Agricultural radial rubber tire tread rubber and preparation process thereof
By using smoke sheet rubber, butadiene rubber and modifiers such as silica fiber, polycarbonate, etc., the tear resistance and noise reduction performance of agricultural tire tread rubber are improved, and the tread rubber is easily scratched or cut. The problem of breakage is eliminated, the service life is extended and the noise is reduced.
Patent Information
- Application Number
- CN202411036132.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing agricultural tire tread rubber is easily scratched or cut when driving on field roads and hard stubble fields, resulting in chipping and chipping, and has a short service life.
It uses tobacco rubber and butadiene rubber as raw materials, combines the advantages of natural rubber and synthetic rubber, adds materials such as silica fiber, polycarbonate and polyborosiloxane, and improves tire performance through modified carbon black and EVA resin and other modifiers. The mechanical properties and noise reduction effect of the top glue form a stable hybrid system to enhance wear resistance and tear resistance.
Significantly improves the tear resistance, tensile resistance and noise reduction performance of the agricultural rubber tire tread compound, extends the service life, reduces noise during driving, and enhances the overall mechanical properties of the tread compound.
Smart Images

Figure BDA0004971114400000121 
Figure BDA0004971114400000131
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of truck tires, and more specifically, to an agricultural radial rubber tire tread rubber and a preparation process thereof. Background Art
[0002] Agricultural tires are a special field, and they do not have problems such as excessive heat generation and high-speed driving. At present, the most widely used agricultural tires are radial tires, which are mainly composed of tread, steel wire or cord carcass, cord layer edge wrapping, wire rings, etc. The tread rubber is the outermost layer of the tire that contacts the road surface and has a pattern printed on the surface. It can give the tire traction, buffer the impact and swing during driving, and prevent the cord layer from being cut and punctured. It is required to have high wear resistance, fatigue resistance, good aging resistance, good tensile strength, elasticity and toughness. It can be made of raw rubber such as natural rubber, styrene-butadiene rubber, cis-isoprene rubber and cis-butadiene rubber. A large amount of carbon black is often added to the rubber to improve its physical and mechanical properties.
[0003] In the prior art, a Chinese invention patent document with application number CN2019106501938 discloses a tire tread rubber, which includes the following components by weight: 13.0 to 23.0 parts of natural rubber, 11.0 to 21.0 parts of neodymium-based butadiene rubber, 39.9 to 53.6 parts of high styrene solution polymerized styrene butadiene rubber, 27.0 to 37.0 parts of medium styrene solution polymerized styrene butadiene rubber, and 78. 0-88.0 parts, environmentally friendly aromatic oil 13.0-23.0 parts, silane coupling agent 10.0-16.0 parts, anti-slip resin 2.0-8.0 parts, activator 3.0-5.0 parts, white carbon black dispersant 2.0-4.0 parts, alkoxysilicon modified polybutadiene liquid rubber 2.0-6.0 parts, antioxidant 3.0-5.0 parts, protective wax 1.0-2.0 parts, vulcanizing agent 4.4-6.4 parts.
[0004] Although the tire tread in the above technology has low rolling resistance, anti-wet skid and dry braking performance, in agricultural machinery, the tires often travel on poor field roads and hard stubble fields, especially in the rainy season, and the tires are easily scratched or cut, resulting in chipping and falling off. Summary of the invention
[0005] In order to improve the tear resistance and cut resistance of agricultural rubber tire tread rubber and extend the service life of agricultural rubber tires, the present application provides an agricultural radial rubber tire tread rubber and a preparation process thereof.
[0006] In a first aspect, the present application provides an agricultural radial rubber tire tread rubber, which adopts the following technical solution: A tread rubber for an agricultural radial rubber tire comprises 158-189.3 parts of a masterbatch, 1.2-1.6 parts of a vulcanizer, 0.5-1 parts of an accelerator, and 0.15-0.2 parts of a scorch retarder; the masterbatch comprises the following raw materials in parts by weight: 55-65 parts of smoked sheet rubber, 35-45 parts of butadiene rubber, 52-60 parts of fillers, 1.8-2.2 parts of softening oil, 3.5-4.5 parts of zinc oxide, 1.8-2.2 parts of a lubricant, 1.5-2 parts of a protective wax, 4-5 parts of an antioxidant, 1.8-2.2 parts of a DCPD resin, and 0.8-1.2 parts of an anti-reversion agent.
[0007] By adopting the above technical scheme, using smoked rubber and butadiene rubber as raw materials, the smoked rubber has good physical properties, good flexibility resistance and low heat generation, and the butadiene rubber is made by polymerization of butadiene, and has high elasticity, cold resistance and wear resistance. The two have good compatibility and can form a stable mixed system. They combine the advantages of natural rubber and synthetic rubber and have relatively excellent physical and mechanical properties.
[0008] Optionally, the butadiene rubber comprises neodymium-based butadiene rubber and nickel-based butadiene rubber in a mass ratio of 1:0.3-0.5.
[0009] By adopting the above technical scheme, the neodymium-based butadiene rubber is a polybutadiene rubber with a high cis-1,4-structure content obtained by coordination polymerization with a rare earth catalyst. It has the advantages of high stereoregularity and adjustable relative molecular weight distribution, high molecular chain flexibility, and can reduce tire hysteresis, reduce heat generation, and improve wear resistance and anti-skid performance. The nickel-based butadiene rubber has a narrow molecular weight distribution, a regular structure, and good wear resistance, cold resistance and elasticity. The two can be used in combination to complement each other and improve the comprehensive performance of the tread rubber.
[0010] Optionally, the protective wax comprises the following raw materials in parts by weight: 2.8-4.2 parts of paraffin wax, 1-2 parts of microcrystalline wax, 0.5-1 parts of alkylphenol formaldehyde tackifying resin and 1.2-2.4 parts of silica fiber.
