Solid electrolyte, battery and manufacturing method thereof

By setting a specific roughness on the surface of the solid electrolyte and combining it with polishing and etching technology, the capacity retention and life problems of traditional Li metal batteries during high-capacity operation are solved, and a solid-state battery with high charging rate and long life is achieved.

CN118782886APending Publication Date: 2024-10-15CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310376946.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional Li metal batteries have capacity retention and longevity issues when operating at high capacities, especially as charging rates increase.

Method used

Charging is improved by setting predetermined surface roughness on the first major surface (facing the anode) and the second major surface (facing the cathode) of the solid electrolyte to approximately 0.6 μm or less and approximately 1 μm or greater, respectively, in combination with polishing and etching techniques. rate and reduce interface resistance, increasing battery life and capacity retention.

Benefits of technology

It achieves high charging rate and long life of the battery, reduces the formation of dendrites, solves the safety problems of traditional batteries such as leakage and poor chemical stability, and improves the utilization rate and energy density of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782886A_ABST
    Figure CN118782886A_ABST
Patent Text Reader

Abstract

The invention relates to a solid electrolyte, a battery and a manufacturing method thereof. The battery includes a cathode, a solid electrolyte, and an anode. And a solid electrolyte having a first main surface facing the anode and a second main surface facing the cathode, the first main surface having a surface roughness Ra of 0.6 [mu] m or less, and the second main surface having a surface roughness Ra of 1 [mu] m or more. The battery may further include a liquid electrolyte between the second major surface and the anode. The method includes polishing the first major surface of the solid electrolyte to form a surface roughness Ra of 0.6 microns or less. The method includes polishing the second major surface of the solid electrolyte to form a surface roughness Ra of 1 micron or greater. The method may include heating a lithium-containing precursor to form a lithium-containing anode disposed on the first major surface. The method may include disposing a solid state electrolyte over the cathode with the second major surface facing the cathode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solid electrolyte, a battery and a method for manufacturing the same, and more particularly, to a battery including a solid electrolyte and a method for manufacturing the same. Background Art

[0002] Solid-state batteries (SSBs), such as SS lithium (Li) metal batteries based on inorganic solid electrolytes (SSEs) (e.g., garnet-type SSEs), have attracted much attention due to their high safety, improved energy density, high ionic conductivity, and stability to Li metal. However, conventional Li metal batteries often suffer from capacity retention and / or lifespan issues, especially when operated at higher capacities. Therefore, it is necessary to address these issues. Summary of the invention

[0003] The present disclosure provides a solid electrolyte, a battery and a method for manufacturing the same, comprising one or more surfaces of a solid electrolyte having a predetermined surface roughness Ra. The surface roughness Ra of the first main surface (e.g., facing the anode) of the solid electrolyte can be about 0.6 μm or less (e.g., about 0.1 μm to about 0.5 μm), which can increase the charging rate that the battery can withstand. The surface roughness of the second main surface (e.g., facing the cathode) of the solid electrolyte can be about 1 μm or greater (e.g., about 1.2 μm to about 3 μm), which can reduce the interfacial resistance of the battery. The low surface roughness Ra of the first main surface (e.g., about 0.6 μm or less or about 0.1 μm to about 0.5 μm) is further combined with the high surface roughness Ra of the second main surface (e.g., about 1 μm or greater or about 1.2 μm to about 3 μm), which can unexpectedly increase the life of the battery and / or the capacity retention rate of the battery, and is confirmed by the embodiments of this article. Without wishing to be bound by theory, it is believed that a low roughness of the first major surface (e.g., about 0.6 μm or less or about 0.1 μm to about 0.5 μm) increases the charging rate by providing a substantially uniform surface for the anode, which enables uniform contact with the anode, reduces current concentration on the surface, and / or reduces the formation of dendrites. Without wishing to be bound by theory, it is believed that a high roughness of the second major surface (e.g., about 1 μm or more or about 1.2 μm to about 3 μm) reduces the interface resistance by increasing the surface area of ​​the interface between the solid electrolyte and the liquid electrolyte.

[0004] The method of the present disclosure includes polishing the first main surface and / or the second main surface to achieve a predetermined surface roughness Ra. Polishing may include etching, mechanical polishing or a combination thereof. Without wishing to be bound by theory, etching for a short time (e.g., about 4 minutes or less) can reduce surface irregularities without increasing the surface roughness of the first main surface (e.g., by etching the grain boundaries of a solid electrolyte). Without wishing to be bound by theory, etching for a short time (e.g., about 4 minutes or less) can reduce surface irregularities without increasing the surface roughness of the first main surface (e.g., by etching the grain boundaries of a solid electrolyte). Without wishing to be bound by theory, etching for a longer period of time (e.g., about 7 minutes or more) can increase the surface roughness of the second main surface, such as by etching the grain boundaries of a solid electrolyte and / or leaching a portion of a solid electrolyte. An abrasive having a high mesh count (highgrit) (or a low median particle size, low median particle size) for mechanically polishing the first main surface can produce a low surface roughness of the first main surface.

[0005] The method and battery may include a lithium-containing anode. In one aspect, the lithium-containing anode may be a lithium alloy, which may increase the wettability of the lithium-containing material on the first major surface of the solid electrolyte, which enables the battery to withstand high charging rates even when the lithium alloy is heated at 300°C and above. In one aspect, the lithium-containing anode may consist essentially of lithium metal. The method of the present disclosure includes heating the lithium metal at a temperature of about 330°C or above, which may wet or otherwise conform the lithium metal to the first major surface, which unexpectedly increases the charging rate that the battery can withstand, as demonstrated in the embodiments herein, for example, by providing close and / or uniform contact between the lithium metal anode and the first major surface of the solid electrolyte.

[0006] Providing a solid electrolyte (e.g., in a solid-state battery) can address common safety issues, such as leakage, poor chemical stability, and flammability, which are common in batteries using liquid electrolytes. In addition, providing a solid electrolyte can also inhibit the shuttling of polysulfides from the cathode to the anode, resulting in improved electrode (e.g., anode, cathode) utilization and high discharge capacity and energy density. Providing a solid electrolyte can reduce the formation of dendrites (e.g., lithium dendrites), which otherwise cause battery failure. Providing an intermediate layer comprising a liquid electrolyte can wet the interface between the cathode and the solid electrolyte, thereby reducing the interfacial resistance therebetween, while minimizing the total amount of liquid electrolyte in the solid-state battery.

[0007] Some exemplary aspects of the present disclosure are described below, while it should be understood that any features of the various aspects may be used alone or in combination with each other.

[0008] Aspect 1. A battery comprising:

[0009] an anode containing lithium;

[0010] A solid electrolyte comprising a first major surface facing a lithium-containing anode and a second major surface opposite the first major surface, wherein the first major surface comprises a surface roughness Ra of about 0.6 micrometers or less and the second major surface comprises a surface roughness of about 1 micrometer or more;

[0011] a liquid electrolyte disposed on the second major surface of the solid electrolyte; and

[0012] A cathode is disposed over the second major surface of the solid electrolyte, with the liquid electrolyte located between the second major surface and the cathode.

[0013] Aspect 2. The battery according to aspect 1, wherein the surface roughness Ra of the first major surface is in the range of about 0.1 micrometer to about 0.5 micrometer.

[0014] Aspect 3. The battery of any of aspects 1-2, wherein the surface roughness Ra of the second major surface is in the range of about 1.2 microns to about 3 microns.

[0015] Aspect 4. The battery according to any one of aspects 1 to 3, wherein the interface resistance between the cathode and the lithium-containing anode is about 60 Ωcm at 25°C. 2 or smaller.

[0016] Aspect 5. The battery according to aspect 4, wherein the interface resistance is in the range of about 10Ωcm 2 to about 40Ωcm 2 .

[0017] Aspect 6. The battery of aspects 1-3, wherein the interfacial resistance of the battery is about 50% or less of the interfacial resistance of another battery that is identical to the battery except that the first major surface and the second major surface are interchanged.

[0018] Aspect 7. The battery according to any one of aspects 1 to 5, wherein the battery can withstand at least 10 cycles of 1.6 mA / cm 2 or greater charging current density up to 1 mAh / cm 2 The capacity is 0.5 mA / cm 2 The discharge rate is the discharge cycle, where the area is based on the surface area of ​​the lithium-containing anode.

[0019] Aspect 8. The battery according to aspect 7, wherein the battery can withstand at least 10 cycles of 2 mA / cm 2 The charging current density is charged to 1 mAh / cm2 capacity and cycled at a discharge rate of 0.5 mA / cm 2 of the battery.

[0020] Aspect 9. The battery according to any one of Aspects 7-8, wherein another battery identical to the battery except that the first major surface and the second major surface are interchanged cannot withstand 10 cycles of charging to 1 mAh / cm 2 at a charging current density of 1.25 mA / cm 2 capacity and cycled at a discharge rate of 0.5 mA / cm 2 of the battery.

[0021] Aspect 10. The battery according to any one of Aspects 1-6, wherein the battery has a cut-off voltage of 4.5 V and is cycled at a charging rate of 0.5 C and a discharge rate of 0.17 C at 60 °C to 3 mAh / cm 2 of the maximum capacity 60 times and includes a capacity retention rate of about 90% or higher, and the area is based on the surface area of the lithium-containing anode.

[0022] Aspect 11. The battery according to any one of Aspects 1-10, wherein the lithium-containing anode includes an alloy of lithium with at least one of magnesium, silver, or a combination thereof.

[0023] Aspect 12. The battery according to any one of Aspects 1-11, wherein the cathode includes at least one of the following: lithium cobaltite (LCO), lithium manganite spinel (LMO), lithium nickel cobalt aluminate (NCA), lithium nickel manganese cobalt oxide (NCM) (LiNi d Co e Mn 1-d-e O 2 , where 0 < d < 1, 0 < e < 1), lithium iron phosphate (LiFePO 4 )(LFP), lithium cobalt phosphate (LCP), lithium titanate, lithium niobium tungstate, lithium nickel manganate, and lithium titanium sulfide (LiTiS 2 ) or a combination thereof.

[0024] Aspect 13. The battery according to any one of Aspects 1-12, wherein the solid electrolyte contains lithium, lanthanum, zirconium, and oxygen.

[0025] Aspect 14. The battery according to any one of Aspects 1-13, wherein the solid electrolyte contains at least one of the following:

[0026] (i) Li 7-3a La 3 Zr 2 L a O12 , where L = Al, Ga or Fe and 0 <a<0.33;

[0027] (ii)Li 7 La 3-b Zr 2 M b O 12 , where M = Bi or Y and 0 <b<1;

[0028] (iii)Li 7-c La 3 (Zr 2-c ,N c ) 12 , where N = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 <c<1;

[0029] (iv) Protonated LLZO (e.g., H x Li 6.5-x La 3 Zr 1.5 I 0.5 O 12 , where I = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 < x < 4, or H x Li 6.25-x E 0.25 La 3 Zr 2 O 12 , where E = Al, Ga or Fe and 0 < x < 4); or

[0030] A combination of them.

[0031] Aspect 15. The battery of any one of aspects 1-14, wherein the thickness of the solid electrolyte between the first major surface and the second major surface is about 20 microns to about 300 microns, and the solid electrolyte comprises a sintered tape.

