction of n-butane was 1.81%, the promoter was 2(5H)-furanone, the amount of promoter added was 0.1% of the amount of n-butane, the temperature of the molten salt was 430°C, the pressure was 0.03MPa, and the volume space velocity of the mixture was 1800h -1 The real-time evaluation results are shown in Table 1.

[0071] Example 4

[0072] The method of Example 1 was followed, except that the accelerators used were furan and 2(5H)-furanone, wherein the molar ratio of furan to 2(5H)-furanone was 1:1, and the total amount of accelerator added was 0.5% of the amount of butane. The real-time evaluation results are shown in Table 1.

[0073] Example 5

[0074] The method of Example 1 was followed, except that the accelerators used were furan, 2,5-dihydrofuran and 2(5H)-furanone, wherein the molar ratio of furan:2,5-dihydrofuran:2(5H)-furanone was 1:1:8, and the total amount of accelerator added was 0.7% of the amount of butane. The real-time evaluation results are shown in Table 1.

[0075] Example 6

[0076] The method of Example 1 was followed, except that the accelerators were furan and 2(5H)-furanone, wherein the molar ratio of furan to 2(5H)-furanone was 1:9, the total amount of accelerator added was 0.5% of the amount of butane substance, and 0.1% of water vapor, 0.1% of carbon monoxide, and 0.1% of trimethyl phosphate were added. The real-time evaluation results are shown in Table 1.

[0077] Example 7

[0078] The method of Example 1 was followed, except that the accelerators used were furan and 2(5H)-furanone, wherein the molar ratio of furan to 2(5H)-furanone was 3:7, and the total amount of accelerator added was 0.03% of the amount of butane. The real-time evaluation results are shown in Table 1.

[0079] Example 8

[0080] The method of Example 1 was followed, except that the accelerators used were furan and 2,5-dihydrofuran, wherein the molar ratio of furan to 2,5-dihydrofuran was 5:5, and the total amount of accelerator added was 4% of the amount of butane. The real-time evaluation results are shown in Table 1.

[0081] Example 9

[0082] The catalyst was loaded into a fixed bed reactor with a single tube specification of Φ25×2×4000mm (outer diameter 25mm, wall thickness 2mm, height 4000mm), and a mixture of furan, 2,5-dihydrofuran, 2(5H)-furanone, air and n-butane was added into the fixed bed reactor. The molar ratio of furan: 2,5-dihydrofuran: 2(5H)-furanone: n-butane was 1:1:1:7, and the total volume fraction of the four substances (furan, 2,5-dihydrofuran, 2(5H)-furanone, n-butane) was 1.81%. At a molten salt temperature of 435°C, a pressure of 0.02MPa, and a volume space velocity of 2000h -1 The real-time evaluation results are shown in Table 1.

[0083] The total volume fraction of the four substances = the volume of the four substances introduced / (the volume of the four substances introduced + the volume of air introduced) × 100%.

[0084] Comparative Example 1

[0085] The method of Example 1 was followed, except that no accelerator was added. The real-time evaluation results are shown in Table 1.

[0086] Comparative Example 2

[0087] The method of Example 1 was followed, except that no promoter was added, and water vapor was added at 1% of the amount of butane. The real-time evaluation results are shown in Table 1.

[0088] Comparative Example 3

[0089] The method of Example 1 was followed, except that no promoter was added, and 0.1% of trimethyl phosphate was added. The real-time evaluation results are shown in Table 1.

[0090] Comparative Example 4

[0091] The catalyst was loaded into a fixed bed reactor with a single tube specification of Φ25×2×4000mm (outer diameter 25mm, wall thickness 2mm, height 4000mm). A mixture of furan and air was added into the fixed bed reactor. The volume fraction of furan was 1.81%. At a molten salt temperature of 435°C and a pressure of 0.02MPa, the volume space velocity of the mixture was 2000h -1 The real-time evaluation results are shown in Table 1.