[0011] The tread of agricultural tires is wider and has a larger support surface, which will displace more air and push more air masses. The shock absorption ability is poor and the noise is louder during driving. If an emergency occurs, it is difficult to hear the voices of nearby people giving warnings. By adopting the above technical solution, silica fiber is used as a reinforcing phase and is evenly dispersed in paraffin and microcrystalline wax, which can more effectively fill the tiny cracks in the wax body, thereby improving the mechanical strength of the overall material. Moreover, silica fiber can construct a three-dimensional network structure in the tread rubber with the wax body and form a supporting frame in the wax body, which can not only enhance the mechanical strength of the wax layer, but also improve the overall mechanical properties of the tread rubber. Moreover, silica fiber has a porous structure and a high specific surface area, which gives it excellent sound absorption performance, thereby achieving sound insulation and noise reduction effects, and can effectively absorb and dissipate sound wave energy. , reduce the noise level, alkyl phenol formaldehyde tackifying resin has excellent viscosity to natural rubber, because the phenol ring has a certain degree of branching and good flexibility of the substituted alkane group, has good compatibility with rubber molecules, phenolic hydroxyl has a certain polarity, can form hydrogen bonds with each other, in the mixing process on the rubber interface to form an interpenetrating hydrogen bond network structure, thereby enhancing the mutual penetration and diffusion between rubber molecules or at the two bonding surfaces, so that the rubber achieves uniform and full fusion, facilitates the uniform dispersion of silica fibers in the wax body and rubber material, facilitates the distribution of a more uniform silica network structure, and enhances the interface bonding force between silica and paraffin wax, smoke sheet rubber and other materials, good interface bonding force can ensure the effective transfer of stress between materials, thereby improving the wear resistance, noise reduction effect and mechanical strength of the tread rubber.
[0012] Optionally, the preparation method of the nano silicon dioxide fiber is as follows: Adding nano silicon powder into a mixture of ethanol and distilled water, and uniformly dispersing by ultrasonication to obtain a dispersion; The polycarbonate is dissolved to obtain a matrix solution with a concentration of 8-10 wt%, and the dispersion liquid is added and stirred evenly to obtain a spinning solution, and electrospinning is performed to obtain a fiber membrane, wherein the mass ratio of nano silicon powder to polycarbonate is 1:8-10; The fiber membrane is kept at 300-330° C. for 6-7 hours, then heated to 800-820° C., calcined for 0.5-1 hour, cooled to room temperature, and ball-milled to obtain nano-silica fibers with a length of 100-150 μm.
[0013] By adopting the above technical scheme, polycarbonate is a thermoplastic engineering plastic with excellent mechanical properties, weather resistance, heat resistance and transparency, etc., and has good sound insulation effect. Silicon dioxide in polycarbonate can reduce the cross-linking points of matrix molecules, improve the compatibility of polycarbonate and silicon dioxide, form phase separation in the microphase interval, thereby improving the damping performance of polycarbonate, and when sound waves pass through the material, the resistance they receive is greater, and the loss of sound energy increases. In addition, the addition of nanoparticles can also improve the mechanical properties of the fiber. Nano-silicon powder with a small particle size and a large specific surface area has a high interfacial bonding strength with polycarbonate. When sound waves are transmitted, they need to overcome greater resistance, thereby improving the sound insulation effect of the composite material; and polycarbonate is used as the fiber matrix of nano-silicon dioxide, which has high impact strength. When the silicon dioxide fiber is impacted by external force, it can better absorb and disperse energy, and play a buffering and shock-absorbing role through elastic deformation absorption and dispersion capabilities, so that the material is not easy to break or deform after being impacted, which is beneficial to protecting the service life of the tread rubber, and can achieve the effect of buffering and noise reduction.
[0014] Optionally, the silica fiber is pretreated as follows: The polyborosiloxane and isopropanol are mixed in a mass ratio of 5:1-2 to obtain a composite liquid, and 0.5-1wt% of glass fiber powder is added to the composite liquid, and ultrasonically homogenized to obtain a treatment liquid; The silica fiber is immersed in the treatment liquid for 10-12 hours, filtered, and dried at 100-120°C for 8-10 hours to obtain an intermediate; the intermediate is mixed with a zinc sulfate solution, a sodium carbonate solution and hexadecyltrimethylammonium bromide are added, the temperature is raised to 60-70°C, stirred for 20-24 hours, filtered, and calcined at 400-600°C for 3-4 hours, and the mass ratio of the intermediate, the zinc sulfate solution, the sodium carbonate solution and the hexadecyltrimethylammonium bromide is 1-2:10:10:0.1-0.2.
[0015] By adopting the above technical scheme, polyborosiloxane has greater viscosity, isopropanol is used as a solvent for dilution to form a polyborosiloxane polymer solution, and glass fiber powder is added. It improves the shock absorption, buffering and noise reduction effects through elastic deformation, and can block and absorb noise, improve the sound absorption ability, and the formed treatment liquid is impregnated with silica fiber. Polyborosiloxane forms a film on the silica fiber, and entanglement is generated between its molecules. The boron oxygen dynamic reversible bonds are rebonded, so that the film has self-repairing properties, and the silica fiber has certain long-term anti-cracking and wear-resistant effects. Then, zinc sulfate and sodium carbonate are used to synthesize zinc carbonate, which is calcined to form zinc oxide. Zinc oxide uses silica fiber as a carrier and is coated on the surface of silica fiber, which can improve the cross-linking degree of the rubber, accelerate vulcanization, improve processing performance, physical and mechanical properties, heat resistance, etc., and has a strong reinforcement effect on the mechanical properties of the tread rubber.
[0016] Optionally, the polyborosiloxane is prepared by mixing terminal hydroxyl polydimethylsiloxane having a hydroxyl mass fraction of 2.5% and boric acid in a molecular molar ratio of 1:1.
[0017] By adopting the above technical scheme, the silanol group at the end of the terminal hydroxyl polydimethylsiloxane molecular chain and the boronolol group in boric acid are dehydrated and condensed to form polyborosiloxane. The bond length of Si-O bond is longer, and the steric hindrance and rotation barrier are lower, so the molecular chain exhibits good flexibility. When the polyborosiloxane is damaged, the molecular chains can approach each other and become entangled with each other, so that a self-repairing effect can be achieved, thereby improving the service life of the tread rubber and improving the crack resistance and wear resistance.
[0018] Optionally, the particle size of the glass fiber powder is 50-100 nm.