[0032] Aspect 16. The battery of any of aspects 1-14, wherein the thickness of the solid electrolyte between the first major surface and the second major surface ranges from about 500 microns to about 2 millimeters, and the solid electrolyte comprises a consolidated pellet.

[0033] Aspect 17. The battery of any one of aspects 1-16, wherein the ratio of the weight of the cathode to the cathode surface area of ​​the cathode is in the range of about 5 mg / cm 2 To about 50mg / cm 2 .

[0034] Aspect 18. The battery of any one of aspects 1-16, wherein the ratio of the volume of the liquid electrolyte to the area of ​​the cathode is in the range of about 5 μL / cm 2 to about 20 μL / cm 2 .

[0035] Aspect 19. A battery as described in any one of aspects 1-18, wherein the liquid electrolyte comprises a lithium salt in a solvent, the lithium salt comprising at least one of the following: lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium trifluoromethanesulfonate (LiSO 3 CF 3 )、LiC(SO 2 CF 3 ) 3 or a combination thereof.

[0036] Aspect 20. The battery of aspect 19, wherein the solvent comprises sulfolane, and the concentration of the lithium salt in the liquid electrolyte ranges from about 1 molar to about 3 molar.

[0037] Aspect 21. A method of forming a battery, comprising:

[0038] polishing the first major surface of the solid electrolyte to form a surface roughness Ra of about 0.6 micrometers or less;

[0039] polishing a second major surface of the solid electrolyte to form a surface roughness Ra of about 1 micrometer or more, the second major surface being opposite to the first major surface;

[0040] heating the lithium-containing precursor at a temperature of about 300° C. or greater to form a lithium-containing anode disposed on the first major surface; and

[0041] A solid electrolyte is disposed above the cathode with a second major surface of the solid electrolyte facing the cathode.

[0042] Aspect 22. The method of aspect 21, wherein heating the lithium-containing precursor comprises heating at a temperature of about 330° C. to about 400° C. for about 5 minutes to about 10 minutes.

[0043] Aspect 23. The method of aspect 22, wherein the lithium-containing anode consists essentially of lithium metal.

[0044] Aspect 24. The method of any one of aspects 21-22, wherein the lithium-containing anode comprises an alloy of lithium and at least one of magnesium, silver, or a combination thereof.

[0045] Aspect 25. The method of any of Aspects 21-24, wherein polishing the first major surface comprises mechanical polishing.

[0046] Aspect 26. The method of aspect 25, wherein the mechanical polishing comprises polishing with a grit size of about 1000 or greater.

[0047] Aspect 27. The method of any of Aspects 21-26, wherein polishing the second major surface comprises mechanical polishing with a mesh size of about 600 or less.

[0048] Aspect 28. The method of any of Aspects 21-24, wherein polishing the first major surface comprises etching in an acidic solution.

[0049] Aspect 29. The method of aspect 28, wherein the etching comprises contacting the first major surface with an acidic solution comprising an acidic solution having a concentration of about 0.1 molar to about 3 molar for about 4 minutes or less.

[0050] Aspect 30. The method of any one of aspects 21-26 and 28, wherein polishing the second major surface comprises etching in an acidic solution comprising a concentration of about 0.1 molar to about 3 molar for about 7 minutes to about 30 minutes.

[0051] Aspect 31. The method of any one of Aspects 21-30, further comprising disposing a liquid electrolyte on the cathode such that the liquid electrolyte is located between the cathode and the second major surface, the liquid electrolyte comprising a lithium-containing salt.

[0052] Aspect 32. The method of aspect 31, wherein the solvent comprises sulfolane, and the concentration of the lithium salt in the liquid electrolyte ranges from about 1 molar to about 3 molar.

[0053] Aspect 33. The method of any of Aspects 21-32, wherein the surface roughness Ra of the first major surface is in a range of about 0.1 micrometers to about 0.5 micrometers.

[0054] Aspect 34. The method of any of Aspects 21-33, wherein the surface roughness Ra of the second major surface is in a range of about 1.2 microns to about 3 microns.

[0055] Aspect 35. The method according to any one of aspects 21-34, wherein the interfacial resistance between the cathode and the lithium-containing anode at 25° C. is about 60 Ω cm 2 or smaller.

[0056] Aspect 36. The method as described in Aspects 21 - 34, wherein the interfacial resistance of the battery is about 50% or less of the interfacial resistance of another battery that is the same as the battery except that the first major surface and the second major surface are interchanged.

[0057] Aspect 37. The method as described in any one of Aspects 21 - 36, wherein the battery can withstand at least 10 cycles of charging to a capacity of 1 mAh / cm² at a charging current density of 1.6 mA / cm² or greater at 25°C and discharging at a discharging rate of 0.5 mA / cm², where the area is based on the surface area of the lithium-containing anode. 2 or greater and discharging at a discharging rate of 0.5 mA / cm² 2 to a capacity of 1 mAh / cm², 2 where the area is based on the surface area of the lithium-containing anode.

[0058] Aspect 38. The method as described in Aspect 37, wherein the battery can withstand at least 10 cycles of charging to a capacity of 1 mAh / cm² at a charging current density of 2 mA / cm² at 25°C and discharging at a discharging rate of 0.5 mA / cm². 2 and discharging at a discharging rate of 0.5 mA / cm² 2 to a capacity of 1 mAh / cm² 2 at 25°C.

[0059] Aspect 39. The method as described in any one of Aspects 37 - 38, wherein another battery that is the same as the battery except that the first major surface and the second major surface are interchanged cannot withstand 10 cycles of charging to a capacity of 1 mAh / cm² at a charging current density of 1.25 mA / cm² at 25°C and discharging at a discharging rate of 0.5 mA / cm². 2 and discharging at a discharging rate of 0.5 mA / cm² 2 to a capacity of 1 mAh / cm² 2 at 25°C.

[0060] Aspect 40. The method as described in any one of Aspects 21 - 36, wherein the battery has a capacity retention rate of 90% or higher after 60 cycles of charging at a cut-off voltage of 4.5 V and 60°C at a charging rate of 0.5 C and discharging at a discharging rate of 0.17 C to a maximum capacity of 3 mAh / cm², and the area is based on the surface area of the lithium-containing anode. 2 and the area is based on the surface area of the lithium-containing anode.

[0061] Aspect 41. The method as described in any one of Aspects 21 - 40, wherein the cathode comprises at least one of the following: lithium cobaltite (LCO), lithium manganite spinel (LMO), lithium nickel cobalt aluminate (NCA), lithium nickel manganese cobalt oxide (NCM) (LiNi d Co e Mn 1-d-e O 2 , where 0 < d < 1, 0 < e < 1), lithium iron phosphate (LiFePO 4) (LFP), lithium cobalt phosphate (LCP), lithium titanate, lithium niobate tungstate, lithium nickel manganate and lithium titanium sulfide (LiTiS 2 ) or a combination thereof.

[0062] Aspect 42. The method of any one of aspects 21-41, wherein the solid electrolyte comprises at least one of the following:

[0063] (i)Li 7-3a La 3 Zr 2 L a O 12 , where L = Al, Ga or Fe and 0 <a<0.33;

[0064] (ii)Li 7 La 3-b Zr 2 M b O 12 , where M = Bi or Y and 0 <b<1;

[0065] (iii)Li 7-c La 3 (Zr 2-c ,N c ) 12 , where N = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 <c<1;

[0066] (iv) Protonated LLZO (e.g., H x Li 6.5-x La 3 Zr 1.5 I 0.5 O 12 , where I = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 < x < 4, or H x Li 6.25-x E 0.25 La 3 Zr 2 O 12 , where E = Al, Ga or Fe and 0 < x < 4); or

[0067] A combination of them.

[0068] Aspect 43. The method of any of Aspects 21-42, wherein the thickness of the solid electrolyte between the first major surface and the second major surface ranges from about 20 microns to about 300 microns, and the solid electrolyte comprises a sintered tape.

[0069] Aspect 44. The method of any one of Aspects 21-42, wherein the thickness of the solid electrolyte between the first major surface and the second major surface is about 500 microns to about 2 millimeters, and the solid electrolyte comprises consolidated granules.

[0070] Aspect 45. The method of any one of aspects 21-44, wherein the ratio of the weight of the cathode to the cathode surface area of ​​the cathode is in the range of about 5 mg / cm 2 To about 50mg / cm 2 .

[0071] Aspect 46. The battery of any one of Aspects 21-44, wherein the ratio of the volume of the liquid electrolyte to the area of ​​the cathode is in the range of about 5 μL / cm 2 to about 20 μL / cm 2 .

[0072] Aspect 47. A solid electrolyte comprising

[0073] a body comprising a garnet-based material;

[0074] a first major surface of the body, the first major surface comprising a surface roughness Ra of about 0.6 microns or less; and

[0075] A second major surface of the body opposite the first major surface, the second major surface comprising a surface roughness Ra of about 1 micrometer or greater.

[0076] Aspect 48. The battery of aspect 47, wherein the surface roughness Ra of the first major surface ranges from about 0.1 micrometers to about 0.5 micrometers.

[0077] Aspect 49. The battery of any of Aspects 47-48, wherein the surface roughness Ra of the second major surface ranges from about 1.2 microns to about 3 microns.

[0078] Aspect 50. The battery of any of Aspects 47-49, wherein the thickness of the solid electrolyte between the first major surface and the second major surface is from about 20 microns to about 300 microns, and the solid electrolyte comprises a sintered tape.

[0079] Aspect 51. The battery of any of Aspects 47-50, wherein the thickness of the solid electrolyte between the first major surface and the second major surface ranges from about 500 microns to about 2 millimeters, and the solid electrolyte comprises consolidated granules.

[0080] Aspect 52. A method for treating a solid electrolyte:

[0081] polishing the first major surface of the solid electrolyte to form a surface roughness Ra of about 0.6 micrometers or less; and

[0082] A second main surface of the solid electrolyte is polished to form a surface roughness Ra of about 1 micrometer or more, the second main surface being opposite to the first main surface.

[0083] Aspect 53. The method of aspect 52, wherein polishing the first major surface comprises mechanical polishing.

[0084] Aspect 54. The method of aspect 53, wherein the mechanical polishing comprises polishing with a mesh size of about 1000 or greater.

[0085] Aspect 55. The method of any of Aspects 52-54, wherein polishing the second major surface comprises mechanical polishing with a mesh size of about 600 or less.

[0086] Aspect 56. The method of aspect 52, wherein polishing the first major surface comprises etching in an acidic solution.

[0087] Aspect 57. The method of aspect 56, wherein the etching comprises contacting the first major surface with an acidic solution comprising an acidic solution having a concentration of about 0.1 molar to about 3 molar for about 4 minutes or less.

[0088] Aspect 58. The method of any one of aspects 52-54 and 56, wherein polishing the second major surface comprises etching in an acidic solution comprising a concentration of about 0.1 molar to about 3 molar for about 7 minutes to about 30 minutes.