[0092] Furan volume fraction = furan input volume / (furan input volume + air input volume) × 100%.

[0093] Table 1

[0094]

[0095]

[0096] It can be seen from the results in Table 1 that the total conversion rate and the selectivity of maleic anhydride in the method provided by the present invention are significantly improved, so that the yield of maleic anhydride is greatly improved. Moreover, this improvement is not because the yield of maleic anhydride oxidized by the promoter itself is high, thereby leading to an increase in the total yield, but the presence of the promoter promotes the reaction of n-butane oxidation to maleic anhydride, and has a good application prospect.

[0097] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing maleic anhydride by oxidation of n-butane, characterized in that: The method comprises: contacting a promoter, n-butane and an oxidant under the action of a catalyst; Wherein, the promoter is selected from at least one of 2,5-dihydrofuran, furan and 2(5H)-furanone.

2. The method according to claim 1, wherein: The promoter is selected from at least two of 2,5-dihydrofuran, furan and 2(5H)-furanone; Preferably, the molar ratio of furan, 2,5-dihydrofuran and 2(5H)-furanone is 5-60:0-15:35-95, preferably 8-55:0-15:45-95.

3. The method according to claim 1, wherein: The amount of the promoter is 0.01-5%, preferably 0.1-1% of the amount of n-butane; Based on the total volume of n-butane and the oxidant, the volume fraction of n-butane is 1.5-2%.

4. The method according to any one of claims 1 to 3, wherein: When the reaction is a continuous reaction, the method comprises: adding a mixture of a promoter, an oxidant and n-butane into a reactor containing a catalyst for contact.

5. The method according to any one of claims 1 to 3, wherein: When the reaction is an intermittent reaction, the method comprises: adding a promoter into a reactor containing a catalyst to contact the promoter with n-butane and an oxidant; Alternatively, the method comprises: adding a mixture of a promoter and n-butane into a reactor containing a catalyst to contact the mixture with an oxidant; Alternatively, the method comprises: adding a mixture of a promoter and an oxidant into a reactor containing a catalyst to contact with n-butane; Alternatively, the method comprises: adding a mixture of a promoter, an oxidant and normal butane into a reactor containing a catalyst for contact.

6. The method according to any one of claims 1 to 3, wherein: The reaction raw materials of this method also contain water vapor; Preferably, the amount of water vapor used is 0-1%, preferably 0-0.5%, of the amount of n-butane.

7. The method according to any one of claims 1 to 3, wherein: The reaction raw materials of this method also contain a phosphorus supplement; Preferably, the amount of the phosphorus supplement agent is 0-1%, preferably 0-0.5%, of the amount of n-butane substance.

8. The method according to any one of claims 1 to 7, wherein: The reaction conditions include: temperature of 370-440°C, preferably 400-440°C; volume space velocity of 1000-2200h -1 , preferably 1500-2100h -1 ; The pressure is 0.01-0.09MPa, preferably 0.02-0.08MPa.

9. The method according to any one of claims 1 to 8, wherein: The oxidant is an oxygen-containing gas, preferably air.

10. The method according to any one of claims 1 to 9, wherein: The catalyst is a vanadium phosphorus oxygen catalyst; Preferably, based on the total mass of the catalyst, the mass content of vanadium is 28-35%, preferably 30-34%; the mass content of phosphorus is 15-25%, preferably 18-22%; Preferably, the bulk density of the catalyst is 0.6-0.85 g / cm 3 , preferably 0.7-0.8 g / cm 3 .

Citation Information

Patent Citations

  • Vanadium-phosphorus oxide catalyst for preparing maleic anhydride through butane oxidation, and preparation method thereof

    CN104607219A

  • Process method for preparing maleic anhydride from n-butane by oxidation

    CN108101871A

  • Vanadium phosphorus oxide catalyst for preparing maleic anhydride from n-butane through oxidation and preparation method thereof

    CN108339558A

  • Production technology for preparing maleic anhydride through oxidation of n-butane

    CN109053647A