[0019] By adopting the above technical solution, the glass fiber particle size is made smaller and can be dispersed in the composite liquid and loaded on the silica fiber during impregnation, which can effectively absorb and block the propagation of sound waves and produce better sound insulation. In addition, the glass fiber itself has good hardness and strength and can maintain good stability and durability during friction and wear, thereby improving the noise reduction effect and wear resistance of silica.
[0020] Optionally, the filler is modified carbon black, and the modified carbon black is prepared by the following method: By weight, 3-3.5 parts of carbon black and 3-3.5 parts of fly ash are mixed, and surface treated with 0.06-0.07 parts of silane coupling agent to prepare a pretreated material; 10-11 parts of EVA resin are melted at 120-125° C., the pretreated material, 0.3-0.7 parts of azodicarbonamide and 0.2-0.4 parts of diisopropylbenzene peroxide are added, kneaded for 30-40 minutes, hot pressed for 8-10 minutes and cold pressed for 4-5 minutes at 130-140° C. and 8-10 MPa, and crushed into 2-5 mm particles.
[0021] By adopting the above technical scheme, fly ash, as a bulk industrial solid liquid, not only occupies a large amount of land resources, but also poses a serious threat to the environment and water sources. At present, the use of fly ash is mainly limited to the preparation of cement and other building materials. EVA resin is a thermoplastic resin formed by high-pressure bulk polymerization of non-polar, crystalline ethylene monomer and strongly polar, non-crystalline vinyl acetate monomer in the presence of an initiator. It is a high-branched random copolymer. Its foaming material, as a multifunctional new material composed of solid phase and gas phase, has good plasticity, good elasticity, and can absorb shock. In order to achieve the advantages of load-bearing, heat preservation, sound insulation and sound absorption, fly ash is mixed with carbon black, and the surface is modified by silane coupling agent to improve the compatibility of carbon black, fly ash and EVA resin. After foaming with azodicarbonamide, EVA can produce pores, which are the same as the outside world through the surface of the material. When the sound wave is incident on the surface of the material, the many tiny holes that penetrate each other inside make the sound wave fully contact and rub with the micropore wall, and convert the sound energy into heat energy for consumption, so as to have a better sound absorption coefficient. The fly ash and carbon black are fixed in the composite material by EVA resin, which can improve the wear resistance of the composite material.
[0022] Optionally, the antioxidant includes antioxidant RD and antioxidant 4020 in a mass ratio of 1.5:2.5-3.5; The softening oil is selected from at least one of aromatic oil, naphthenic oil and paraffin oil; The lubricant is selected from at least one of stearic acid, paraffin oil and silicone oil; The scorch retarder is selected from at least one of N-cyclohexylthiophthalimide and N,N-dibenzhydryl-1,6-hexanediisocyanate; The accelerator is selected from at least one of accelerator DM, accelerator NS and accelerator TMTD; The vulcanizing agent is selected from at least one of sulfur, benzoyl peroxide or sulfur monochloride; The anti-reversion agent is anti-reversion agent WK-901 or PK-900.
[0023] By adopting the above technical solution, the antioxidant reduces the influence of external factors such as heat, mechanical stress, light and chemical corrosion on the tread rubber, prevents it from degradation and aging, and thus causes the tread rubber to lose its use value.
[0024] Lubricants can form a lubricating film on the rubber surface, reduce the friction resistance in rubber mixing, extrusion, calendering and other processes, and improve processing performance and product quality.
[0025] Softening oil can play the role of plasticization, softening and filling, and can improve the processing performance and physical properties of rubber. Aromatic oil is mainly composed of aromatic hydrocarbons, with good compatibility and comprehensive performance. Cycloalkane oil is mainly composed of cycloalkanes, with good low-temperature performance, and can reduce the brittle temperature of rubber. Paraffin oil is mainly composed of straight-chain alkanes, which can improve the rubber's antioxidant properties and high temperature resistance.
[0026] Anti-scorch agents are mainly used to prevent premature vulcanization of rubber during processing, extend the mixing and processing time of rubber, and avoid hardening or coking of rubber when the expected degree of vulcanization has not been reached.
[0027] Accelerators can accelerate the vulcanization process, reduce the vulcanization temperature, shorten the vulcanization time, and improve the physical and mechanical properties and aging resistance of rubber.
[0028] Vulcanizing agents are used to cross-link rubber molecules, making the tread rubber have better elasticity, wear resistance, oil resistance and other properties, thereby increasing the service life of the rubber.
[0029] Anti-reversion agent is mainly used to prevent rubber from reversion to its original state under long-term high temperature, thereby extending the service life of tread rubber.
[0030] In a second aspect, the present application provides a process for preparing a tread rubber for an agricultural radial rubber tire, which adopts the following technical solution: A preparation process of agricultural radial rubber tire tread rubber comprises the following steps: mixing smoked rubber, butadiene rubber, filler, softening oil, zinc oxide, lubricant, protective wax, antioxidant, DCPD resin and anti-reversion agent, and discharging the rubber at 155-165° C. to obtain a masterbatch; The master rubber is mixed with a vulcanizing agent, an accelerator and a scorch retarder, and kneaded, and discharged at 95-105° C. to obtain a tread rubber.
[0031] By adopting the above technical scheme, the masterbatch is mixed and kneaded with components such as a vulcanizing agent, thereby improving the tear resistance and tensile strength of the tread rubber, so that the manufactured agricultural rubber tire has good durability.
[0032] In summary, this application has the following beneficial effects: 1. Since the present application adopts smoked rubber, neodymium-based butadiene rubber, nickel-based butadiene rubber, etc. as raw materials for tread rubber, the tread rubber prepared by combining various raw materials has strong mechanical properties such as tensile resistance and tear resistance, and good wear resistance.
[0033] 2. In the present application, paraffin wax, microcrystalline wax, alkylphenolic tackifying resin and silica fiber are preferably used to prepare protective wax, which can improve the overall mechanical properties of the tread rubber and achieve noise reduction and sound absorption effects. In addition, polycarbonate is used as the main material of the silica fiber, so that the silica fiber has good elastic deformation ability, so that the agricultural tire has good buffering and shock absorption effects and low noise during driving.