[0089] Aspect 59. The method of any one of aspects 52-58, wherein the solid electrolyte comprises at least one of the following:

[0090] (i)Li 7-3a La 3 Zr 2 L a O 12 , where L = Al, Ga or Fe and 0 <a<0.33;

[0091] (ii)Li 7 La 3-b Zr 2 M b O 12 , where M = Bi or Y and 0 <b<1;

[0092] (iii)Li 7-c La 3 (Zr 2-c ,N c )12 , where N = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 <c<1;

[0093] (iv) Protonated LLZO (e.g., H x Li 6.5-x La 3 Zr 1.5 I 0.5 O 12 , where I = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 < x < 4, or H x Li 6.25-x E 0.25 La 3 Zr 2 O 12 , where E = Al, Ga or Fe and 0 < x < 4); or

[0094] A combination of them.

[0095] Aspect 60. The method of any of Aspects 52-59, wherein the solid electrolyte between the first major surface and the second major surface has a thickness ranging from about 20 microns to about 300 microns, and the solid electrolyte comprises a sintered tape.

[0096] Aspect 61. The method of any of Aspects 52-59, wherein the thickness of the solid electrolyte between the first major surface and the second major surface is about 500 microns to about 2 millimeters, and the solid electrolyte comprises consolidated granules. BRIEF DESCRIPTION OF THE DRAWINGS

[0097] The above features and advantages and other features and advantages of aspects of the present disclosure may be better understood by reading the following detailed description with reference to the accompanying drawings, in which:

[0098] Figure 1 Schematically illustrates the general structure of a solid-state battery according to aspects of the present disclosure;

[0099] Figure 2 shows a simplified solid-state battery with a solid-state electrolyte according to aspects of the present disclosure;

[0100] Figure 3 Steps in an exemplary method including disposing a precursor on a solid electrolyte to form an anode are shown;

[0101] Figure 4 Steps in an exemplary method including heating a precursor and a solid electrolyte are shown;

[0102] Figure 5 Steps in an exemplary method including disposing a liquid electrolyte above a cathode are shown;

[0103] Figure 6 Steps in an exemplary method including disposing a solid-state electrolyte above a cathode are shown;

[0104] Figure 7 Steps in an exemplary method including etching a first major surface of a solid-state electrolyte are shown;

[0105] Figure 8 Steps in an exemplary method including etching a second major surface of a solid-state electrolyte are shown;

[0106] Fig. 9 Steps in an exemplary method including mechanically polishing a first major surface of a solid-state electrolyte are shown;

[0107] Fig.10 Steps in an exemplary method including mechanically polishing a second major surface of a solid-state electrolyte are shown;

[0108] Fig.11 Scanning electron microscope (SEM) images of Examples AD are schematically shown;

[0109] Fig.12 Nyquist plots of Example 1 and Comparative Examples AA-CC are shown;

[0110] Fig.13 Nyquist plots of Example 2 and Comparative Examples DD-FF are shown;

[0111] Fig.14 shows a capacity-voltage (CV) curve of Comparative Example AA;

[0112] Fig.15 The CV curve diagram of Example 1 is shown;

[0113] Fig.16 CV curve diagram of Comparative Example BB is shown;

[0114] Fig.17 shows the CV curve graph of Comparative Example CC;

[0115] Fig.18 shows the CV curve graph of Comparative Example DD;

[0116] Fig.19 The CV curve diagram of Example 2 is shown;

[0117] Fig. 20 shows the CV curve graph of Comparative Example EE;

[0118] Fig.21 shows the CV curve graph of Comparative Example FF;

[0119] Fig. 22 Nyquist plots of Example 3 and Comparative Examples GG-HH are shown;

[0120] Fig.23 The capacity retention rates of Example 3 and Comparative Examples GG-HH are shown;

[0121] Fig.24 The CV curve diagram of Example 4 is shown;

[0122] Fig.25 shows the CV curve graph of Comparative Example II;

[0123] Fig.26 shows a CV graph of Comparative Example JJ; and

[0124] Fig. 27 shows a CV curve graph of Comparative Example KK;

[0125] In the present disclosure, the accompanying drawings are used to emphasize certain aspects. Therefore, unless otherwise explicitly stated, the relative sizes of different regions, parts and substrates shown in the drawings should not be considered to be proportional to their actual relative sizes. DETAILED DESCRIPTION

[0126] Various aspects will now be described more fully with reference to the accompanying drawings, in which exemplary aspects are shown. Whenever possible, the same reference numbers are used throughout the drawings to refer to the same or like parts.

[0127] Figure 1-2 A view of a solid-state battery 101 or 201 is shown, which includes a solid electrolyte having a first major surface 109 and / or a second major surface 107 having a predetermined surface roughness Ra. In aspects, the surface roughness Ra of the second major surface 107 can be greater than the surface roughness Ra of the first major surface 109. In aspects, the surface roughness Ra of the first major surface 109 can be about 0.6 μm or less (e.g., about 0.1 μm to about 0.5 μm), and / or the surface roughness Ra of the second major surface 107 can be about 1 μm or greater (e.g., about 1.2 μm to about 3 μm). Unless otherwise stated, the discussion of features of aspects of a solid-state electrolyte or battery can be equally applied to corresponding features of any aspect of the present disclosure. For example, the same part number throughout the present disclosure can indicate that in some aspects, the identified features are identical to each other, and unless otherwise stated, the discussion of the identified features of one aspect can be equally applied to the identified features of any other aspect of the present disclosure.

[0128] Figure 1 The general structure of the solid-state battery 101 is schematically shown, and Figure 2A simplified solid-state battery 201 in the form of a button cell is shown. Figure 1 As shown, the solid-state battery 101 or 201 may include, in sequence, a first current collector 102 (e.g., a substrate), a cathode 104 disposed on the first current collector, an optional intermediate layer 114 disposed on the cathode 104, an optional first coating 106, a solid electrolyte 108, an optional second intermediate layer or coating 110 and an anode 112, and a second current collector 116 disposed on the anode 112. Figure 1 As shown, the solid-state battery 101 may optionally include an optional first coating 106 located between the cathode 104 and the solid-state electrolyte 108, and / or the solid-state battery 101 may optionally include an optional second intermediate layer or coating 110 located between the anode 112 and the solid-state electrolyte 108. Figure 1-2 As shown, solid-state electrolyte 108 is positioned between cathode 104 and anode 112. The components of solid-state battery 101 may be arranged horizontally or vertically relative to each other.

[0129] The first current collector 102 includes a conductive material. As used herein, the electronic conductivity of the conductive material measured at 20° C. is 100 Siemens / meter (S / m) according to ASTME1004-17. In aspects, the first current collector may include nickel foam (Ni), carbon fiber, or solid metal contact (solid metal contact) (e.g., aluminum, stainless steel, copper, platinum, nickel, gold, zinc, cobalt, nickel, ruthenium, lithium, lead, titanium, nickel-chromium alloy (nichrome), etc.). In aspects, the first current collector 102 may be a mechanically stable and / or dimensionally stable matrix supporting other elements of the solid-state battery 101 or 201. In aspects, the first current collector 102 may include the same material as the cathode 104 (discussed below) so that the first current collector 102 is part of the cathode 104.

[0130] The cathode 104 includes a conductive material. In aspects, the cathode 104 can be configured to release and reincorporate cations (e.g., alkali metals - lithium or sodium, alkaline earth metals - magnesium or calcium). In aspects, the cathode 104 can include at least one of an alkali metal (e.g., lithium, sodium) or an alkaline earth metal (e.g., magnesium, calcium). In aspects, the cathode 104 can include one or more of the materials for the anode 112 discussed below. In further aspects, the cathode 104 can include the same material as the anode 112. In aspects, the cathode 104 can include a fluoride compound. In further aspects, the cathode 104 can include at least one transition metal, such as cobalt, manganese, nickel, niobium, tantalum, vanadium, titanium, copper, chromium, tungsten, molybdenum, tin, germanium, antimony, bismuth, iron, or combinations thereof. In aspects, the cathode 104 can include a lithium-based electrode, such as lithium cobalt oxide (LCO), lithium manganese spinel (LMO), lithium nickel cobalt aluminate (NCA), lithium nickel manganese cobalt oxide (NCM) (LiNi d Co e Mn 1-d-e O 2 , where 0 < d < 1, 0 < e < 1, e.g., LiNi 0.5 Co 0.2 Mn 0.3 O 2 (NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622), etc.), lithium iron phosphate (LiFePO 4 )(LFP), lithium cobalt phosphate (LCP), lithium titanate, lithium niobium tungstate, lithium nickel manganate, and lithium titanium sulfide (LiTiS 2 ) or combinations thereof. In aspects, the cathode 104 can include a sodium-based electrode, such as, NaVPO 4 F, NaMnO 2 , Na 2 / 3 Mn 1- y Mg y O 2 (0 < y < 1), Na 2 Li 2 Ti 5 O 12 , Na 2 Ti 3 O 7 , or combinations thereof. In aspects, the cathode 104 can include a magnesium-based electrode, such as magnesiochromite (MgCr 2 O 4 ), MgMn 2 O4 or a combination thereof. Cathode 104 may be a sintered electrode. Alternatively, cathode 104 may be unsintered. An exemplary aspect of cathode 104 is an NCM cathode. In an aspect, the weight of cathode 104 is proportional to the cathode surface area (e.g., Figure 5-6 The ratio of the first major surface 105 of the cathode 104 shown in FIG. 1 may be about 5 mg / cm2 (mg / cm 2 ), about 8mg / cm 2 or larger, about 10 mg / cm 2 or greater, about 15 mg / cm 2 or larger, about 20 mg / cm 2 or greater, about 50 mg / cm 2 or larger, about 30 mg / cm 2 or less, about 25 mg / cm 2 or smaller, about 20 mg / cm 2 or less, or about 15 mg / cm 2 In one aspect, the ratio of the weight of cathode 104 to the cathode surface area of ​​cathode 104 can be about 5 mg / cm 2 To about 50mg / cm 2 , about 8mg / cm 2 To about 30mg / cm 2 , about 10mg / cm 2 To about 25mg / cm 2 , about 15mg / cm 2 To about 20mg / cm 2 , or any range or sub-range therebetween.

