Epitaxial wafer for Micro-LED and preparation method thereof, Micro-LED

By designing an alternating laminate structure of multiple quantum well layers and hole injection enhancement layers in the epitaxial sheet of Micro-LED, the proportion of In components and layer thickness are optimized, and the problem of low light efficiency of Micro-LED at low current density is solved. , achieving higher luminous efficiency and yield.

CN118782700BActive Publication Date: 2024-11-22JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411267783.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

Micro-LED has low light efficiency at low current density, and the existing technology has failed to effectively improve its efficiency.

Method used

An epitaxial sheet for Micro-LED is designed, which includes a substrate, a buffer layer, an N-type GaN layer, an active layer and a P-type GaN layer, in which a multi-quantum well layer and hole injection enhancement are laminated. The layer is optimized by alternately stacking InxGa1-xN, InyGa1-yN, InαGa1-αN and AlγInβGa1-γ-βN layer structures to reduce mismatch stress and improve lattice quality.

Benefits of technology

It effectively improves the light efficiency and yield of Micro-LED at low operating current density, improves hole injection efficiency, and avoids the problem of decreased light efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782700B_ABST
    Figure CN118782700B_ABST
Patent Text Reader

Abstract

The present invention discloses an epitaxial wafer for Micro-LED and a preparation method thereof, and Micro-LED, which relate to the field of semiconductor optoelectronic devices. The epitaxial wafer includes a substrate, a buffer layer, an N-type GaN layer, an active layer, and a P-type GaN layer in sequence; the active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer, and a third multi-quantum well layer in sequence; the first multi-quantum well layer includes alternately stacked In x Ga 1‑x N layer and the first GaN layer, the second multi-quantum well layer includes alternately stacked In y Ga 1‑y N layer and the second GaN layer, the first hole injection enhancement layer includes alternately stacked In α Ga 1‑α N layer and Al γ In β Ga 1‑γ‑β N layer, the second hole injection enhancement layer includes alternately stacked In δ Ga 1‑δ N layer and the third GaN layer, the third multi-quantum well layer includes alternately stacked In z Ga 1‑z N layer and the fourth GaN layer; 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.01. The implementation of the present invention can improve the light efficiency of Micro-LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor optoelectronic devices, and in particular to an epitaxial wafer for Micro-LED and a preparation method thereof, and Micro-LED. Background Art

[0002] With the booming development of emerging wearable and portable technologies, micron-sized LED chips (Micro-LED) have received great attention and research from scientific research institutions and enterprises due to their application prospects in display, visible light communication, biomedicine and other fields. In addition, Micro LED display has excellent performance such as nanosecond (ns) level high-speed response performance, stable characteristics of inorganic materials, high light efficiency, high reliability, high color purity and contrast, and transparency. The combination of these characteristics is unattainable by liquid crystal display (LCD) and organic LED (OLED).

[0003] Although Micro-LED has many excellent properties, it also faces challenges in manufacturing technology and material device physics. For example, the problem of the decrease in device peak EQE and the corresponding increase in current density as the chip size decreases has not been completely solved. The efficiency of Micro-LED with an operating current density in the range of 0.01~0.5A / cm² is still obviously insufficient. In fact, even conventional-sized chips for general lighting and backlight display applications have relatively low efficiency at this current density. The reason is that in order to balance efficiency and cost factors, the operating current density of conventional-sized chips is 20A / cm². 2 Up to 40A / cm 2 The goal of the corresponding epitaxial structure design and material growth is to improve the efficiency under high current density, and its peak EQE is usually in the current density range of 1~4A / cm², without paying attention to the device efficiency under low current density. Under different current densities, the dominant reasons for the light-emitting mechanism of LED devices are different, and the corresponding epitaxial layer structure should also change. For example, at a small current density of 0.01~0.5A / cm² in the Micro LED working range, the carrier concentration in the quantum well is relatively low, the proportion of Auger recombination is small, and the corresponding quantum well recombination volume can be reduced, which means that the number of quantum wells can be reduced, the number of defects can be reduced, and the EQE of the device under low current density can be improved. Therefore, in-depth mechanism research, design and growth of LED epitaxial layer structure under low current density working conditions of Micro-LED is a necessary key technology for the research and development of high-efficiency Micro-LED devices driven by low working current density. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an epitaxial wafer for Micro-LED and a preparation method thereof, which has high luminous efficiency at low current density.

[0005] Another technical problem to be solved by the present invention is to provide a Micro-LED having high luminous efficiency at low current density.

[0006] In order to solve the above problems, the present invention discloses an epitaxial wafer for Micro-LED, which comprises a substrate, a buffer layer, an N-type GaN layer, an active layer and a P-type GaN layer sequentially stacked on the substrate;

[0007] The active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer and a third multi-quantum well layer sequentially stacked on the N-type GaN layer;

[0008] The first multi-quantum well layer includes alternately stacked In x Ga 1-x N layer and a first GaN layer, the second multi-quantum well layer includes alternately stacked In y Ga 1-y N layer and a second GaN layer, the first hole injection enhancement layer includes alternately stacked In α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layer, the second hole injection enhancement layer includes alternately stacked In δ Ga 1-δ N layer and a third GaN layer, wherein the third multi-quantum well layer includes alternately stacked In z Ga 1-z N layer and a fourth GaN layer;

[0009] Among them, 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.01.

[0010] As an improvement of the above technical solution, the period number of the first multi-quantum well layer is 2-6, the value range of x is 0.12-0.21, and the In x Ga 1-x The thickness of the N layer is 2.1 nm to 4.2 nm, and the thickness of the first GaN layer is 8 nm to 16 nm; and / or

[0011] The period number of the second multi-quantum well layer is 3 to 8, the value range of y is 0.22 to 0.28, and the In y Ga 1-y The thickness of the N layer is 2.5 nm to 4.8 nm, and the thickness of the second GaN layer is 7 nm to 13.8 nm; and / or

[0012] The period number of the third multi-quantum well layer is 1 to 3, the value range of z is 0.12 to 0.21, and the In z Ga 1-z The thickness of the N layer is 2.1 nm to 4.2 nm, and the thickness of the fourth GaN layer is 6 nm to 12.6 nm.