[0034] 3. In the present application, polyborosiloxane and glass fiber powder are preferably used to treat the silica fiber, and then zinc oxide is synthesized on its surface by zinc sulfate and sodium carbonate to improve the cross-linking degree of the rubber and further enhance the mechanical properties and noise reduction effect.
[0035] 4. In the present application, fly ash, EVA resin and azodicarbonamide are preferably used to modify carbon black. Fly ash can increase the wear resistance and noise reduction effect of the rubber material, and EVA can improve the wear resistance and noise reduction and sound absorption effect of the tread rubber. DETAILED DESCRIPTION
[0036] The following examples further illustrate the present application in detail.
[0037] Preparation Examples 1-4 of Silica Fibers Preparation Example 1: (1) 3 g of nano silicon powder was added to a mixture of 150 mL of ethanol and 50 mL of distilled water, and ultrasonicated for 30 min to disperse uniformly to obtain a dispersion. The particle size of the nano silicon powder was 20 nm. (2) 30 g of polycarbonate was dissolved in an organic solvent to obtain a matrix solution with a concentration of 10 wt%, and the dispersion was added and stirred evenly to obtain a spinning solution, and electrospinning was performed to obtain a fiber membrane. The organic solvent was dimethylformamide and tetrahydrofuran, and the volume ratio of the two was 75:25. The mass ratio of nano-silicon powder and polycarbonate was 1:10. The polycarbonate was selected from Lotte Chemical of South Korea, model PC-1100. The voltage during electrospinning was 16 kV, the injection rate was 1.5 mL / h, and the receiving distance was 20 cm; (3) The prepared fiber membrane was kept at 330°C for 6 hours, then heated to 800°C and calcined for 1 hour. After cooling to room temperature, it was ball milled to obtain nano-silica fibers with a length of 150 μm.
[0038] Preparation Example 2: (1) 3 g of nano silicon powder was added to a mixture of 150 mL of ethanol and 50 mL of distilled water, and ultrasonicated for 30 min to disperse uniformly to obtain a dispersion. The particle size of the nano silicon powder was 30 nm. (2) 24 g of polycarbonate was dissolved in an organic solvent to obtain a matrix solution with a concentration of 8 wt%, and the dispersion was added and stirred evenly to obtain a spinning solution, and electrospinning was performed to obtain a fiber membrane. The organic solvent was dimethylformamide and tetrahydrofuran, and the volume ratio of the two was 75:25. The mass ratio of nano-silicon powder and polycarbonate was 1:8. The polycarbonate was selected from Lotte Chemical of South Korea, model PC-1100. The voltage during electrospinning was 16 kV, the injection rate was 1.5 mL / h, and the receiving distance was 20 cm. (3) The prepared fiber membrane was kept at 300°C for 7 hours, then heated to 820°C and calcined for 0.5 hours. After cooling to room temperature, it was ball milled to obtain nano-silica fibers with a length of 100 μm.
[0039] Preparation Example 3: The difference from Preparation Example 1 is that an equal amount of polyvinylpyrrolidone (PVP) is used to replace polycarbonate.
[0040] Preparation Example 4: The difference from Preparation Example 1 is that in step (3), the fiber membrane is not kept at 300°C for 6 hours and calcined at 800°C for 1 hour, but the fiber membrane is directly ball-milled to obtain silica fibers with a length of 150 μm.
[0041] Preparation Example 5-10 of Modified Carbon Black Preparation Example 5: 35 g of carbon black and 35 g of fly ash were mixed, 0.7 g of silane coupling agent KH858 was dissolved in 99.3 g of anhydrous ethanol, and added to the mixture of carbon black and fly ash, and immersed at room temperature for 10 h, filtered, and dried to obtain a pretreated material, wherein the carbon black model was N234 and the fly ash was grade II fly ash; 110g EVA resin was melted at 120°C, and pretreated material, 7g azodicarbonamide and 4g diisopropylbenzene peroxide were added, mixed for 40min, hot pressed for 10min and cold pressed for 4min at 140°C and 10MPa, and crushed into 5mm particles. The EVA resin was selected from DuPont of the United States, and the product number was 150W.
[0042] Preparation Example 6: 30 g of carbon black and 30 g of fly ash were mixed, 0.6 g of silane coupling agent KH858 was dissolved in 99.4 g of anhydrous ethanol, and added to the mixture of carbon black and fly ash, and immersed at room temperature for 10 h, filtered, and dried to obtain a pretreated material, wherein the carbon black model was N234 and the fly ash was grade II fly ash; 100g EVA resin was melted at 125°C, and pretreated material, 3g azodicarbonamide and 2g diisopropylbenzene peroxide were added, mixed for 30min, hot pressed for 8min and cold pressed for 5min at 130°C and 8MPa, and crushed into 2mm particles. The EVA resin was selected from DuPont of the United States, and the product number was 150W.
[0043] Preparation Example 7: The difference from Preparation Example 5 is that the silane coupling agent KH858 is not used to perform surface treatment on carbon black and fly ash.
[0044] Preparation Example 8: The difference from Preparation Example 5 is that fly ash is not added.
[0045] Preparation Example 9: The difference from Preparation Example 5 is that the foaming agent azodicarbonamide is not added.
[0046] Preparation Example 10: The difference from Preparation Example 5 is that EVA resin, azodicarbonamide and diisopropylbenzene peroxide are not used, and the pretreated material is used as modified carbon black. Example
[0047] Example 1: An agricultural radial rubber tire tread rubber, comprising 172.5 kg masterbatch, 1.4 kg vulcanizer, 0.7 kg accelerator and 0.18 kg anti-scorch agent, wherein the vulcanizer is sulfur powder, the accelerator is accelerator NS, the anti-scorch agent is anti-scorch agent CTP (N-cyclohexylthiophthalamide), the raw material dosage of the masterbatch is shown in Table 1, wherein the smoke sheet rubber is 3# smoke sheet rubber, selected from Jiangsu Bohai Rubber and Plastic Technology Co., Ltd., with a product number of RSS3, and the butadiene rubber is neodymium butadiene rubber, selected from Shanghai Duokang Industrial , the item number is CB24, the filler is carbon black, the model is N234, the softening oil is aromatic oil, selected from Shandong Xinjiu New Material Technology Co., Ltd., the item number is TC-FTY, the lubricant is stearic acid, the protective wax is selected from Henan Jiapei Environmental Protection Technology Co., Ltd., the item number is LY-03, the antioxidant includes antioxidant RD and antioxidant 4020 with a mass ratio of 1.5:2.5, the DCPD resin is selected from Guangzhou Qian'an Chemical Co., Ltd., the model is XD-1000, and the anti-aging reversion agent is selected from Germany Lanxess, the model is PK-900.