[0131] like Figure 1 As shown, the solid-state battery 101 may optionally include an intermediate layer 114 located between the cathode 104 and the solid-state electrolyte 108. In aspects, the intermediate layer 114 may include a liquid electrolyte (e.g., an ionic liquid, a eutectic solvent (DES) or an aprotic solvent). As used herein, an "electrolyte" is capable of transporting ions therein ("ionic conductivity"), and the ionic conductivity corresponds to the conductivity of the electrolyte (e.g., a DES-based electrolyte). The intermediate layer 114 may be a liquid at room temperature (i.e., 25°C) and / or at an operating temperature of the solid-state battery 101 (e.g., about 50°C to about 60°C). In aspects, the liquid electrolyte may include a lithium-containing salt and a solvent. In further aspects, the lithium-containing salt may include one or more of the following: lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4), lithium trifluoromethanesulfonate (LiSO 3 CF 3 )、LiC(SO 2 CF 3 ) 3 or a combination thereof. In a further aspect, the concentration of the lithium salt can be about 0.5 molar (M) or greater, about 1 M or greater, about 1.2 M or greater, about 1.5 M or greater, about 3 M or less, about 2.5 M or less, or about 2 M or less, for example, in the range of about 0.5 M to about 3 M, about 1 M to about 3 M, about 1.2 M to about 2.5 M, about 1.5 M to about 2 M, or any range or sub-range therebetween. An exemplary aspect of the solvent is cyclopentane sulfone, but other solvents are possible in other aspects. Providing an intermediate layer 114 including a liquid electrolyte can wet the interface between the cathode 104 and the solid electrolyte, thereby reducing the interfacial resistance therebetween while minimizing the total amount of liquid electrolyte in the solid-state battery 101. In aspects, the volume of the liquid electrolyte of the intermediate layer 114 is relative to the cathode surface area of ​​the cathode 104 (e.g., Figure 5-6 The first major surface 105 of the cathode 104 shown in FIG. 1 may be about 5 μL / cm 2 or larger, about 8 μL / cm 2 or larger, about 10 μL / cm 2 or larger, about 12 μL / cm 2 or larger, about 15 μL / cm 2 or larger, about 20 μL / cm 2 or smaller, about 15 μL / cm 2 or smaller, about 12 μL / cm 2 or smaller, about 10 μL / cm 2 In one aspect, the volume of the liquid electrolyte of the intermediate layer 114 relative to the cathode surface area of ​​the cathode 104 may be about 5 μL / cm 2 About 2 μL / cm 2 , about 8μL / cm 2 or to about 15 μL / cm 2 or about 10 μL / cm 2 to about 12 μL / cm 2 , or any range or sub-range therebetween.

[0132] like Figure 1-2As shown, solid-state batteries 101 and 201 include a solid electrolyte 108 located between a cathode 104 and an anode 112. Throughout the disclosure, "solid-state battery" includes a solid electrolyte. As used herein, a solid electrolyte is a material that is solid at room temperature and at the operating temperature of the solid-state battery (e.g., about 50 °C). In an aspect, the solid electrolyte 108 may include an inorganic solid electrolyte. Providing a solid electrolyte can address common safety issues such as leakage, poor chemical stability, and flammability that are common in batteries using liquid electrolytes. In addition, providing a solid electrolyte can also inhibit the shuttle of polysulfides from the cathode to the anode, resulting in improved utilization of the electrodes (e.g., anode, cathode) as well as high discharge capacity and energy density. Providing a solid electrolyte can reduce the formation of dendrites (e.g., lithium dendrites), which otherwise can cause battery failure.

[0133] In an aspect, the solid electrolyte 108 may include lithium phosphorus oxynitride (LiPON), lithium garnet (Li 7 La 3 Zr 2 O 12 ), lithium phosphorus sulfide, or a combination thereof. In a further aspect, the LIPON material may include a structure Li 3+y PO 4-x N x , where y > 0 and 0 < x < 4. In a further aspect, the solid electrolyte 108 may contain lithium, lanthanum, zirconium, oxygen, or a combination thereof (e.g., each of lithium, lanthanum, zirconium, and oxygen - LLZO compound). As used herein, "LLZO" refers to a compound containing lithium, lanthanum, zirconium, and oxygen. In an even further aspect, the solid electrolyte 108 may include a lithium-garnet, for example, at least one of the following: (i) Li 7-3a La 3 Zr 2 L a O 12 , where L = Al, Ga, or Fe and 0 < a < 0.33; (ii) Li 7 La 3-b Zr 2 M b O 12 , where M = Bi, Ca, or Y and 0 < b < 1; (iii) Li 7-c La 3 (Zr 2-c ,N c )O 12 , where N = In, Si, Ge, Sn, V, W, Te, Nb, or Ta and 0 < c < 1; (iv) protonated LLZO (e.g., H x Li 6.5-x La 3Zr 1.5 I 0.5 O 12 , where I = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 < x < 4, or H x Li 6.25-x E 0.25 La 3 Zr 2 O 12 , where E = Al, Ga or Fe and 0 < x < 4), or a combination thereof. In one aspect, the solid electrolyte 108 may include at least one of the following: Li 10 G 2 S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO 4 ) 3 , Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 , Li 0.55 La 0.35 TiO 3 , interpenetrating polymer network (ipn-PEA) electrolytes of poly(ethyl acrylate), three-dimensional ceramic / polymer networks, in situ plasticized polymers, composite polymers with well-aligned ceramic nanowires, PEO-based solid polymers, flexible polymers, polymeric ionic liquids, in situ formed Li 3 PS 4 , Li 6 PS 5 Cl or a combination thereof.

[0134] like Figure 1-2 As shown, the solid electrolyte 108 includes a first main surface 109 and a second main surface 107 opposite to the first main surface 109, and the thickness of the solid electrolyte 108 (for example, see Figure 7The thickness 707 in the solid electrolyte 108 can be defined between the first major surface 109 and the second major surface 107. In aspects, the thickness of the solid electrolyte 108 can be about 20 μm or more, about 40 μm or more, about 60 μm or more, about 80 μm or more, about 100 μm or more, about 150 μm or more, about 300 μm or more, about 500 μm or more, about 600 μm or more, about 700 μm or more, about 800 μm or more, about 1 mm or more, about 2 mm or less, about 1.5 mm or less, about 1.2 mm or less, about 1 mm or less, about 800 μm or less, about 500 μm or less, about 300 μm or less, about 250 μm or less, about 200 μm or less, about 150 μm or less, about 120 μm or less, or about 100 μm or less. In aspects, the thickness of the solid electrolyte 108 can be about 20 μm to about 2 mm, about 40 μm to about 1.5 mm, about 60 μm to about 1 mm, about 80 μm to about 800 μm, about 100 μm to about 500 μm, about 150 μm to about 300 μm, about 150 μm to about 250 μm, or any range or sub-range therebetween. In aspects, the thickness of the solid electrolyte 108 can be about 300 μm or less, for example, about 20 μm to about 300 μm, about 40 μm to about 250 μm, about 60 μm to about 200 μm, about 80 μm to about 150 μm, about 100 μm to about 150 μm, or any range or sub-range therebetween. In aspects, the thickness of the solid electrolyte 108 can be about 500 μm or greater, for example, about 500 μm to about 2 mm, about 600 μm to about 1.5 mm, about 700 μm to about 1 mm, about 800 μm to about 1 mm, or any range or sub-range therebetween.

[0135] In aspects, the solid electrolyte 108 may include a sintered tape. As used herein, a sintered tape refers to a material formed by sintering a ceramic green body, the thickness of which is substantially the same as that of the solid electrolyte. In other aspects, a solid electrolyte 108 including a sintered tape may include a thickness of about 300 μm or less, for example, about 20 μm to about 300 μm, about 40 μm to about 250 μm, about 60 μm to about 200 μm, about 80 μm to about 150 μm, about 100 μm to about 150 μm, or any range or sub-range therebetween. In aspects, the solid electrolyte 108 may include a consolidated pellet. As used herein, a solid electrolyte including a consolidated pellet refers to a material formed by pressing previously sintered particles together. Compared to a sintered tape, a consolidated pellet may include larger grains and a greater thickness. In a further aspect, the solid electrolyte 108 comprising consolidated pellets can include a thickness of about 500 μm or greater, for example, about 500 μm to about 2 mm, about 600 μm to about 1.5 mm, about 700 μm to about 1 mm, about 800 μm to about 1 mm, or any range or sub-range therebetween.

[0136] As used herein, a confocal laser scanning microscope is used to measure the surface profile over a test area of ​​10 μm × 10 μm, which is used to characterize the main surface of the solid electrolyte using the parameters defined in ISO 4287:1997. As used herein, the surface roughness Ra is calculated by the arithmetic mean of the absolute deviation of the surface profile from the average position. As used herein, Ra is measured using a VK-X250 (Keyence) laser scanning microscope. In aspect, the first main surface 109 of the solid electrolyte 108 may include a surface roughness Ra of about 0.6 μm or less, about 0.5 μm or less, about 0.4 μm or less, about 0.05 μm or more, about 0.1 μm or more, about 0.2 μm or more, about 0.3 μm or more, or about 0.4 μm or more. In various aspects, the first major surface 109 of the solid electrolyte 108 may include a surface roughness Ra of about 0.05 μm to about 0.6 μm, about 0.1 μm to about 0.5 μm, about 0.2 μm to 0.5 μm, about 0.3 μm to 0.5 μm, about 0.4 μm to about 0.5 μm, or any range or sub-range therebetween. Without wishing to be bound by theory, it is believed that the low roughness of the first major surface (e.g., about 0.6 μm or less or about 0.1 μm to about 0.5 μm) provides a substantially uniform surface for the anode (which enables uniform contact with the anode, reduces current concentration across the surface, and / or reduces the formation of dendrites) to achieve an increase in charging rate.

[0137] In aspects, the second major surface 107 of the solid electrolyte 108 may include a surface roughness Ra of about 1 μm or more, about 1.2 μm or more, about 1.3 μm or more, about 1.4 μm or more, about 2.5 μm or less, about 3 μm or less, about 2.5 μm or less, or about 2 μm or less, about 1.8 μm or less, about 1.6 μm or less, about 1.5 μm or less, or about 1.4 μm or less. In aspects, the second major surface 108 of the solid electrolyte 107 may include a surface roughness Ra of about 1 μm to about 3 μm, about 1 μm to about 2.5 μm, about 1.2 μm to 2 μm, about 1.2 μm to 1.8 μm, about 1.3 μm to about 1.5 μm, about 1.3 μm to about 1.4 μm, or any range or sub-range therebetween. Without wishing to be bound by theory, it is believed that the high roughness of the second major surface (eg, about 1 μm or more or about 1.2 μm to about 3 μm) reduces the interfacial resistance by increasing the surface area of ​​the interface between the solid electrolyte and the liquid electrolyte.

[0138] In aspects, the optional first coating 106 can include a carbon-based interlayer (e.g., interlinked, freestanding, microporous / mesoporous, functionalized, biomass-derived), a polymer-based interlayer, a metal-based coating (e.g., Ni foam, etc.), a liquid electrolyte (e.g., LiPF in ethylene carbonate (EC) / dimethyl carbonate (DMC) 6 ), based on ionic liquids (e.g., LiCF 3 SO 3 / CH 3 CONH 2 、LiTFSI / N-methylacetamide (NMA), PEO 18 LiTFSI-10%SiO 2 -10% IL, etc., where LiTFSI is bis(trifluoromethane)sulfonyl imide lithium salt (LiN(CF 3 SO 2 ) 2 ), SiO 2The IL may be a nanoparticle, and the IL is an ionic liquid), or a combination thereof. Exemplary aspects of the polymer-based intermediate layer include carbon polysulfides (CS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPY), poly(3,4-ethylenedioxythiophene) (PEDOT), polystyrene sulfonic acid (PSS), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyallylamine hydrochloride (PAH), polyvinylidene fluoride-co-hexafluoropropylene (P(VDF-co-HFP)), polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVDF), poly(diallyldimethylammonium) bis(trifluoromethanesulfonyl) imide (TFSI) (PDDATFSI) or a combination thereof. In aspects, the optional first coating 106 may include at least one element, or at least two elements, or at least three elements selected from the group consisting of nitrogen, carbon, cobalt, titanium, tantalum, and tungsten.