[0013] As an improvement of the above technical solution, the number of periods of the first hole injection enhancement layer is 2 to 5, the value range of α is 0.01 to 0.08, and the In α Ga 1-α The thickness of the N layer is 0.5nm~2.5nm; the value range of γ is 0.03~0.3, the value range of β is 0.01~0.08, and the Al γ In β Ga 1-γ-β The thickness of the N layer is 0.8 nm to 3 nm; and / or

[0014] The period number of the second hole injection enhancement layer is 2-10, the value range of δ is 0.02-0.1, and the In δ Ga 1-δ The thickness of the N layer is 0.5nm-2.5nm, and the thickness of the third GaN layer is 0.8nm-3nm.

[0015] As an improvement of the above technical solution, the first GaN layer is doped with Si, and the doping concentration is 1.8×10 17 cm -3 ~7.6×10 18 cm -3 ; and / or

[0016] The second GaN layer is doped with Si, and the doping concentration is 1.2×10 17 cm -3 ~7.5×10 17 cm -3 ; and / or

[0017] The fourth GaN layer is an unintentionally doped GaN layer; and / or

[0018] In x Ga 1-x N layer, the In y Ga 1-y The N layers are all unintentionally doped; and / or

[0019] In z Ga 1-z The N layer is doped with Mg at a concentration of 5×10 18 cm -3 ~7.6×10 19 cm-3 .

[0020] As an improvement of the above technical solution, the thickness of the first GaN layer is greater than the thickness of the second GaN layer, and the thickness of the second GaN layer is greater than the thickness of the fourth GaN layer.

[0021] As an improvement of the above technical solution, the In δ Ga 1-δ The N layer is doped with Mg, and its doping concentration is 3.6×10 18 cm -3 ~5.2×10 19 cm -3 , the third GaN layer is an unintentionally doped GaN layer; and / or

[0022] In α Ga 1-α N layer and Al γ In β Ga 1-γ-β The N layers are all unintentionally doped structures.

[0023] Correspondingly, the present invention also discloses a method for preparing an epitaxial wafer for Micro-LED, which is used to prepare the above-mentioned epitaxial wafer for Micro-LED, and comprises:

[0024] Providing a substrate, and sequentially growing a buffer layer, an N-type GaN layer, an active layer, and a P-type GaN layer on the substrate;

[0025] The active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer and a third multi-quantum well layer sequentially stacked on the N-type GaN layer;

[0026] The first multi-quantum well layer includes alternately stacked In x Ga 1-x N layer and a first GaN layer, the second multi-quantum well layer includes alternately stacked In y Ga 1-y N layer and a second GaN layer, the first hole injection enhancement layer includes alternately stacked In α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layer, the second hole injection enhancement layer includes alternately stacked In δ Ga 1-δ N layer and a third GaN layer, wherein the third multi-quantum well layer includes alternately stacked In z Ga 1-z N layer and a fourth GaN layer;

[0027] Among them, 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.01.

[0028] As an improvement of the above technical solution, the In x Ga 1-x The growth temperature of the N layer is 750°C to 900°C and the growth pressure is 50 torr to 300 torr; and / or

[0029] The growth temperature of the first GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr; and / or

[0030] In y Ga 1-y The growth temperature of the N layer is 706°C to 890°C, and the growth pressure is 50 torr to 300 torr; and / or

[0031] The growth temperature of the second GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr; and / or

[0032] In α Ga 1-α The growth temperature of the N layer is 780°C to 890°C and the growth pressure is 50 torr to 300 torr; and / or

[0033] The Al γ In β Ga 1-γ-β The growth temperature of the N layer is 780°C to 890°C and the growth pressure is 50 torr to 300 torr; and / or

[0034] In δ Ga 1-δ The growth temperature of the N layer is 780°C to 890°C and the growth pressure is 50 torr to 300 torr; and / or

[0035] The growth temperature of the third GaN layer is 780° C. to 890° C., and the growth pressure is 50 torr to 300 torr; and / or

[0036] In z Ga 1-z The growth temperature of the N layer is 750°C to 900°C and the growth pressure is 50 torr to 300 torr; and / or

[0037] The growth temperature of the fourth GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr.

[0038] As an improvement of the above technical solution, the In z Ga 1-z The growth temperature of the N layer is greater than that of the In x Ga 1-x The growth temperature of the N layer, the In x Ga 1-x The growth temperature of the N layer is greater than that of the In y Ga 1-y Growth temperature of the N layer.

[0039] Correspondingly, the present invention also discloses a Micro-LED, which includes the above-mentioned epitaxial wafer for Micro-LED.

[0040] The implementation of the present invention has the following beneficial effects:

[0041] 1. In an epitaxial wafer for Micro-LED in one embodiment of the present invention, the active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer and a third multi-quantum well layer stacked in sequence; wherein the first multi-quantum well layer includes In x Ga 1-x N layer and the first GaN layer, the second multi-quantum well layer includes alternately stacked In y Ga 1-y N layer and the second GaN layer, the first hole injection enhancement layer includes alternately stacked In α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layer, the second hole injection enhancement layer includes alternately stacked In δ Ga 1-δ N layer and the third GaN layer, the third multi-quantum well layer includes alternately stacked In z Ga 1-z N layer and the fourth GaN layer; wherein 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.01. In this embodiment, a multi-quantum well structure in which the In component first increases and then decreases is constructed in the active layer, which effectively reduces the mismatch stress, improves the lattice quality of the active layer, improves the light efficiency of the Micro-LED at low operating current density, and also improves its yield. In addition, the first hole injection enhancement layer (In α Ga 1-α N / A γ In β Ga 1-γ-β N), the second hole injection enhancement layer (In δ Ga 1-δN / GaN) can improve the hole injection efficiency and avoid the problem of reduced light efficiency due to lack of holes in the active layer close to the N-type GaN layer. In summary, the light efficiency of Micro-LED at low current density is effectively improved.