[0048] The preparation process of the above agricultural radial rubber tire tread rubber comprises the following steps: The smoked sheet rubber, butadiene rubber, filler, softening oil, zinc oxide, lubricant, protective wax, antioxidant, DCPD resin and anti-reversion agent were mixed for 5 hours, and the rubber was discharged at 155°C to obtain a masterbatch; The masterbatch was mixed with the vulcanizer, accelerator and scorch retarder and kneaded for 4 hours, and the rubber was discharged at 95°C to obtain the tread rubber.
[0049] Table 1 Raw material dosage of masterbatch in Examples 1-3 Raw material / kg Example 1 Example 2 Example 3 Smoked rubber sheet (3#) 60 55 65 Butadiene rubber (neodymium series) 40 35 45 Filler (Carbon Black N234) 56 52 60 Softening oil (aromatic oil) 2 1.8 2.2 Zinc Oxide 4 3.5 4.5 Lubricant (stearic acid) 2 1.8 2.2 Protective wax 1.5 1.8 2 Antioxidant RD 1.5 1.5 1.5 Antioxidant 4020 2.5 3 3.5 DCDP resin 2 1.8 2.2 Anti-aging agent PK-900 1 0.8 1.2 Example 2: An agricultural radial rubber tire tread rubber, comprising 158 kg masterbatch, 1.2 kg vulcanizer, 0.5 kg accelerator and 0.15 kg anti-scorch agent, wherein the vulcanizer is benzoyl peroxide, the accelerator is accelerator DM, the anti-scorch agent is anti-scorch agent DPG (N, N-diphenylmethylene-1,6-hexane diisocyanate), the raw material dosage of the masterbatch is shown in Table 1, wherein the smoke sheet rubber is 3# smoke sheet rubber, selected from Jiangsu Bohai Rubber and Plastic Technology Co., Ltd., with the product number RSS3, and the butadiene rubber is neodymium butadiene rubber selected from Shanghai Duokang Industrial, item number CB24, filler is carbon black, model number N234, softening oil is aromatic oil, selected from Shandong Xinjiu New Material Technology Co., Ltd., item number TC-FTY, lubricant is stearic acid, protective wax is selected from Henan Jiapei Environmental Protection Technology Co., Ltd., item number LY-03, antioxidants include antioxidant RD and antioxidant 4020 with a mass ratio of 1.5:3, DCPD resin is selected from Guangzhou Qian'an Chemical Co., Ltd., model number XD-1000, anti-aging agent is selected from Shanghai Junpu, model number WK-901.
[0050] The preparation process of the above agricultural radial rubber tire tread rubber comprises the following steps: The smoked sheet rubber, butadiene rubber, filler, softening oil, zinc oxide, lubricant, protective wax, antioxidant, DCPD resin and anti-vulcanization reversion agent were mixed for 5 hours, and the rubber was discharged at 165°C to obtain a masterbatch; The masterbatch was mixed with the vulcanizer, accelerator and scorch retarder for 4 hours and discharged at 105°C to obtain the tread rubber.
[0051] Example 3: An agricultural radial rubber tire tread rubber, comprising 189.3 kg masterbatch, 1.6 kg vulcanizer, 1 kg accelerator and 0.2 kg anti-scorch agent, wherein the vulcanizer is benzoyl peroxide, the accelerator is accelerator DM, the anti-scorch agent is anti-scorch agent DPG (N, N-diphenylmethylene-1,6-hexane diisocyanate), the raw material dosage of the masterbatch is shown in Table 1, wherein the smoke sheet rubber is 3# smoke sheet rubber, selected from Jiangsu Bohai Rubber and Plastic Technology Co., Ltd., with the product number RSS3, and the butadiene rubber is neodymium-based butadiene rubber selected from Shanghai Polymer Technology Co., Ltd. Kangshiye, item number CB24, filler is carbon black, model number N234, softening oil is aromatic oil, selected from Shandong Xinjiu New Material Technology Co., Ltd., item number TC-FTY, lubricant is stearic acid, protective wax is selected from Henan Jiapei Environmental Protection Technology Co., Ltd., item number LY-03, antioxidants include antioxidant RD and antioxidant 4020 with a mass ratio of 1.5:3.5, DCPD resin is selected from Guangzhou Qian'an Chemical Co., Ltd., model number XD-1000, anti-aging agent is selected from Shanghai Junpu, model number WK-901.
[0052] The preparation process of the above agricultural radial rubber tire tread rubber comprises the following steps: The smoked sheet rubber, butadiene rubber, filler, softening oil, zinc oxide, lubricant, protective wax, antioxidant, DCPD resin and anti-vulcanization reversion agent were mixed for 5 hours, and the rubber was discharged at 165°C to obtain a masterbatch; The masterbatch was mixed with the vulcanizer, accelerator and scorch retarder for 4 hours and discharged at 105°C to obtain the tread rubber.
[0053] Example 4: An agricultural radial rubber tire tread rubber. Compared with Example 1, the butadiene rubber includes neodymium butadiene rubber and nickel butadiene rubber in a mass ratio of 1:0.5. The neodymium butadiene rubber is selected from Shanghai Duokang Industry with the item number CB24, and the nickel butadiene rubber is selected from Daqing Petrochemical with the model number BR9000.
[0054] Example 5: An agricultural radial rubber tire tread rubber. Compared with Example 1, the butadiene rubber includes neodymium butadiene rubber and nickel butadiene rubber in a mass ratio of 1:0.3. The neodymium butadiene rubber is selected from Shanghai Duokang Industry with the item number CB24, and the nickel butadiene rubber is selected from Daqing Petrochemical with the model number BR9000.