[0139] In one aspect, the optional second intermediate layer or coating 110 may include materials or aspects of the optional first coating 106 and / or intermediate layer 114 discussed above. In one aspect, the optional second intermediate layer or coating 110 may include an anode protectant, such as an electrolyte additive (e.g., LiNO 3 , lanthanum nitrate, copper acetate, P 2 S 5 etc.), artificial interface layers (e.g., Li 3 N, (CH 3 ) 3 SiCl、Al 2 O 3 , LiAl, etc.), composite metals (such as Li 7 B 6 , Li-rGO (reduced graphene oxide), layered Li-rGO, etc.) or a combination thereof. In aspects, the optional second intermediate layer or coating 110 may include a thin layer of metal (e.g., Au) (the metal thin layer may be ion sputtered to form a contact interface between the anode 112, the solid electrolyte 108, and the other materials of the optional second intermediate layer or coating 110). In aspects, the optional second intermediate layer or coating 110 may include a lithium fluoride coating. In aspects, such as Figure 2 As shown, the solid-state battery 201 may not have the optional second intermediate layer or second coating so that the anode 112 is in contact with the solid-state electrolyte 108.

[0140] like Figure 1-2 As shown, the anode 112 can be disposed on the solid electrolyte 108. In one aspect, as Figure 2As shown, the first major surface 113 of the anode 112 can be disposed on the first major surface 109 of the solid electrolyte 108. As shown, the anode 112 includes a second major surface 115 opposite the first major surface 113, and its anode thickness 119 is defined as the average distance between the two when the solid-state battery 201 is in a fully charged state (defined below). In aspects, the anode thickness 119 can be about 1 micrometer (μm) or more, about 10 μm or more, about 50 μm or more, about 100 μm or more, about 150 μm or more, about 500 μm or less, about 400 μm or less, about 300 μm or less, or about 250 μm or less. In aspects, anode thickness 119 can be about 1 μm to about 500 μm, about 10 μm to about 400 μm, about 50 μm to about 300 μm, about 100 μm to about 300 μm, about 150 μm to about 250 μm, or any range or sub-range therebetween.

[0141] Anode 112 is a lithium-containing anode. In aspects, the lithium-containing anode may be substantially composed of lithium metal. Alternatively, in aspects, the lithium-containing anode may include an alloy of lithium with at least one of magnesium (Mg), silver (Ag), or a combination thereof. In a further aspect, the lithium-containing alloy may further include a second component selected from the group consisting of calcium (Ca), aluminum (Al), gallium (Ga), boron (B), carbon (C), silicon (Si), tin (Sn), zinc (Zn), indium (In), antimony (Sb), silver (Ag), and a combination thereof. Exemplary aspects of the second component include calcium (Ca), tin (Sn), and silver (Ag). Providing a lithium-containing anode comprising a lithium alloy can increase the wettability of the anode on the coating, which can reduce the interfacial resistance of the battery (e.g., achieving and / or maintaining good contact with a solid electrolyte through the coating), is beneficial to the high area capacity of the battery, and / or is beneficial to the high charging current density of the battery.

[0142] Figure 2 A solid-state battery 201 is shown. Figure 2 As shown, the solid-state battery 201 may include a button cell form factor, but in other aspects the battery may include other forms. Figure 1 In comparison, because the optional first coating 106 is omitted, Figure 2 is a simplified solid-state battery 201. Thus, the intermediate layer 114 can be in direct contact with the cathode 104 and the solid electrolyte 108, for example, because the optional first coating 106 is omitted. In aspects such as Figure 2 As shown, the area of ​​the first major surface 113 of the anode 112 can be less than or equal to (e.g., less than) the area of ​​the first major surface 109 of the solid electrolyte 108. In a further aspect, as shown, the area of ​​the first major surface 113 of the anode 112 can be substantially equal to the corresponding area of ​​the cathode 104. Alternatively, as shown Figure 1As shown, the area of ​​the first major surface 113 of the anode 112 can be substantially equal to the area of ​​the first major surface 109 of the solid electrolyte 108. Figure 2 As shown, the electrically insulating layers 205a and 205b may be located between the first current collector 102 and the second current collector 116 to prevent short circuits in the solid-state battery 201 and / or form a barrier to protect the contents of the solid-state battery 201. As used herein, the electrically insulating layers 205a and 205b include 10 -5 S / cm or less electronic conductivity. In even further aspects, as shown, electrical insulating layers 205a and 205b can be configured to maintain the construction of solid-state battery 201, for example, by preventing solid electrolyte 108 from contacting second current collector 116. In further aspects, electrical insulating layers 205a and 205b can include polymer materials, such as fluoropolymers, rubber, polyurethane or silicone. In aspects, as shown, solid-state battery 201 can further include a conductive spacer 203 between anode 112 and second current collector 116. In further aspects, conductive spacer 203 can include foam (e.g., foam Ni), which can help maintain contact between adjacent components of the solid-state battery and / or control the stress amount borne by the components of the solid-state battery. Although not shown, a conductive spacer can be placed between the cathode and the first current collector.

[0143] As used herein, "interface resistance" is measured using electrical impedance spectroscopy (EIS) at 25°C at a frequency of 0.1 Hertz (Hz) to 1 Megahertz (MHz). Unless otherwise specified, EIS was measured using a Solartron 1260A (Solartron) impedance analyzer. The Nyquist plot consists of the real part of the impedance (Z', in Ωcm) on the horizontal axis. 2 The imaginary part of the impedance on the vertical axis (Z), in Ωcm 2 The interface resistance is defined as the difference between the real parts of the impedances of the endpoints of the arc in the EIS result (i.e., the Nyquist plot), where the higher endpoint is considered to be the inflection point in the impedance result. To determine the "interface resistance", the battery is configured such that the lithium-containing anode is disposed on the first main surface of the solid electrolyte and the second main surface of the solid electrolyte faces the cathode. In the aspect, the interface resistance can be about 60Ωcm 2 Or smaller, about 50Ωcm 2 Or smaller, about 40Ωcm 2 Or smaller, about 30Ωcm 2 Or smaller, about 25Ωcm 2 or less, or about 20Ωcm 2 In one aspect, the interface resistance may be about 10 Ωcm 2 to about 60Ωcm2 , about 10Ωcm 2 to about 50Ωcm 2 , about 10Ωcm 2 to about 40Ωcm 2 , about 15Ωcm 2 to about 30Ωcm 2 , about 20Ωcm 2 To about 25Ωcm 2 Or any range or sub-range therebetween. In various aspects, the interfacial resistance of another battery in which the first major surface and the second major surface of the solid electrolyte are interchanged will be greater than the interfacial resistance of the battery in which the major surfaces are not interchanged. In a further aspect, the interfacial resistance of the battery (in which the major surfaces are not interchanged), expressed as a percentage of the other battery (in which the major surfaces are interchanged), can be about 50% or less, about 40% or less, about 33% or less, or about 30% or less. In a further aspect, the interfacial resistance of the battery (in which the major surfaces are not interchanged), expressed as a percentage of the other battery (in which the major surfaces are interchanged), can be in the range of about 5% to about 50%, about 10% to about 40%, about 20% to about 33%, about 25% to about 30%, or any range or sub-range therebetween.

[0144] Unless otherwise specified, cycling includes charging at 1C to a predetermined nominal area capacity and discharging at 0.5C while the battery is maintained at 25°C. As used herein, "nominal capacity" (e.g., nominal area capacity) refers to the capacity achieved using predetermined charging conditions in the first charging step of the battery. The area capacity is expressed based on the surface area of ​​the anode. Unless otherwise specified, battery testing is performed at 25°C using a battery testing system CT2001A (Landt), including cycling and capacity retention at various nominal area capacities. Unless otherwise specified, the battery is configured such that the anode is disposed on a first major surface of the solid electrolyte and the second major surface of the solid electrolyte faces the cathode. In aspect, the battery can withstand at least 10 cycles at 25°C at 1.6 mA / cm 2 (1.6C) or higher, about 1.8mA / cm 2 (1.8C) or higher, or about 2mA / cm 2 (2C) charging current density is charged to 1 mAh / cm 2 Nominal area capacity and 0.5 mA / cm 2 As used herein, "withstand" means that the battery does not exhibit short circuit or non-ohmic behavior during cycling. In one aspect, another battery in which the first major surface and the second major surface of the solid-state electrode are interchanged may not withstand 10, 8, or 6 cycles of 1.25 mA / cm2 at 25°C. 2(1.25C) charging current density to 1 mAh / cm 2 Nominal area capacity and 0.5 mA / cm 2 In another aspect, another battery in which the first main surface and the second main surface of the solid-state electrode are interchanged may not withstand 10 cycles of discharge at 25°C and 1 mA / cm 2 (1C) or higher, about 1.25mA / cm 2 (1.25C) or higher or about 1.5mA / cm 2 (1.5C) or higher charging current density to 1 mAh / cm 2 Nominal area capacity and 0.5 mA / cm 2 In one aspect, 60 or more cycles (e.g., charging to 1 mAh / cm at 1C at 25°C) were performed at a cutoff voltage of 4.5V. 2 The battery can exhibit a capacity retention rate of 90% or more, 92% or more, or 95% or more after a nominal area capacity of 1000A and a discharge at 0.5C. In one aspect, 60 or more cycles (e.g., charging to 1 mAh / cm at 1C) are performed at a cutoff voltage of 4.5V and 60°C. 2 The battery can exhibit a capacity retention rate of 90% or more, 92% or more, or 95% or more after a nominal area capacity of 0.5C is discharged. In one aspect, the ... at a nominal area capacity of 0.5C. 2 After cycling with a nominal area capacity of 1000MW and discharged at 0.17C, the battery can exhibit a capacity retention rate of 90% or more, 92% or more, or 95% or more.

[0145] Reference Figure 3-10 Aspects of methods for processing solid electrolytes and / or methods for manufacturing solid-state batteries according to aspects of the present disclosure are discussed with reference to the example method steps shown in . The method may include providing a solid electrolyte, which may include one or more of the materials discussed above related to solid electrolytes. In aspects, the solid electrolyte 108 may include a sintered tape, for example, with a thickness of about 20 μm to about 300 μm. Alternatively, in aspects, the solid electrolyte 108 may include a consolidated pellet, for example, with a thickness of about 500 μm to about 2 mm.

[0146] In terms of Figure 7 and Fig. 9As shown, the method includes polishing the initial first main surface of the solid electrolyte 108 to obtain a predetermined first surface roughness Ra of the first main surface 109. The predetermined first surface roughness can be within one or more ranges of the surface roughness Ra of the first main surface of the solid electrolyte discussed above, for example, about 0.6 μm or less, or about 0.1 μm to about 0.5 μm. In a further aspect, the thickness 707 of the solid electrolyte 108 before polishing (for example, between the first main surface 109 and the initial second main surface 705) can be substantially the same as the thickness of the solid electrolyte in the solid-state battery 101 or 201.