[0042] 2. In one embodiment of the present invention, the thickness of the first GaN layer is greater than that of the second GaN layer, and the thickness of the second GaN layer is greater than that of the fourth GaN layer, that is, the barrier layer adopts a decreasing structure. Based on this structural design, holes can be more easily injected into the first multi-quantum well layer and the second multi-quantum well layer arranged close to the N-type GaN layer, thereby compounding the light emission and improving the light efficiency.

[0043] 3. In one embodiment of the present invention δ Ga 1-δ N-layer, In z Ga 1-z The N layer is doped with Mg, which can provide more holes at a low current density and improve the light efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is a schematic structural diagram of an epitaxial wafer for Micro-LED in one embodiment of the present invention;

[0045] Figure 2 It is a flow chart of a method for preparing an epitaxial wafer for Micro-LED in one embodiment of the present invention. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0047] refer to Figure 1 An embodiment of the present invention discloses an epitaxial wafer for Micro-LED, which includes a substrate 100, a buffer layer 200, an N-type GaN layer 300, an active layer 400 and a P-type GaN layer 500 sequentially stacked on the substrate 100. The active layer 400 includes a first multi-quantum well layer 410, a second multi-quantum well layer 420, a first hole injection enhancement layer 430, a second hole injection enhancement layer 440 and a third multi-quantum well layer 450 sequentially stacked on the N-type GaN layer 300; the first multi-quantum well layer 410 includes In x Ga 1-x The N layer 411 and the first GaN layer 412, the second multi-quantum well layer 420 includes In y Ga 1-y The N layer 421 and the second GaN layer 422, the first hole injection enhancement layer 430 include In α Ga 1-α N layer 431 and Alγ In β Ga 1-γ-β The N layer 432 and the second hole injection enhancement layer 440 include In δ Ga 1-δ The N layer 441 and the third GaN layer 442, the third multi-quantum well layer 450 includes In z Ga 1-z N layer 451 and fourth GaN layer 452; 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.01. Based on the active layer 400 of this embodiment, on the one hand, the In in the first multi-quantum well layer 410 x Ga 1-x The In component ratio in the N layer 411 is less than that in the second multi-quantum well layer 420. y Ga 1-y The proportion of N layer 421, In in the third multi-quantum well layer 450 z Ga 1-z The In component ratio of the N layer 451 is less than that of the In in the second multi-quantum well layer 420. y Ga 1-y The proportion of the N layer 421 is increased, that is, a multi-quantum well structure in which the In component first increases and then decreases is constructed. This structural design can effectively reduce the lattice mismatch stress between the InGaN material and the barrier layer material in the active layer 400, improve the crystal quality of the active layer 400, and thus improve the radiation recombination efficiency of the active region; and, due to the corresponding relationship of the above-mentioned In component proportions, the In z Ga 1-z The lattice mismatch between the N layer 451 and the fourth GaN layer 452 is less than that between the In x Ga 1-x The mismatch between the N layer 411 and the first GaN layer is less than that between the In y Ga 1-y The lattice mismatch between the N layer 421 and the second GaN layer 422 greatly reduces the defects caused by mismatch stress, significantly improves the crystal quality of the active layer 400, improves the light efficiency of the Micro-LED at low operating current density, and also improves its yield. α Ga 1-α N / A γ In β Ga 1-γ-β N), the second hole injection enhancement layer 440 (In δ Ga 1-δN / GaN), which can improve the hole injection efficiency and avoid the problem of reduced light efficiency due to lack of holes in the active layer 400 close to the N-type GaN layer 300. In summary, the epitaxial wafer in this embodiment effectively improves the light efficiency of Micro-LED at a low current density.

[0048] The period number of the first multi-quantum well layer 410 is 1-7. If the period number is too small, it is difficult to effectively reduce the compressive stress in the second multi-quantum well layer 420. If the period number is too large, it will affect the main wavelength of light emission. Preferably, the period number of the first multi-quantum well layer 410 is 2-6.

[0049] Among them, x Ga 1-x The ratio of In component in N layer 411 (i.e., x) is 0.1-0.25, and is 0.12, 0.15, 0.18, 0.21 or 0.24, but not limited thereto. Preferably, it is 0.12-0.21. x Ga 1-x The thickness of the N layer 411 is 2 nm to 5 nm, and is exemplarily 2.5 nm, 3 nm, 3.5 nm, 4 nm or 4.5 nm, but is not limited thereto. x Ga 1-x The thickness of the N layer 411 is 2.1 nm to 4.2 nm.

[0050] The thickness of the first GaN layer 412 is 5 nm to 18 nm, and is exemplarily 6 nm, 8 nm, 11 nm, 14 nm or 17 nm, but is not limited thereto. Preferably, the thickness of the first GaN layer 412 is 8 nm to 16 nm.

[0051] The period number of the second multi-quantum well layer 420 is 3 to 10. In this embodiment, the second multi-quantum well layer 420 is a core light-emitting structure, and its period number is relatively large. y Ga 1-y The In component in the N layer 421 is relatively high, and the mismatch stress with the quantum barrier structure (the second GaN layer 422) is relatively large, which will produce a large compressive stress and reduce the light efficiency, so the number of periods should not be too many. Exemplarily, the number of periods of the second multi-quantum well layer 420 is 4, 6, 8 or 9, but is not limited thereto. Preferably, the number of periods of the second multi-quantum well layer 420 is 3 to 8.