[0055] Example 6: An agricultural radial rubber tire tread rubber. Compared with Example 4, the protective wax is made by mixing the following raw materials, melting and mixing at 80°C, drying and crushing: 4.2kg paraffin wax, 2kg microcrystalline wax, 1kg alkyl phenolic tackifying resin and 2.4kg silica fiber, the alkyl phenolic tackifying resin is selected from Guangzhou Liben Rubber Raw Material, model T-5600, and the silica fiber is made by Preparation Example 1.
[0056] Example 7: An agricultural radial rubber tire tread rubber. Compared with Example 4, the protective wax is made by mixing the following raw materials, melting and mixing at 80°C, drying and crushing: 2.8kg paraffin wax, 1kg microcrystalline wax, 0.5kg alkyl phenolic tackifying resin and 1.5kg silica fiber, the alkyl phenolic tackifying resin is selected from Guangzhou Liben Rubber Raw Material, model T-5600, and the silica fiber is made by Preparation Example 2.
[0057] Example 8: An agricultural radial rubber tire tread rubber, compared with Example 6, the silica fiber is made from Preparation Example 3.
[0058] Example 9: An agricultural radial rubber tire tread rubber. Compared with Example 6, the silica fiber is made from Preparation Example 4.
[0059] Example 10: An agricultural radial rubber tire tread rubber, compared with Example 6, no alkylphenol formaldehyde tackifying resin is added to the protective wax.
[0060] Example 11: An agricultural radial rubber tire tread rubber, compared with Example 6, no silica fiber is added to the protective wax.
[0061] Example 12: An agricultural radial rubber tire tread rubber, compared with Example 6, the silica fiber is pretreated as follows: 5 kg of polyborosiloxane and isopropanol were mixed in a mass ratio of 5:1 to obtain a composite liquid, 1 wt % of glass fiber powder was added to the composite liquid, and ultrasonicated at 300 W and 40 KHz for 3 h to obtain a treatment liquid, wherein the polyborosiloxane was prepared by mixing a terminal hydroxyl polydimethylsiloxane having a hydroxyl mass fraction of 2.5% and boric acid in a molecular molar ratio of 1:1, and reacting at 150° C. for 10 min, the terminal hydroxyl polydimethylsiloxane was selected from Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd., model JP-203, and the particle size of the glass fiber powder was 100 nm; 2.4 kg of silica fiber was immersed in the treatment solution for 12 h, filtered, and dried at 100 °C for 10 h to obtain an intermediate; The intermediate was mixed with a 3 mol / l zinc sulfate solution, 2 mol / l sodium carbonate solution and hexadecyltrimethylammonium bromide were added, the temperature was raised to 70°C, stirred for 20 hours, filtered, and calcined at 400°C for 4 hours. The mass ratio of the intermediate, zinc sulfate solution, sodium carbonate solution and hexadecyltrimethylammonium bromide was 1:10:10:0.1.
[0062] Embodiment 13: A tread rubber for an agricultural radial rubber tire. Compared with Embodiment 6, the silica fiber is pretreated as follows: 5 kg of polyborosiloxane is mixed with isopropanol in a mass ratio of 5:2 to obtain a composite liquid, 1 wt % of glass fiber powder is added to the composite liquid, and ultrasonicated at 300 W and 40 KHz for 3 h to obtain a treated liquid, wherein the polyborosiloxane is prepared by mixing a terminal hydroxyl polydimethylsiloxane having a hydroxyl mass fraction of 2.5% and boric acid in a molecular molar ratio of 1:1, and reacting at 150° C. for 10 min. The terminal hydroxyl polydimethylsiloxane is selected from Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd., model JP-203, and the particle size of the glass fiber powder is 50 nm; 2.4 kg of silica fiber was immersed in the treatment solution for 10 h, filtered, and dried at 120 °C for 8 h to obtain an intermediate; The intermediate was mixed with a 3 mol / l zinc sulfate solution, 2 mol / l sodium carbonate solution and hexadecyltrimethylammonium bromide were added, the temperature was raised to 60°C, stirred for 24 hours, filtered, and calcined at 600°C for 3 hours. The mass ratio of the intermediate, zinc sulfate solution, sodium carbonate solution and hexadecyltrimethylammonium bromide was 2:10:10:0.2.
[0063] Example 14: An agricultural radial rubber tire tread rubber, compared with Example 12, the silica fiber is pretreated as follows: Mix 2.4 kg of silica fiber with a 3 mol / l zinc sulfate solution, add 2 mol / l sodium carbonate solution and hexadecyltrimethylammonium bromide, heat to 70°C, stir for 20 hours, filter, and calcine at 400°C for 4 hours. The mass ratio of silica fiber, zinc sulfate solution, sodium carbonate solution and hexadecyltrimethylammonium bromide is 1:10:10:0.1.
[0064] Example 15: An agricultural radial rubber tire tread rubber, compared with Example 12, the silica fiber is pretreated as follows: 5 kg of polyborosiloxane and isopropanol were mixed in a mass ratio of 5:1 to obtain a composite liquid, 1 wt % of glass fiber powder was added to the composite liquid, and ultrasonicated at 300 W and 40 KHz for 3 h to obtain a treatment liquid, wherein the polyborosiloxane was prepared by mixing a terminal hydroxyl polydimethylsiloxane having a hydroxyl mass fraction of 2.5% and boric acid in a molecular molar ratio of 1:1, and reacting at 150° C. for 10 min, and the terminal hydroxyl polydimethylsiloxane was selected from Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd., and the model was JP-203; 2.4 kg of silica fibers were immersed in the treatment solution for 12 h, filtered, and dried at 100° C. for 10 h.
[0065] Example 16: An agricultural radial rubber tire tread rubber, compared with Example 12, the silica fiber is pretreated as follows: 5 kg of polyborosiloxane was mixed with isopropanol at a mass ratio of 5:1 to obtain a composite liquid, and ultrasonicated at 300 W and 40 KHz for 3 h to obtain a treatment liquid. The polyborosiloxane was prepared by mixing a terminal hydroxyl polydimethylsiloxane having a hydroxyl mass fraction of 2.5% and boric acid at a molecular molar ratio of 1:1, and reacting at 150° C. for 10 min. The terminal hydroxyl polydimethylsiloxane was selected from Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd., and the model was JP-203; 2.4 kg of silica fibers were immersed in the treatment solution for 12 h, filtered, and dried at 100° C. for 10 h.