[0147] In a further aspect, Figure 7 As shown, polishing first major surface 109 can include etching first major surface 109 with acidic solution 703. In even further aspects, as shown, acidic solution 703 can be contained in acid bath 701. In even further aspects, as shown, etching first major surface 109 and etching second major surface 107 can not be performed simultaneously, although in other aspects the major surfaces can be etched simultaneously for at least a portion of the time. In even further aspects, the acidic solution can include an inorganic acid (e.g., HCl, HNO 3 , H 2 SO 4 , H 3 PO 4). In a further aspect, the concentration of the inorganic acid can be about 0.1 molar (M) or greater, about 0.5M or greater, about 1M or greater, about 1.5M or greater, about 3M or less, about 2M or less, or about 1.5m or less. In a further aspect, the concentration of the inorganic acid can be in the range of about 0.1M to about 3M, about 0.5M to about 2M, about 1M to about 1.5M, or any range or sub-range therebetween. In an even further aspect, the acidic solution can include a pH of about 3 or less, about 1 or less, or about 1 or less. In a further aspect, the acidic solution can be maintained at a temperature of about 20°C or more, about 25°C or more, about 30°C or more, about 40°C or less, about 35°C or less, or about 30°C or less. In a further aspect, the acidic solution can be maintained at a temperature of about 20°C to about 40°C, about 20°C to about 35°C, about 25°C to about 30°C, or any range or sub-range therebetween. In a further aspect, etching (e.g., contact between an acidic solution and the first major surface) can occur for about 4 minutes or less, about 3 minutes or less, about 2 minutes or less, about 10 seconds or longer, about 30 seconds or longer, or about 1 minute or longer. In a further aspect, etching can occur for about 10 seconds to about 4 minutes, about 30 seconds to about 3 minutes, about 1 minute to about 2 minutes, or any range or sub-range therebetween. Without wishing to be bound by theory, etching for a short time (e.g., about 4 minutes or less) can reduce surface irregularities without increasing the surface roughness of the first major surface (e.g., by etching the grain boundaries of a solid electrolyte).

[0148] Or, in a further aspect, Fig. 9 As shown, polishing the first major surface 109 may include mechanical polishing. For example, as shown, mechanical polishing the first major surface 109 may include rotating (as shown by arrow 903) a grinding tool 901, which includes a grinding surface 907 of an abrasive 905. In an even further aspect, the abrasive 905 of the grinding surface 907 may include a mesh number of about 1000 or greater (e.g., a median particle size of about 10 microns or less) or about 1200 or greater (e.g., a median particle size of about 8 microns or less). In an even further aspect, the abrasive 905 may include a greater hardness than the solid electrolyte 108, for example, the abrasive may include silicon carbide or other materials used in "sandpaper". Providing a high mesh number (or low median particle size) abrasive for mechanically polishing the first major surface can produce a low surface roughness of the first major surface.

[0149] In terms of Figure 8 and Fig.10As shown, the method may further include polishing the initial second main surface 705 of the solid electrolyte 108 to obtain a predetermined second surface roughness Ra of the second main surface 107. The predetermined second surface roughness may be within one or more ranges of the surface roughness Ra of the second main surface of the solid electrolyte discussed above, for example, about 1 μm or greater, or about 1.2 μm to about 3 μm.

[0150] In a further aspect, Figure 8 As shown, the initial second major surface 705 (see Figure 7 and 9 ) to form the second main face 107 may include etching the second main surface 107 or 705 with an acidic solution 803. In an even further aspect, as shown, the acidic solution 803 may be contained in the acidic bath 801. In an even further aspect, the acidic solution 803 may include an inorganic acid (e.g., HCl, HNO 3 , H 2 SO 4 , H 3 PO 4 ). In a further aspect, the concentration of the inorganic acid can be about 0.1 molar (M) or greater, about 0.5M or greater, about 1M or greater, about 1.5M or greater, about 3M or less, about 2M or less, or about 1.5m or less. In a further aspect, the concentration of the inorganic acid can be in the range of about 0.1M to about 3M, about 0.5M to about 2M, about 1M to about 1.5M, or any range or sub-range therebetween. In an even further aspect, the acidic solution can include a pH of about 3 or less, about 1 or less, or about 1 or less. In a further aspect, the acidic solution can be maintained at a temperature of about 20°C or more, about 25°C or more, about 30°C or more, about 40°C or less, about 35°C or less, or about 30°C or less. In a further aspect, the acidic solution can be maintained at a temperature of about 20°C to about 40°C, about 20°C to about 35°C, about 25°C to about 30°C, or any range or sub-range therebetween. In an even further aspect, as shown, etching the second major surface 107 or 705 can be performed simultaneously with etching the first major surface 109, although the major surface can be etched simultaneously for at least a portion of the time the second major surface is etched. In a further aspect, etching (e.g., contact between the acidic solution and the second major surface) can occur for a time of about 7 minutes or more, about 10 minutes or more, about 15 minutes or more, about 30 minutes or less, about 25 minutes or less, about 20 minutes or less, or about 15 minutes or less. In a further aspect, etching can occur for a time of about 7 minutes to about 30 minutes, about 7 minutes to about 25 minutes, about 7 minutes to about 20 minutes, about 10 minutes, or about 15 minutes, or any range or sub-range therebetween. In an even further aspect, polishing the first major surface (see Figure 7 ) and the second major surface (see Figure 8 ) can include etching corresponding main surface.In further aspect, the time period of etching the second main surface can be longer than the time period of etching the first main surface, for example, about 3 minutes or longer, about 5 minutes or longer or about 7 minutes or longer.It should be understood that the first main surface can be polished by etching and / or mechanical polishing in combination with etching the second main surface.In the case of not wishing to be bound by theory, the etching of a longer time period (for example, about 7 minutes or longer) can increase the surface roughness of the second main surface, for example, by etching the grain boundaries of the solid electrolyte and / or leaching part of the solid electrolyte.

[0151] Or, in a further aspect, such as Fig.10 As shown, the initial second major surface 705 (see Figure 7 and 9 ) to form the second major surface 107 may include mechanical polishing. For example, as shown, mechanical polishing the second major surface 107 or 705 may include rotating (as shown by arrow 1003) a grinding tool 1001, which includes a grinding surface 1007 of an abrasive 1005. In a further aspect, the abrasive 1005 of the grinding surface 1007 may include a mesh size of about 600 or less (e.g., a median particle size of about 20 microns or greater) or about 400 or less (e.g., a median particle size of about 25 microns or greater). In an even further aspect, the abrasive 1005 may include a greater hardness than the solid electrolyte 108, for example, the abrasive may include silicon carbide or other materials used in "sandpaper". In an even further aspect, polishing the first major surface (see Fig. 9 ) and the second main surface (see Fig.10 ) may include mechanical polishing of the corresponding main surface. In a further aspect, the mesh number of the abrasive used for mechanical polishing the first main surface may be greater than the mesh number of the abrasive used for mechanical polishing the second main surface, about 200 or more, about 400 or more, or about 600 or more. In a further aspect, the median particle size of the abrasive used for mechanical polishing the first main surface may be smaller than the value particle size of the abrasive used for mechanical polishing the second main surface by about 5 μm or more, about 10 μm or more, or about 12 μm or more. It should be understood that the first main surface can be polished by etching and / or mechanical polishing in combination with mechanical polishing the second main surface. Providing a low mesh number (or high median particle size) abrasive for mechanical polishing the second main surface can produce a high surface roughness of the second main surface. The method for treating the solid electrolyte can be completed after polishing the first main surface and polishing the second main surface.

[0152] The method of manufacturing a battery (e.g., a solid-state battery) may further include providing an anode on the first major surface of the solid-state electrolyte. Figure 3As shown, the method may include disposing a lithium-containing material 305 on a first major surface 109 of a solid-state electrolyte 108. In a further aspect, as shown, disposing the lithium-containing material 305 may include dispensing one or more molten metals 303 (e.g., elemental metals or alloys in a molten state) from a source 301 (e.g., a metal foil, a catheter, a micropipette, or a syringe). Alternatively, disposing the lithium-containing material 305 for the anode 112 may include deposition from a vapor phase, for example, by sputtering from one or more sources (e.g., elemental targets or alloy targets) and / or by thermal evaporation, but other methods of physical vapor deposition (PVD) may also be used to form the anode 112. In aspects, the lithium-containing material 305 and / or the anode 112 may consist essentially of lithium metal. Alternatively, in aspects, the lithium-containing material 305 and / or the anode 112 may include an alloy of lithium with at least one of magnesium, silver, or a combination thereof. Alternatively, the lithium-containing material may be disposed on the solid-state electrolyte by attaching a metal foil containing the lithium-containing material to the first major surface of the solid-state electrolyte, which may be described below with reference to Figure 4 to be processed.

[0153] In one aspect, after or during the provision of the alloy (eg, lithium-containing material 305, anode 112), as Figure 4As shown, the solid electrolyte 108 and the lithium-containing material (e.g., anode 112) can be in an environment maintained at a first temperature. For example, as shown, the solid electrolyte 108 can be placed in an oven 401 maintained at a first temperature. The first temperature is greater than the melting point of one or more materials used to form the anode. In a further aspect, the first temperature can be about 50°C or more, about 100°C or more, about 125°C or more, or about 150°C or more than the melting point of one or more materials used to form the anode. For example, the melting temperature of lithium metal is about 180°C. In aspect, the first temperature can be about 280°C or more, about 300°C or more, about 320°C or more, about 500°C or less, about 400°C or less, or about 350°C or less, for example, about 280°C to about 500°C, about 300°C to about 400°C, about 320°C to about 350°C, or any range or sub-range therebetween. In a further aspect, after the lithium-containing material is provided, the solid electrolyte 108 and the lithium-containing material can be maintained at the first temperature for about 1 minute or more, about 3 minutes or more, about 5 minutes or more, about 15 minutes or more, about 20 minutes or more, about 1 hour or less, about 45 minutes or less, about 30 minutes or less, or about 25 minutes or less. In a further aspect, after the lithium-containing material is provided, the solid electrolyte 108 and the lithium-containing material can be maintained at the first temperature for about 1 minute to about 1 hour, about 3 minutes to about 45 minutes, about 5 minutes to about 30 minutes, about 15 minutes to about 30 minutes, about 20 minutes to about 25 minutes, or any range or sub-range therebetween. Providing temperatures and times within the above one or more ranges can achieve wetting of the lithium-containing material or otherwise conforming to the first main surface 109 of the solid electrolyte 108. As discussed in the Examples, an anode consisting essentially of lithium can be heated at about 330°C or higher (e.g., about 330°C to about 400°C) to ensure that the resulting anode forms intimate and / or uniform contact with the first major surface of the solid-state electrolyte, while lithium alloys can be heated over a wider temperature range (e.g., about 300°C or higher) to achieve similar properties and / or performance.