[0052] Among them, y Ga 1-y The ratio of In component in N layer 421 (i.e., y) is 0.22-0.32, and is 0.25, 0.28, 0.3 or 0.31, but is not limited thereto. Preferably, it is 0.22-0.28. y Ga1-y The thickness of the N layer 421 is 2nm-5nm, and is exemplarily 2.4nm, 2.8nm, 3.2nm, 3.8nm, 4.4nm or 4.9nm, preferably 2.5nm-4.8nm. Since the In component accounts for a large proportion and the stress accumulation is high, in order to improve the crystal quality, the thickness needs to be relatively large.

[0053] The thickness of the second GaN layer 422 is 7 nm to 15 nm. The thinner second GaN layer 422 can reduce the barrier to hole carriers, making it easier for them to enter the In y Ga 1-y The N layer 421 emits light in combination. Exemplarily, the thickness of the second GaN layer 422 is 7.5 nm, 9 nm, 10.5 nm, 13 nm or 14.5 nm, but is not limited thereto. Preferably, the thickness is 7 nm to 13.8 nm.

[0054] The number of periods of the first hole injection enhancement layer 430 is 2-5, and is exemplarily 3, 4 or 5, but is not limited thereto.

[0055] Among them, α Ga 1-α The ratio of In component in N layer 431 (i.e., α) is 0.01-0.1, and is 0.02, 0.04, 0.06 or 0.08, but is not limited thereto. Preferably, it is 0.01-0.08. α Ga 1-α The thickness of the N layer 431 is 0.5 nm to 4 nm, and is exemplarily 0.8 nm, 1.4 nm, 2 nm, 2.6 nm, 3.2 nm or 3.8 nm, but is not limited thereto, and is preferably 0.5 nm to 2.5 nm.

[0056] Among them, Al γ In β Ga 1-γ-β The ratio of In component in N layer 432 (i.e., β) is 0.01-0.1, and is 0.02, 0.04, 0.06 or 0.08, but is not limited thereto. Preferably, it is 0.01-0.08. γ In β Ga 1-γ-β The thickness of the N layer 432 is 0.5 nm to 4 nm, and is exemplarily 0.8 nm, 1.4 nm, 2 nm, 2.6 nm, 3.2 nm or 3.8 nm, but is not limited thereto, and is preferably 0.8 nm to 3 nm.

[0057] The number of periods of the second hole injection enhancement layer 440 is 2-10, and is exemplarily 3, 5, 7 or 9, but is not limited thereto.

[0058] Among them,δ Ga 1-δ The ratio of In component in N layer 441 (ie, δ) is 0.02-0.15, and is 0.03, 0.07, 0.11 or 0.14, but is not limited thereto. Preferably, it is 0.02-0.1. δ Ga 1-δ The thickness of the N layer 441 is 0.5 nm to 3 nm, and is exemplarily 0.8 nm, 1.2 nm, 1.6 nm, 2 nm, 2.5 nm or 2.9 nm, but is not limited thereto, and is preferably 0.5 nm to 2.5 nm.

[0059] The thickness of the third GaN layer 442 is 0.5 nm to 5 nm, and is exemplarily 0.8 nm, 1.4 nm, 2 nm, 3 nm, 4 nm or 4.5 nm, but is not limited thereto, and is preferably 0.8 nm to 3 nm.

[0060] The number of periods of the third multi-quantum well layer 450 is 1-5, exemplarily 2, 3, 4 or 5, but not limited thereto, and preferably 1-3.

[0061] Among them, z Ga 1-z The ratio of In component in N layer 451 (i.e., z) is 0.1-0.25, and is 0.11, 0.13, 0.17, 0.19, 0.21 or 0.23, but is not limited thereto. Preferably, it is 0.12-0.21. z Ga 1-z The thickness of the N layer 451 is 2 nm to 5 nm, exemplarily 2.2 nm, 3 nm, 4 nm or 4.5 nm, but not limited thereto, preferably 2.1 nm to 4.2 nm.

[0062] The thickness of the fourth GaN layer 452 is 6 nm to 15 nm, exemplarily 7 nm, 8 nm, 10 nm, 11 nm, 13 nm or 14 nm, but not limited thereto, preferably 6 nm to 12.6 nm.

[0063] The substrate 100 is a sapphire substrate, a silicon substrate or a SiC substrate, but is not limited thereto. A sapphire substrate is preferred.

[0064] The buffer layer 200 may be an AlN layer or an AlGaN layer, but is not limited thereto. Preferably, it is an AlN layer. The thickness of the buffer layer 200 is 30 nm to 80 nm.

[0065] The N-type GaN layer 300 is a Si-doped GaN layer, and its Si doping concentration is 5×10 18 cm -3 ~5×10 19 cm -3, thickness is 1μm~3μm.

[0066] The P-type GaN layer 500 is a Mg-doped GaN layer, and its Mg doping concentration is 1×10 19 cm -3 ~1×10 21 cm -3 The thickness of the P-type GaN layer 500 is 150 nm to 300 nm.

[0067] Preferably, in one embodiment, the first GaN layer 412 is doped with Si, and the doping concentration is 1.8×10 17 cm -3 ~7.6×10 18 cm -3 Through this embodiment, the In content in the first multi-quantum well layer 410 can be increased. x Ga 1-x The interface quality of the N layer 411 and the first GaN layer 412 can reduce the fluctuation of the In component, and at the same time can shield the polarization electric field to a certain extent, thereby effectively improving the light efficiency. x Ga 1-x The N layer 411 is a non-doped structure. If it is doped with Mg, it will affect the efficiency of electron carriers entering the active layer 400 and reduce the light efficiency. If it is doped with Si, the mismatch between electrons and holes will be too high, which will also reduce the light efficiency.