[0066] Example 17: An agricultural radial rubber tire tread rubber, compared with Example 12, wherein the filler is modified carbon black, and the modified carbon black is made by Preparation Example 5.
[0067] Example 18: An agricultural radial rubber tire tread rubber, compared with Example 12, wherein the filler is modified carbon black, and the modified carbon black is made by Preparation Example 6.
[0068] Example 19: An agricultural radial rubber tire tread rubber, compared with Example 17, wherein the filler is modified carbon black, and the modified carbon black is made by Preparation Example 7.
[0069] Example 20: An agricultural radial rubber tire tread rubber, compared with Example 17, wherein the filler is modified carbon black, and the modified carbon black is made by Preparation Example 8.
[0070] Example 21: An agricultural radial rubber tire tread rubber, compared with Example 17, wherein the filler is modified carbon black, and the modified carbon black is made by Preparation Example 9.
[0071] Example 22: An agricultural radial rubber tire tread rubber, compared with Example 17, wherein the filler is modified carbon black, and the modified carbon black is made by Preparation Example 10.
[0072] Comparative Example Comparative Example 1: A tire tread rubber comprises the following components in parts by weight: 18.0 parts of natural rubber, 16.0 parts of neodymium-based butadiene rubber, 46.75 parts of high styrene solution polymerized styrene butadiene rubber, 32.0 parts of medium styrene solution polymerized styrene butadiene rubber, 83.0 parts of white carbon black, 17.7 parts of environmentally friendly aromatic oil, 14.0 parts of silane coupling agent, 5.0 parts of anti-slip resin, 4.0 parts of activator, 3.0 parts of white carbon black dispersant, 4.0 parts of alkoxysilicon-modified polybutadiene liquid rubber, 4.0 parts of antioxidant, 1.5 parts of protective wax, and 5.4 parts of vulcanizing accelerator.
[0073] Performance testing The tread rubber was prepared according to the methods in the examples and comparative examples, and the performance was tested according to the following methods. The test results are recorded in Table 2.
[0074] 1. Tensile strength and tensile permanent deformation: GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber" is used for testing.
[0075] 2. Tear strength: Test in accordance with GB / T529-2008 "Determination of tear strength of vulcanized rubber or thermoplastic rubber (trouser-shaped, right-angled and crescent-shaped specimens)".
[0076] 3. Noise: Test in accordance with GB / T32789-1016 “Tire noise test method – drum method”.
[0077] 4. Akron wear: Tested in accordance with GB / T1689-2014 "Determination of wear resistance of vulcanized rubber (using Akron abrasion tester)".
[0078] 5. Rebound resilience: Tested in accordance with GB / T1681-2009 "Determination of rebound resilience of vulcanized rubber".
[0079] Table 2 Performance test of rubber tire tread It can be seen from the data in Table 2 that the tread rubber prepared in Examples 1-3 has good tear resistance and tensile resistance, and is not easily scratched or cut when driving on hard stubble fields and other farmland.
[0080] Compared with Example 1, Example 4 and Example 5 use nickel-based and neodymium-based butadiene rubbers, the combination of which produces better tensile and tear resistance, and also increases the wear resistance.
[0081] Compared with Example 4, Example 6 and Example 7 use paraffin wax, microcrystalline wax, phenolic tackifying resin and silica fiber to prepare protective wax. Table 2 shows that the tread rubbers prepared in Example 6 and Example 7 have increased tensile strength, decreased tensile permanent deformation rate, improved resilience, increased wear resistance, and improved noise reduction effect.
[0082] In Example 8, the silica fiber prepared in Preparation Example 3 was used, and PVP was used to replace polycarbonate in Preparation Example 3. In Example 9, the silica fiber prepared in Preparation Example 4 was used, and Preparation Example 4 was not calcined. Compared with Preparation Example 6, the tensile strength of the tread rubber prepared in Examples 8 and 9 decreased, and the wear resistance was weakened.
[0083] In Example 10, no alkylphenol formaldehyde tackifying resin was added. Compared with Example 6, the tensile strength of the tread rubber was reduced, the tensile permanent deformation rate was increased, and the Akron wear was increased.
[0084] Compared with Example 6, no silica fiber is added in Example 11. As shown in Table 2, the noise reduction effect of the tread rubber is reduced, the rebound elasticity is slightly reduced, the wear resistance is weakened, and the mechanical properties are deteriorated.
[0085] Compared with Example 6, Examples 12 and 13 also use polyborosiloxane and the like to pretreat the silica fiber. Table 2 shows that the tread rubbers prepared in Examples 12 and 13 have increased tensile strength, reduced tensile permanent deformation, increased tear resistance, increased noise reduction effect, and improved wear resistance.
[0086] Compared with Example 12, in Example 14, zinc sulfate solution and calcium carbonate solution are further used to treat the silica fiber, in Example 15, polyborosiloxane and glass fiber powder are used to treat the silica fiber, and in Example 16, only polyborosiloxane is used to treat the silica fiber. The data in Table 2 show that the tread rubber prepared in Example 14 has decreased tensile strength, weakened tear resistance, and poor wear resistance, the tensile strength of the tread rubber in Example 15 decreases, the noise reduction effect is significantly reduced, and the wear resistance decreases, and the noise reduction effect of the tread rubber in Example 16 is poor.
[0087] Compared with Example 12, Example 17 and Example 18 use the modified carbon black prepared in Preparation Example 5 and Preparation Example 6 as fillers, respectively. The tensile strength and resilience of the tread rubber prepared thereby are increased, and the noise reduction effect is significantly improved.
[0088] In Example 19, the modified carbon black prepared in Preparation Example 7 was used. In Preparation Example 7, the silane coupling agent KH858 was not used to treat the carbon black and fly ash. Compared with Example 17, the tread rubber prepared in Example 19 had decreased tensile strength, weakened wear resistance, and decreased noise reduction ability.