[0154] In terms of Figure 5As shown, the method may further include providing an intermediate layer 114 by providing a liquid electrolyte 505 on the cathode 104. In a further aspect, the liquid electrolyte may include a lithium salt and a solvent, which may include one or more of the materials of the intermediate layer 114 discussed above. In a further aspect, the concentration of the lithium salt in the solvent may be within one or more ranges discussed above. In a further aspect, as shown, providing the liquid electrolyte 505 may include dispensing a predetermined amount of liquid 503 from a container 501 (e.g., a conduit, a flexible tube, a micropipette, or a syringe), thereby forming a liquid electrolyte 505 on the first major surface 105 of the cathode 104. In a further aspect, the predetermined amount of the intermediate layer 114 (e.g., liquid electrolyte 505) expressed as a ratio of the volume of the intermediate layer (e.g., liquid electrolyte) to the area of ​​the first major surface of the cathode may be within one or more corresponding ranges discussed above. Providing this ratio of the volume of the intermediate layer to the area of ​​the first major surface of the cathode may be sufficient to wet the interface between the cathode and the solid electrolyte while minimizing problems associated with conventional liquid electrolytes (e.g., in liquid-based batteries or liquid-solid hybrid batteries). Although not shown, the cathode may be disposed on the first current collector, and the intermediate layer is disposed on the cathode.

[0155] In terms of Figure 6 As shown, as shown by arrow 601, the method can further include disposing a solid electrolyte 108 on the cathode 104. As shown, the cathode 104 can be opposite to the first major surface 109 of the solid electrolyte 108, the optional second intermediate layer or coating 110, and / or the anode 112. As shown, the solid electrolyte 108 is located between the cathode 104 and the anode 112. Although not shown, when the solid electrolyte is disposed on the cathode, additional elements (e.g., a current collector) can be present, and / or additional elements can be added after the cathode is disposed to form a battery (e.g., solid-state battery 101 or 201).

[0156] Example

[0157] Various aspects are further illustrated by the following examples. Example AD is a lithium garnet (discussed below) solid electrolyte polished under different conditions. Example CD, Example 1 and Comparative Examples (CE) AA-CC include a sintered strip of a lithium garnet (discussed below) solid electrolyte having a thickness of 120 μm and a diameter of 14 mm. Example AB, Examples 2 and 4, and Comparative Examples DD-FF and II-KK include a consolidated pellet of a lithium garnet (discussed below) solid electrolyte having a net thickness of 600 μm and a diameter of 14 mm. Example 3 and Comparative Examples GG-HH include a sintered strip of a lithium garnet (discussed below) solid electrolyte having a thickness of 120 μm, a width of 25.4 mm and a length of 25.4 mm (1 square inch).

[0158] Example 1 and Comparative Example AA-cc included a spodumene (LCO) cathode with a mass loading of 20 mg / cm 2 , which has a diameter of 12 mm. Examples 2 and 4 and Comparative Examples AA-FF and II-KK include a cathode mass loading of 20 mg / cm 2 and a NCM523 cathode with a diameter of 12 mm. Example 3 includes a mass loading of 20 mg / cm 2 , a NCM523 cathode having a width of 20 mm and a length of 20 mm. For Examples 1-3 and Comparative Examples AA-HH, the anode comprises a lithium alloy of 10 atomic % magnesium and the remainder lithium metal. For Example 4 and Comparative Examples II-KK, the anode consists of lithium metal.

[0159] NCM523 refers to LiNi 0.5 Co 0.2 Mn 0.3 O 2 (Precursors commercially available from Landt Instruments). NCM523 and LCO are separately formed into slurries having a weight ratio of 8:1:1 of precursors, super P carbon black (available from Timcal-Imerys) and polyvinylidene fluoride (PVDF) (dissolved in N-methylpyrrolidone), which are coated on an aluminum (Al) foil having a predetermined thickness and dried under vacuum. After polishing the surface of the solid electrolyte (discussed below and in Tables 1-4), a lithium-containing material for the anode is disposed on the coating and heated at 300°C (Examples 1-3 and Comparative Examples AA-HH and JJ-KK) or 330°C (Example 4 and Comparative Example II) for 5 minutes. In Examples 1-4 and Comparative Example AA-KK, 10 μL / cm2 of 1.2 M LIFSI dissolved in cyclopentane was added. 2 The liquid electrolyte is placed on the cathode, and then the solid electrolyte is placed above the cathode with the liquid electrolyte in between. Examples 1-2 and 4 and Comparative Examples AA-FF and II-KK are formed similar to Figure 2 The solid-state battery 201 in the form of a CR2025 button cell shown in FIG. 201 , wherein the Ni foam is disposed above the anode. Example 3 and Comparative Examples GG-HH are formed into soft-pack batteries using an aluminum-plastic film.

[0160] Lithium garnet solid electrolyte is cubic phase Li 6.5 La 3 Zr 1.4 Ta 0.5 O 12 (LLZTO), which is composed of LiOH·H 2 O(AR), La 2 O 3(99.99%), ZrO 2 (AR), Ta 2 O 5 The initial powder (99.99%) was synthesized according to the stoichiometric ratio. 2 wt% excess LiOH·H was added 2 O to compensate for the lithium loss during processing. 2 O 3 Heat at 900°C for 12 hours to remove any moisture and / or CO 2 . The raw materials were mixed by a wet grinding process using yttrium stabilized zirconia (YSZ) balls and isopropyl alcohol (IPA) as grinding media. For consolidated pellets, pellets were formed by drying and calcining the mixture at 950°C in an alumina crucible for 6 hours, producing pure cubic garnet phase powder. These powders were pressed into green pellets and sintered at 1230°C for 1 hour in a platinum crucible covered with 15 wt% Li excess LLZTO powder. For sintered tapes, the mixture was mixed with an organic binder system comprising a propionate solvent, a dispersant, a plasticizer and an acrylate-based polymer, and tape cast using a doctor blade to form a green tape. The green tape was sintered at 1000°C to 1300°C for 10 minutes.

[0161] As shown in Table 1, the surface of the lithium garnet solid electrolyte was treated with a 1M HCl solution at 25°C, or mechanically polished with a silicon carbide (SiC) abrasive. For example, Examples AD. Unless otherwise specified in the Reference Examples and Comparative Examples, "etching" refers to treatment with a 1M HCl solution at 25°C, and "SiC" refers to mechanical polishing with a SiC abrasive. Fig.11 (a)-(d) schematically show scanning electron microscope (SEM) images of Examples AD at the same scale (magnification), with contrast enhanced to improve visibility. Fig.11 As shown in (a), Example A, which was etched for 1 minute, has a flat surface with visible smooth grain boundaries that define the garnet grains of the consolidated pellet 1101. Fig.11As shown in (b), Example B, in which the surface was etched for 10 minutes, was porous, with pores 1105 formed between the grains 1103 etched to have an irregular appearance. As shown in Table 1, the surface roughness Ra of Example A was 0.5 μm, while that of Example B was 1.5 μm. Therefore, an increase in etching time is associated with an increase in surface roughness. Without wishing to be bound by theory, it is believed that a relatively short etching time can reduce surface irregularities without increasing the surface roughness of the first major surface (e.g., by etching the grain boundaries of the solid electrolyte), while a relatively long etching time can increase the surface roughness of the first major surface, for example, by etching the grain boundaries of the solid electrolyte and / or leaching out a portion of the solid electrolyte. As Fig.11 As shown in (c), the surface of Example C mechanically polished with 1200 grit SiC abrasive (median particle size of about 8 μm) is smooth and flat, with small flaws 1111 associated with the abrasive grains, and no discernible texture of the grains in the sintered ribbon. Fig.11 As shown in Table 1, the surface of Example D mechanically polished with 400 mesh SiC abrasive (median particle size of about 25 μm) is rough, with visible grains 1115 and several large scratches 1113 associated with the abrasive grains in the sintered strip. As shown in Table 1, the surface roughness Ra of Example C is 0.4 μm, while that of Example D is 1.2 μm. Therefore, an increase in mesh (a decrease in particle size) is associated with a decrease in surface roughness. For Examples 1-4 and Comparative Examples AA-KK, the treatment of each major surface was selected from the treatment in Example AD, and the method (etching with SiC) and the resulting surface roughness Ra are shown in Tables 2-4.

[0162] Table 1: Properties of Examples AD

[0163]

[0164] Table 2 shows the properties of Examples 1-2 and Comparative Examples AA-FF. As described above, Example 1 and Comparative Examples AA-CC include sintered tape solid electrolytes that are etched to achieve the roughness values ​​shown in Table 2; and Example 2 and Comparative Examples DD-FF include consolidated granular solid electrolytes that are mechanically polished to achieve the roughness values ​​shown in Table 2. Examples 1-2 include a surface roughness Ra of 0.6 μm or less on the first main surface, which is less than the surface roughness Ra of greater than 1 μm on the second main surface. Comparative Examples BB and EE are the same as Examples 1 and 2, respectively, wherein the surface roughness Ra of the first main surface and the second main surface are interchanged. Both main surfaces in Comparative Examples AA and DD include a surface roughness Ra of 0.6 μm or less, and both main surfaces in Comparative Examples CC and FF include a surface roughness Ra greater than 1 μm.

[0165] Table 2: Properties of Examples 1-2 and Comparative Examples AA-FF

[0166]

[0167] * = Examples that can withstand all tested charging current densities

[0168] Fig.12 shows Nyquist plots for Example 1 and Comparative Examples AA-CC; and Fig.13 The Nyquist plots of Example 2 and Comparative Example DD-FF are shown. As described above, Figure 12-13 The data shown in were measured by EIS at 25°C using a Solartron 1260A (Solartron) impedance analyzer with a frequency of 0.1 Hz to 1 megahertz (MHz). Figure 12-13 In FIG. 1 , the horizontal axes 1201 and 1301 correspond to the real part of the impedance (Z', in Ωcm 2 ), and the vertical axes 1203 and 1303 correspond to the imaginary part of the impedance (Z", in Ωcm 2 As described above, the interface resistance shown in Table 2 is measured as the difference between the real parts of the impedances at the end points of the arcs of the curves corresponding to the EIS results in the Nyquist plot. Curves 1207 and 1209 correspond to Comparative Examples AA and BB, respectively, where the interface resistance is greater than 70 Ω cm 2 Curves 1205 and 1211 correspond to Example 1 and Comparative Example CC, respectively, where the interface resistance is about 20 Ωcm 2 . Therefore, the lower surface roughness Ra (e.g., 0.6 μm or less) of the first major surface in Example 1 and Comparative Example CC produces a lower surface roughness than the higher surface roughness Ra (e.g., greater than 1 μm) of the first major surface in Comparative Examples AA-BB. Similarly. Curves 1307 and 1309 correspond to Comparative Examples DD and EE, respectively, where the interface resistance is 110 Ωcm 2 or greater; and curves 1305 and 1311 correspond to Example 2 and Comparative Example FF, respectively, wherein the interface resistance is about 60Ωcm 2 or less. Therefore, Example 1-2 achieves about 60Ωcm 2 Although the interface resistance of the sintered tape (Example 1) is lower relative to the consolidated tape (Example 2), the trend that a lower surface roughness Ra of the first major surface (e.g., 0.6 μm or less) is associated with reduced interface resistance is Figure 12-13 is consistent in.