[0068] Preferably, in one embodiment, the second GaN layer 422 is doped with Si, and the doping concentration is 1.2×10 17 cm -3 ~7.5×10 17 cm -3 Through this embodiment, the In in the second multi-quantum well layer 420 can be increased. y Ga 1-y The interface quality between the N layer 421 and the second GaN layer 422 can reduce the fluctuation of In composition and shield the polarization electric field to a certain extent, thereby effectively improving the light efficiency. y Ga 1-y The In component accounts for a high proportion in the N layer 421, so a lower doping concentration is used to prevent the expansion of In y Ga 1-y The lattice mismatch between the N layer 421 and the second GaN layer 422 further reduces the light efficiency. y Ga 1-y The N layer 421 is a non-doped structure. If it is doped with Mg, it will affect the efficiency of electron carriers entering the active layer 400 and reduce the light efficiency. If it is doped with Si, the mismatch between electrons and holes will be too high, which will also reduce the light efficiency.

[0069] Preferably, in one embodiment, In z Ga 1-z The N layer 451 is doped with Mg at a concentration of 5×10 18 cm -3 ~7.6×10 19 cm -3 Based on this embodiment, one, In z Ga 1-z The N layer 451 can deplete electrons and prevent them from entering the P-type GaN layer 500 to form non-radiative recombination and reduce the light efficiency. z Ga 1-z The N layer 451 itself can provide some holes, which can improve the light efficiency. Based on this embodiment, the fourth GaN layer 452 is an unintentionally doped GaN layer. If Si is doped into it, the probability of holes from the P-type GaN layer 500 entering the active layer 400 will be reduced, thereby reducing the light efficiency. If Mg is doped into it, the hole carrier dispersion will be too poor, thereby reducing the light efficiency.

[0070] Preferably, in one embodiment, the thickness of the first GaN layer 412 is greater than the thickness of the second GaN layer 422 and greater than the thickness of the fourth GaN layer 452. Based on this structure, holes can be more easily injected into the first multi-quantum well layer 410 and the second multi-quantum well layer 420 disposed near the N-type GaN layer 300, thereby compounding and emitting light, thereby improving light efficiency.

[0071] Preferably, in one embodiment, In δ Ga 1-δ The N layer 441 is doped with Mg, and the doping concentration is 3.6×10 18 cm -3 ~5.2×10 19 cm -3 Mg doping can provide holes and also store holes. Based on this embodiment, the third GaN layer 442 is an unintentionally doped GaN layer. α Ga 1-α N layer 431 and Al γ In β Ga 1-γ-β The N layer 432 is a non-intentionally doped structure.

[0072] Preferably, in one embodiment, the epitaxial wafer further includes a non-doped GaN layer 600 , which is disposed between the buffer layer 200 and the N-type GaN layer 300 , and has a thickness of 1 μm to 3 μm.

[0073] Preferably, in one embodiment, the epitaxial wafer further includes a P-type contact layer 700, which is a P-type InGaN layer or a heavily doped P-type GaN layer, preferably a P-type InGaN layer, wherein the In component ratio is 0.05-0.1, and the doping element is Mg, and the doping concentration is 1×10 20 cm -3 ~1×10 21 cm -3 , and its thickness is 5nm~20nm.

[0074] Accordingly, reference Figure 2 The present invention also discloses a method for preparing an epitaxial wafer for Micro-LED, which is used to prepare the above-mentioned epitaxial wafer for Micro-LED, and comprises:

[0075] S1: providing a substrate;

[0076] S2: sequentially growing a buffer layer, an N-type GaN layer, a multi-quantum well layer and a P-type GaN layer on the substrate;

[0077] Specifically, step S2 includes:

[0078] S21: growing a buffer layer on the substrate;

[0079] Specifically, in one embodiment, an AlN layer may be grown by PVD or MOCVD as a buffer layer, but is not limited thereto.

[0080] S22: growing a non-doped GaN layer on the buffer layer;

[0081] Specifically, in one embodiment, the non-doped GaN layer is grown by MOCVD, the growth temperature is 1000° C. to 1200° C., and the growth pressure is 100 torr to 500 torr.

[0082] S23: growing an N-type GaN layer on the non-doped GaN layer;

[0083] Specifically, in one embodiment, the N-type GaN layer is grown by MOCVD, the growth temperature is 1000° C. to 1200° C., and the growth pressure is 100 torr to 500 torr.

[0084] S24: growing an active layer on the N-type GaN layer;

[0085] In one embodiment, step S24 includes:

[0086] S241: growing a first multi-quantum well layer on the N-type GaN layer;

[0087] Specifically, in one embodiment, In is periodically grown by MOCVD. xGa 1-x N layer and a first GaN layer until a first multi-quantum well layer is obtained.

[0088] Among them, x Ga 1-x The growth temperature of the N layer is 750°C~900°C, and the growth pressure is 50torr~300torr; the growth temperature of the first GaN layer is 830°C~920°C, and the growth pressure is 50torr~300torr.

[0089] S242: growing a second multi-quantum well layer on the first multi-quantum well layer;

[0090] Specifically, in one embodiment, In is periodically grown by MOCVD. y Ga 1-y N layer and a second GaN layer until a second multi-quantum well layer is obtained.

[0091] Among them, y Ga 1-y The growth temperature of the N layer is 706°C~890°C, and the growth pressure is 50torr~300torr; the growth temperature of the second GaN layer is 830°C~920°C, and the growth pressure is 50torr~300torr.

[0092] S243: growing a first hole injection enhancement layer on the second multi-quantum well layer;

[0093] Specifically, in one embodiment, In is periodically grown by MOCVD. α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layers are formed until the first hole injection enhancement layer is obtained.