[0089] In Example 20, the modified carbon black prepared in Preparation Example 8 was used, to which fly ash was not added. Compared with Example 17, the noise reduction effect and wear resistance of the tread rubber were reduced.
[0090] Compared with Example 17, in Example 21, azodicarbonamide is not used in the modified carbon black, and the noise reduction effect of the tread rubber is reduced. In Example 22, EVA resin or the like is not used for foaming, so the noise reduction ability of the tread rubber prepared thereby is reduced, and the tensile and tear resistance effects are weakened.
[0091] Comparative Example 1 is a tread rubber in the prior art, whose tensile strength and deformation capacity are inferior to those of the present application. When driving on farmland such as hard stubble fields, cracking and cutting phenomena are prone to occur.
[0092] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An agricultural radial rubber tire tread rubber, It is characterized in that The invention comprises 158-189.3 parts of a masterbatch, 1.2-1.6 parts of a vulcanizing agent, 0.5-1 parts of an accelerator and 0.15-0.2 parts of a scorch retarder; the masterbatch comprises the following raw materials in parts by weight: 55-65 parts of smoked sheet rubber, 35-45 parts of butadiene rubber, 52-60 parts of fillers, 1.8-2.2 parts of softening oil, 3.5-4.5 parts of zinc oxide, 1.8-2.2 parts of a lubricant, 1.5-2 parts of a protective wax, 4-5 parts of an antioxidant, 1.8-2.2 parts of a DCPD resin and 0.8-1.2 parts of an anti-reversion agent.
2. The agricultural radial rubber tire tread rubber according to claim 1, Features: The butadiene rubber comprises neodymium-based butadiene rubber and nickel-based butadiene rubber in a mass ratio of 1:0.3-0.
5.
3. The agricultural radial rubber tire tread rubber according to claim 1, Features: The protective wax comprises the following raw materials in parts by weight: 2.8-4.2 parts of paraffin wax, 1-2 parts of microcrystalline wax, 0.5-1 parts of alkylphenolic tackifying resin and 1.2-2.4 parts of silicon dioxide fiber.
4. The agricultural radial rubber tire tread rubber according to claim 3, Features: The preparation method of the nano silicon dioxide fiber is as follows: Adding nano silicon powder into a mixture of ethanol and distilled water, and uniformly dispersing by ultrasonication to obtain a dispersion; The polycarbonate is dissolved to obtain a matrix solution with a concentration of 8-10 wt%, and the dispersion liquid is added and stirred evenly to obtain a spinning solution, and electrospinning is performed to obtain a fiber membrane, wherein the mass ratio of nano silicon powder to polycarbonate is 1:8-10; The fiber membrane is kept at 300-330° C. for 6-7 hours, then heated to 800-820° C., calcined for 0.5-1 hour, cooled to room temperature, and ball-milled to obtain nano-silica fibers with a length of 100-150 μm.
5. The agricultural radial rubber tire tread rubber according to claim 4, Features: The silica fiber is pretreated as follows: The polyborosiloxane and isopropanol are mixed in a mass ratio of 5:1-2 to obtain a composite liquid, and 0.5-1wt% of glass fiber powder is added to the composite liquid, and ultrasonically homogenized to obtain a treatment liquid; The silica fiber is immersed in the treatment solution for 10-12 hours, filtered, and dried at 100-120° C. for 8-10 hours to obtain an intermediate; The intermediate is mixed with zinc sulfate solution, sodium carbonate solution and hexadecyltrimethylammonium bromide are added, the temperature is raised to 60-70°C, stirred for 20-24 hours, filtered, and calcined at 400-600°C for 3-4 hours, and the mass ratio of the intermediate, zinc sulfate solution, sodium carbonate solution and hexadecyltrimethylammonium bromide is 1-2:10:10:0.1-0.
2.
6. The agricultural radial rubber tire tread rubber according to claim 5, Features: The polyborosiloxane is prepared by mixing terminal hydroxyl polydimethylsiloxane with a hydroxyl mass fraction of 2.5% and boric acid in a molecular molar ratio of 1:
1.
7. The agricultural radial rubber tire tread rubber according to claim 5, Features: The particle size of the glass fiber powder is 50-100 nm.
8. The agricultural radial rubber tire tread rubber according to claim 1, Features: The filler is modified carbon black, and the modified carbon black is prepared by the following method: By weight, 3-3.5 parts of carbon black and 3-3.5 parts of fly ash are mixed, and surface treated with 0.06-0.07 parts of silane coupling agent to prepare a pretreated material; 10-11 parts of EVA resin are melted at 120-125° C., the pretreated material, 0.3-0.7 parts of azodicarbonamide and 0.2-0.4 parts of diisopropylbenzene peroxide are added, kneaded for 30-40 minutes, hot pressed for 8-10 minutes and cold pressed for 4-5 minutes at 130-140° C. and 8-10 MPa, and crushed into 2-5 mm particles.
9. The agricultural radial rubber tire tread rubber according to claim 1, Features: The antioxidant includes antioxidant RD and antioxidant 4020 in a mass ratio of 1.5:2.5-3.5; The softening oil is selected from at least one of aromatic oil, naphthenic oil and paraffin oil; The lubricant is selected from at least one of stearic acid, paraffin oil and silicone oil; The scorch retarder is selected from at least one of N-cyclohexylthiophthalimide and N,N-dibenzhydryl-1,6-hexanediisocyanate; The accelerator is selected from at least one of accelerator DM, accelerator NS and accelerator TMTD; The vulcanizing agent is selected from at least one of sulfur, benzoyl peroxide or sulfur monochloride; The anti-reversion agent is anti-reversion agent WK-901 or PK-900.
10. A process for preparing the agricultural radial rubber tire tread rubber according to any one of claims 1 to 9, Features: The following steps are involved: Mixing cigarette sheet rubber, butadiene rubber, filler, softening oil, zinc oxide, lubricant, protective wax, antioxidant, DCPD resin and anti-reversion agent, and performing rubber removal at 155-165° C. to obtain a masterbatch; The master rubber is mixed with a vulcanizing agent, an accelerator and a scorch retarder, and kneaded, and discharged at 95-105° C. to obtain a tread rubber.