[0094] Among them, α Ga 1-α The growth temperature of the N layer is 780℃~890℃, and the growth pressure is 50torr~300torr; Al γ In β Ga 1-γ-β The growth temperature of the N layer is 780℃~890℃, and the growth pressure is 50torr~300torr.

[0095] S244: growing a second hole injection enhancement layer on the first hole injection enhancement layer;

[0096] Specifically, in one embodiment, In is periodically grown by MOCVD. δ Ga 1-δN layer and the third GaN layer until a second hole injection enhancement layer is obtained.

[0097] Among them, δ Ga 1-δ The growth temperature of the N layer is 780°C~890°C, and the growth pressure is 50torr~300torr; the growth temperature of the third GaN layer is 780°C~890°C, and the growth pressure is 50torr~300torr.

[0098] S245: growing a third multi-quantum well layer on the second hole injection enhancement layer to obtain an active layer;

[0099] Specifically, in one embodiment, In is periodically grown by MOCVD. z Ga 1-z N layer and a fourth GaN layer until a third multi-quantum well layer is obtained.

[0100] Among them, z Ga 1-z The growth temperature of the N layer is 750°C~900°C, and the growth pressure is 50torr~300torr; the growth temperature of the fourth GaN layer is 830°C~920°C, and the growth pressure is 50torr~300torr.

[0101] S25: growing a P-type GaN layer on the active layer;

[0102] Specifically, in one embodiment, the P-type GaN layer is grown by MOCVD, the growth temperature is 900° C. to 1000° C., and the growth pressure is 100 torr to 500 torr.

[0103] S26: growing a P-type contact layer on the P-type GaN layer;

[0104] Specifically, in one embodiment, a P-type InGaN layer is grown by MOCVD as a P-type contact layer, and the growth temperature is 800° C. to 950° C. and the growth pressure is 100 torr to 500 torr.

[0105] Correspondingly, one embodiment of the present invention further discloses a Micro-LED, which includes the above-mentioned epitaxial wafer for Micro-LED.

[0106] The present invention will be further described below with specific embodiments:

[0107] Example 1

[0108] The present embodiment provides an epitaxial wafer for Micro-LED, which includes a substrate, a buffer layer, an undoped GaN layer, an N-type GaN layer, an active layer, a P-type GaN layer and a P-type contact layer stacked in sequence on the substrate.

[0109] The substrate is a sapphire substrate, the thickness of the non-doped GaN layer is 2 μm, and the Si doping concentration of the N-type GaN layer is 8×10 18 cm -3 , thickness is 2.5μm.

[0110] The active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer and a third multi-quantum well layer stacked in sequence on the N-type GaN layer; the first multi-quantum well layer includes In x Ga 1-x N layer and the first GaN layer, the period number of which is 3, In x Ga 1-x The thickness of the N layer (x=0.15) is 3nm, and the thickness of the first GaN layer is 10nm. The second multi-quantum well layer includes alternately stacked In y Ga 1-y N layer and the second GaN layer, the period number of which is 6, In y Ga 1-y The thickness of the N layer (y=0.25) is 4nm, and the thickness of the second GaN layer is 10nm. The first hole injection enhancement layer includes alternately stacked In α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layers, the number of cycles is 3, In α Ga 1-α The thickness of the N layer (α=0.05) is 1.5nm, and the Al γ In β Ga 1-γ-β The thickness of the N layer (γ = 0.15, β = 0.05) is 2.5 nm. The second hole injection enhancement layer includes alternately stacked In δ Ga 1-δ N layer and the third GaN layer, the period number of which is 8, In δ Ga 1-δ N layer (δ = 0.08). The third multi-quantum well layer includes alternately stacked In z Ga 1-z N layer and the fourth GaN layer, the period number of which is 2, In z Ga 1-z The thickness of the N layer (z=0.12) is 3 nm, and the thickness of the fourth GaN layer is 10 nm.

[0111] Among them, the Mg doping concentration in the P-type GaN layer is 5×10 19 cm -3 , with a thickness of 200nm. The P-type contact layer is a P-type InGaN layer, with an In component ratio of 0.08 and a Mg doping concentration of 3×10 20 cm -3 , thickness is 10nm.

[0112] The preparation method of the epitaxial wafer for Micro-LED in this embodiment is as follows:

[0113] (1) Providing a substrate;

[0114] (2) growing a buffer layer on the substrate;

[0115] Specifically, an AlN layer is grown by PVD to serve as a buffer layer.

[0116] (3) growing a non-doped GaN layer on the buffer layer;

[0117] Specifically, the non-doped GaN layer is grown by MOCVD, with a growth temperature of 1080° C. and a growth pressure of 300 torr.

[0118] (4) growing an N-type GaN layer on the undoped GaN layer;

[0119] Specifically, the N-type GaN layer is grown by MOCVD, with a growth temperature of 1100° C. and a growth pressure of 300 torr.

[0120] (5) growing a first multi-quantum well layer on the N-type GaN layer;

[0121] Specifically, In is periodically grown by MOCVD. x Ga 1-x N layer and the first GaN layer until the first multi-quantum well layer is obtained. x Ga 1-x The growth temperature of the N layer is 810° C. and the growth pressure is 200 torr; the growth temperature of the first GaN layer is 900° C. and the growth pressure is 200 torr.

[0122] (6) growing a second multi-quantum well layer on the first multi-quantum well layer;

[0123] Specifically, In is periodically grown by MOCVD. y Ga 1-y N layer and the second GaN layer until the second multi-quantum well layer is obtained. y Ga 1-yThe growth temperature of the N layer is 720° C. and the growth pressure is 200 torr; the growth temperature of the second GaN layer is 900° C. and the growth pressure is 200 torr.

[0124] (7) growing a first hole injection enhancement layer on the second multi-quantum well layer;

[0125] Specifically, In is periodically grown by MOCVD. α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layers are formed until the first hole injection enhancement layer is obtained. α Ga 1-α The growth temperature of the N layer is 830°C and the growth pressure is 200 torr; the Al γ In β Ga 1-γ-β The growth temperature of the N layer is 880°C and the growth pressure is 200 torr.

[0126] (8) growing a second hole injection enhancement layer on the first hole injection enhancement layer;

[0127] Specifically, In is periodically grown by MOCVD. δ Ga 1-δ N layer and the third GaN layer until the second hole injection enhancement layer is obtained. δ Ga 1-δ The growth temperature of the N layer is 820° C. and the growth pressure is 200 torr; the growth temperature of the third GaN layer is 880° C. and the growth pressure is 200 torr.

[0128] (9) growing a third multi-quantum well layer on the second hole injection enhancement layer to obtain an active layer;

[0129] Specifically, In is periodically grown by MOCVD. z Ga 1-z N layer and the fourth GaN layer until the third multi-quantum well layer is obtained. z Ga 1-z The growth temperature of the N layer is 815° C., and the growth pressure is 200 torr; the growth temperature of the fourth GaN layer is 900° C., and the growth pressure is 200 torr.

[0130] (10) Growing a P-type GaN layer on the active layer;

[0131] Specifically, the P-type GaN layer is grown by MOCVD, with a growth temperature of 950° C. and a growth pressure of 300 torr.

[0132] (11) Growing a P-type contact layer on the P-type GaN layer;

[0133] Specifically, a P-type InGaN layer is grown by MOCVD as a P-type contact layer, and the growth temperature is 850° C. and the growth pressure is 300 torr.

[0134] Example 2

[0135] This embodiment provides an epitaxial wafer for Micro-LED, which is different from Embodiment 1 in that:

[0136] The first GaN layer is doped with Si at a doping concentration of 3×10 18 cm -3 The second GaN layer is doped with Si at a concentration of 1.2×10 17 cm -3 ~7.5×10 17 cm -3 .

[0137] The rest are the same as in Example 1.

[0138] Example 3

[0139] This embodiment provides an epitaxial wafer for Micro-LED, which is different from Embodiment 2 in that:

[0140] The thickness of the first GaN layer is 12 nm, the thickness of the second GaN layer is 9 nm, and the thickness of the fourth GaN layer is 8 nm.

[0141] The rest are the same as in Example 2.

[0142] Example 4

[0143] This embodiment provides an epitaxial wafer for Micro-LED, which is different from Embodiment 3 in that:

[0144] In δ Ga 1-δ The N layer is doped with Mg, and its doping concentration is 4.8×10 18 cm -3 ,In z Ga 1-z The N layer is doped with Mg at a concentration of 3.3×10 19 cm -3 .

[0145] The rest is the same as Example 3.

[0146] Comparative Example 1

[0147] This comparative example provides an epitaxial wafer for Micro-LED, which differs from Example 1 in that:

[0148] The active layer only includes the second multi-quantum well layer, and the number of its periods is 10. The first multi-quantum well layer, the first hole injection enhancement layer, the second hole injection enhancement layer and the third multi-quantum well layer are not included. Accordingly, the preparation method also does not include the steps of preparing the first multi-quantum well layer, the first hole injection enhancement layer, the second hole injection enhancement layer and the third multi-quantum well layer.

[0149] The rest are the same as in Example 1.

[0150] Comparative Example 2

[0151] This comparative example provides an epitaxial wafer for Micro-LED, which differs from Example 1 in that:

[0152] The active layer only includes the second multi-quantum well layer, the first hole injection enhancement layer and the second hole injection enhancement layer sequentially stacked on the N-type GaN layer. The first multi-quantum well layer and the third multi-quantum well layer are not included. Accordingly, the preparation method does not include the steps of preparing the first multi-quantum well layer and the third multi-quantum well layer.

[0153] The rest are the same as in Example 1.

[0154] Comparative Example 3

[0155] This comparative example provides an epitaxial wafer for Micro-LED, which differs from Example 1 in that:

[0156] The active layer only includes the first multi-quantum well layer, the second multi-quantum well layer and the third multi-quantum well layer sequentially stacked on the N-type GaN layer, but does not include the first hole injection enhancement layer and the second hole injection enhancement layer. Accordingly, the preparation method does not include the steps of preparing the first hole injection enhancement layer and the second hole injection enhancement layer.

[0157] The rest are the same as in Example 1.

[0158] The epitaxial wafers of Examples 1 to 4 and Comparative Examples 1 to 3 were made into Micro-LEDs, and their luminous brightness was tested under the condition of a current density of 0.2A / cm². The luminous brightness improvement rate was calculated based on the data of Comparative Example 1, and the specific results are shown in the following table:

[0159]

[0160] It can be seen from the table that when the active layer in the embodiment of the present invention is used, the luminous brightness of the Micro-LED at a low current density can be effectively improved.

[0161] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. An epitaxial wafer for Micro-LED, characterized in that: It comprises a substrate, a buffer layer, an N-type GaN layer, an active layer and a P-type GaN layer sequentially stacked on the substrate; The active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer and a third multi-quantum well layer sequentially stacked on the N-type GaN layer; The first multi-quantum well layer includes alternately stacked In x Ga 1-x N layer and a first GaN layer, the second multi-quantum well layer includes alternately stacked In y Ga 1-y N layer and a second GaN layer, the first hole injection enhancement layer includes alternately stacked In α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layer, the second hole injection enhancement layer includes alternately stacked In δ Ga 1-δ N layer and a third GaN layer, wherein the third multi-quantum well layer includes alternately stacked In z Ga 1-z N layer and a fourth GaN layer; Among them, 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.

01.

2. The epitaxial wafer for Micro-LED according to claim 1, characterized in that: The period number of the first multi-quantum well layer is 2 to 6, the value range of x is 0.12 to 0.21, and the In x Ga 1-x The thickness of the N layer is 2.1 nm to 4.2 nm, and the thickness of the first GaN layer is 8 nm to 16 nm; and / or The period number of the second multi-quantum well layer is 3 to 8, the value range of y is 0.22 to 0.28, and the In y Ga 1-y The thickness of the N layer is 2.5 nm to 4.8 nm, and the thickness of the second GaN layer is 7 nm to 13.8 nm; and / or The period number of the third multi-quantum well layer is 1 to 3, the value range of z is 0.12 to 0.21, and the In z Ga 1-z The thickness of the N layer is 2.1 nm to 4.2 nm, and the thickness of the fourth GaN layer is 6 nm to 12.6 nm.

3. The epitaxial wafer for Micro-LED according to claim 1, characterized in that: The number of cycles of the first hole injection enhancement layer is 2 to 5, the value range of α is 0.01 to 0.08, and the In α Ga 1-α The thickness of the N layer is 0.5nm~2.5nm; the value range of γ is 0.03~0.3, the value range of β is 0.01~0.08, and the Al γ In β Ga 1-γ-β The thickness of the N layer is 0.8nm~3nm; and / or The period number of the second hole injection enhancement layer is 2-10, the value range of δ is 0.02-0.1, and the In δ Ga 1-δ The thickness of the N layer is 0.5nm-2.5nm, and the thickness of the third GaN layer is 0.8nm-3nm.

4. The epitaxial wafer for Micro-LED according to any one of claims 1 to 3, characterized in that: The first GaN layer is doped with Si, and the doping concentration is 1.8×10 17 cm -3 ~7.6×10 18 cm -3 ; and / or The second GaN layer is doped with Si, and the doping concentration is 1.2×10 17 cm -3 ~7.5×10 17 cm -3 ; and / or The fourth GaN layer is an unintentionally doped GaN layer; and / or In x Ga 1-x N layer, the In y Ga 1-y The N layers are all unintentionally doped; and / or In z Ga 1-z The N layer is doped with Mg at a concentration of 5×10 18 cm -3 ~7.6×10 19 cm -3 .

5. The epitaxial wafer for Micro-LED according to any one of claims 1 to 3, characterized in that: The thickness of the first GaN layer is greater than that of the second GaN layer, and the thickness of the second GaN layer is greater than that of the fourth GaN layer.

6. The epitaxial wafer for Micro-LED according to any one of claims 1 to 3, characterized in that: In δ Ga 1-δ The N layer is doped with Mg, and its doping concentration is 3.6×10 18 cm -3 ~5.2×10 19 cm -3 , the third GaN layer is an unintentionally doped GaN layer; and / or In α Ga 1-α N layer and Al γ In β Ga 1-γ-β The N layers are all unintentionally doped structures.

7. A method for preparing an epitaxial wafer for Micro-LED, for preparing the epitaxial wafer for Micro-LED as claimed in any one of claims 1 to 6, characterized in that: include: Providing a substrate, and sequentially growing a buffer layer, an N-type GaN layer, an active layer, and a P-type GaN layer on the substrate; The active layer includes a first multi-quantum well layer, a second multi-quantum well layer, a first hole injection enhancement layer, a second hole injection enhancement layer and a third multi-quantum well layer sequentially stacked on the N-type GaN layer; The first multi-quantum well layer includes alternately stacked In x Ga 1-x N layer and a first GaN layer, the second multi-quantum well layer includes alternately stacked In y Ga 1-y N layer and a second GaN layer, the first hole injection enhancement layer includes alternately stacked In α Ga 1-α N layer and Al γ In β Ga 1-γ-β N layer, the second hole injection enhancement layer includes alternately stacked In δ Ga 1-δ N layer and a third GaN layer, wherein the third multi-quantum well layer includes alternately stacked In z Ga 1-z N layer and a fourth GaN layer; Among them, 0.3≥y>x>z≥0.1, z>δ≥α≥β≥0.

01.

8. The method for preparing an epitaxial wafer for Micro-LED according to claim 7, characterized in that: In x Ga 1- x The growth temperature of the N layer is 750°C to 900°C and the growth pressure is 50 torr to 300 torr; and / or The growth temperature of the first GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr; and / or In y Ga 1-y The growth temperature of the N layer is 706°C to 890°C, and the growth pressure is 50 torr to 300 torr; and / or The growth temperature of the second GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr; and / or In α Ga 1-α The growth temperature of the N layer is 780°C to 890°C and the growth pressure is 50 torr to 300 torr; and / or The Al γ In β Ga 1-γ-β The growth temperature of the N layer is 780°C to 890°C and the growth pressure is 50 torr to 300 torr; and / or In δ Ga 1-δ The growth temperature of the N layer is 780°C to 890°C and the growth pressure is 50 torr to 300 torr; and / or The growth temperature of the third GaN layer is 780° C. to 890° C., and the growth pressure is 50 torr to 300 torr; and / or In z Ga 1-z The growth temperature of the N layer is 750°C to 900°C and the growth pressure is 50 torr to 300 torr; and / or The growth temperature of the fourth GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr.

9. The method for preparing an epitaxial wafer for Micro-LED according to claim 7, characterized in that: In z Ga 1-z The growth temperature of the N layer is greater than that of the In x Ga 1-x The growth temperature of the N layer, the In x Ga 1-x The growth temperature of the N layer is greater than that of the In y Ga 1-y Growth temperature of the N layer.

10. A Micro-LED, characterized in that: It comprises an epitaxial wafer for Micro-LED as described in any one of claims 1 to 6.