[0169] Figure 14-17 The capacity-voltage (CV) curves of Comparative Example AA, Example 1, and Comparative Example BB-CC are shown respectively. Figure 14-17 , at 1 mAh / cm at 25 °C in all cycles2 The battery was tested at a discharge rate of 0.5C and at different charge current densities (or charging rates). Initially, the charge current density was 0.5 mA / cm 2 (0.5C), and increase by 0.25mA / cm every 10 cycles 2 (0.25C) to 2mA / cm 2 (2C) maximum value, for simplicity, the last cycle is a given charging current density (until failure occurs), such as Figure 14-17 As shown in Figure 14-17 In the figure, the horizontal axis 1401 corresponds to mAh / cm 2 The vertical axis 1403 corresponds to the instantaneous capacity in units of volts (V). Fig.14 , curves 1405, 1407, 1409, 1411, 1413, 1415, and 1417 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.5C, 0.75C, 1C, 1.25C, 1.5C, 1.75C, and 2C, respectively. Curve 1421 corresponds to the mutually overlapping charge curves from 0.5C to 2C. Fig.14 All charge curves (up to 2C) appear normal. Fig.15 , curves 1505, 1507, 1509, 1511, 1513, 1515, and 1517 correspond to discharge curves at 0.5 C as part of a cycle of charging at 0.5 C, 0.75 C, 1 C, 1.25 C, 1.5 C, 1.75 C, and 2 C, respectively. Curve 1521 corresponds to the overlapping charge curves from 0.5 C to 2 C. Fig.15 All the charging curves (up to 2C) in the graph appear normal. Therefore, Example 1 and Comparative Example AA can withstand at least 10 cycles of 2C charging rate and 0.5C discharge rate at 25°C to reach 1 mAh / cm 2 The nominal area capacity of the cycle.

[0170] Figure 16-17 The capacitance-voltage (CV) curves of comparative examples BB-CC are shown respectively. Fig.16 In FIG. 1 , curves 1605, 1607, 1609, and 1611 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.5C, 0.75C, 1C, and 1.25C, respectively. Curve 1521 corresponds to overlapping charge curves at 0.5C, 0.75C, and 1C, while curve 1623 corresponds to a charge curve at 1.25C. Curve 1611 shows irregularities (e.g., non-ohmic behavior), while curve 1623 shows that a short circuit exists at 1.25C. In FIG. Fig.17, curves 1705, 1707, 1709, 1711, and 1713 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.5C, 0.75C, 1C, 1.25C, and 1.5C, respectively. Curve 1721 corresponds to charging curves 0.5C, 0.75C, and 1C that overlap each other. Curve 1723 corresponds to charging at 1.25C, while curve 1725 corresponds to charging at 1.5C. Curve 1713 shows irregularities, curve 1723 indicates a reduction in capacity when charged at 1.25C, and curve 1725 indicates a failure when charged at 1.5C. Therefore, the comparative example BB-CC cannot withstand at least 10 charges to 1 mAh / cm2 at 1.5C (or 1.25C) at 25°C. 2 The nominal area capacity can be cycled without irregularities or failures. Comparing Example 1 and Comparative Example AA with Comparative Examples BB-CC, the surface roughness Ra of the second major surface is the distinguishing feature. Based on Figure 14-17 As a result, providing a surface roughness Ra of the second major surface of 1 μm or greater (e.g., 1.4 μm, 1.5 μm) increases the charge current density that the battery can withstand (e.g., relative to a surface roughness of 0.6 μm or less).

[0171] Figure 18-21 The capacity-voltage (CV) curves of Comparative Example DD, Example 2, and Comparative Example EE-FF are shown respectively. Figure 18-21 , at 1 mAh / cm at 25 °C in all cycles 2 The cells were tested at a discharge rate of 0.5 C and at different charge current densities (or charge rates). Unlike the sintered strips of Example 1 and Comparative Examples AA-CC, the charge current density for the consolidated pellets of Example 2 and Comparative Examples DD-FF was initially 0.4 mA / cm 2 (0.4C), increase 0.2mA / cm every 10 cycles 2 (0.2C) to 0.8mA / cm 2 (0.8C) maximum, in simplification, the last cycle is a given charging current density (until failure occurs), such as Figure 18-21 In the Figure 18-21 In the figure, the horizontal axis 1801 corresponds to mAh / cm 2 The vertical axis 1803 corresponds to the instantaneous capacity in units of volts (V). Fig.18 , curves 1805, 1807 and 1809 correspond to discharge curves at 0.5 C as part of a cycle of charging at 0.4 C, 0.6 C and 0.8 C, respectively. Curves 1811, 1813 and 1815 correspond to charge curves at 0.4 C, 0.6 C and 0.8 C, respectively. Fig.18All the charge curves in the 1000A (up to 0.8C) appear normal, although the charge curves do not completely overlap each other. Fig.19 In FIG. 1 , curves 1905, 1907 and 1909 correspond to discharge curves at 0.5 C as part of a cycle of charging at 0.4 C, 0.6 C and 0.8 C, respectively. Curves 1911, 1913 and 1915 correspond to charge curves at 0.4 C, 0.6 C and 0.8 C, respectively. Fig.19 All charging curves in (up to 0.8C) appear normal. However, curve 1915 shows that there is a short circuit when charging at 0.8C. Therefore, when the second major surface has a high surface roughness Ra (e.g., about 1 μm or higher), Example 2 and Comparative Example DD can withstand at least 10 times at 25°C with a charge rate of 0.6C or higher (e.g., 0.8C) and a discharge rate of 0.5C to reach 1 mAh / cm 2 The nominal area capacity of the cycle.

[0172] Figure 20-21 The capacitance-voltage (CV) curves of comparative examples EE-FF are shown respectively. Fig. 20 In FIG. 2 , curves 2005 and 2007 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.4C and 0.6C, respectively. Curves 2011 and 2013 correspond to charge curves at 0.4C and 0.6C, respectively. Curve 2013 shows that there is a short circuit when charging at 0.6C. Fig.21 In the figure, curves 2105 and 2107 correspond to the discharge curves at 0.5C as part of the cycle of charging at 0.4C and 0.6C, respectively. Curves 2111 and 2113 correspond to the charging curves at 0.4C and 0.6C, respectively. Curve 2113 shows that failure occurred when charging at 0.6. Therefore, the comparative example EE-FF cannot withstand at least 10 cycles of charging at 0.6C at 25°C to 1 mAh / cm 2 The surface roughness Ra of the second major surface is the distinguishing feature when comparing Example 2 and Comparative Example DD with Comparative Examples EE-FF. Figure 18-21 As a result, providing a surface roughness Ra of the second major surface of 1 μm or greater (e.g., 1.4 μm, 1.5 μm) increases the charge current density that the battery can withstand (e.g., relative to a surface roughness of 0.6 μm or less).

[0173] For Example 3 and Comparative Examples GG-HH, they include soft pack batteries having the properties shown in Table 3. Fig. 22 The Nyquist plots of Example 3 and Comparative Examples GG-HH are shown. Fig. 22 , the horizontal axis 2201 corresponds to the real part of the impedance (Z', in Ωcm2 ), and the vertical axis 2203 corresponds to the imaginary part of the impedance (Z", in Ωcm 2 As described above, the interface resistance shown in Table 3 is measured as the difference between the real parts of the impedances of the arc endpoints of the curves corresponding to the EIS results in the Nyquist plot. Curves 2205, 2207, and 2209 correspond to Example 3 and Comparative Examples GG-HH, respectively. Example 3 and Comparative Example HH include 20Ωcm 2 or smaller (e.g., 15Ωcm 2 or less, 10Ωcm 2 or less). Comparative Example GG has an interface resistance greater than 60Ωcm 2 (For example 70Ωcm 2 Thus, the lower surface roughness Ra (e.g., 0.6 μm or less) of the first major surface in Example 3 and Comparative Example HH produces a lower surface roughness than the higher surface roughness Ra (e.g., greater than 1 μm) of the first major surface in Comparative Example GG.

[0174] Table 3: Properties of Example 3 and Comparative Example GG-HH soft pack batteries

[0175]

[0176] * = Examples that withstand all test cycles

[0177] Fig.23 It shows that Example 3 and Comparative Example GG-HH are heated at 60°C and 0.5C (1.5 mAh / cm 2 ) and 0.17C (0.5mAh / cm 2 ) discharge rate reaches 3mAh / cm 2 The capacity performance of the nominal capacity during cycling. Fig.23, the horizontal axis 2301 represents the number of cycles, and the vertical axis 2303 corresponds to the actual capacity at the end of the corresponding cycle charge, in mAh. Curve 2305 corresponds to Example 3, curve 2307 corresponds to Comparative Example GG, and curve 2309 corresponds to Comparative Example HH. As shown, Example 3 (curve 1705) does not show any irregularities and has a final actual capacity (after 60 cycles) substantially the same as the nominal area capacity after 60 cycles. This shows that under these test conditions, the embodiment can maintain 80% or more, 85% or more, 90% or more, 95% or more and / or 98% or more of the initial capacity after 60 or more cycles. In contrast, Comparative Example FF (curve 2307) begins to show significant irregularities around 7 cycles and eventually fails around 15 cycles. Comparative Example GG (curve 2309) begins to show significant irregularities around 8 cycles and eventually fails around 20 cycles. Example 3 and Comparative Example GG have the same surface roughness Ra of the first main surface, and Example 3 and Comparative Example HH have the same surface roughness Ra of the second main surface. Fig.23 The results in Table 3 show that the cycle stability and / or capacity retention are unexpectedly increased by the combination of a low surface roughness Ra (e.g., about 0.6 μm or less) of the first major surface and a high surface roughness Ra (e.g., about 1 μm or greater) of the second major surface.

[0178] Table 4 shows the properties of Example 4 and Comparative Example II-KK. Example 4 and Comparative Example II-KK are the same as Example 2 and Comparative Example EE-GG, except that the anode is lithium metal instead of a lithium alloy. The lithium metal anode was heated for 5 minutes at the temperature shown in Table 4. Visual inspection of Comparative Example JJ-KK showed that the lithium metal at 300°C did not completely wet the first major surface of the solid electrolyte like the metal alloy at 300°C (e.g., Comparative Example FF-GG). However, visual inspection of Example 4 and Comparative Example II showed that the lithium metal at 330°C wetted the first major surface of the solid electrolyte more completely than the lithium metal at 300°C in Comparative Example JJ-KK.

[0179] Table 4: Properties of Example 4 and Comparative Examples II-KK with Lithium Metal Anode

[0180]

[0181] * = Examples that can withstand all tested charging current densities

[0182] Figure 24-27 The capacitance-voltage (CV) curves of Example 4 and Comparative Example II-KK are shown respectively. Figure 24-27For all cycles, the battery was discharged at 0.5C at 25°C while the charge current density (or charge rate) was varied to 1 mAh / cm 2 As with Example 2 and Comparative Examples DD-FF, for Example 4 and Comparative Examples II-KK, the charge current density was initially 0.4 mA / cm 2 (0.4C), increase 0.2mA / cm every 10 cycles 2 (0.2C), and for simplicity, the last cycle is a given charging current density (until failure), such as Figure 24-27 The maximum charge rate is 1.6C. Figure 24-27 In the figure, the horizontal axis 2401 corresponds to mAh / cm 2 The vertical axis 2403 corresponds to the instantaneous capacity in units of volts (V). Fig.24 , curves 2405, 2407, 2409, 2411, 2413, 2415 and 2417 correspond to discharge curves at 0.5 C as part of a cycle of charging at 0.4 C, 0.6 C, 0.8 C, 1 C, 1.2 C, 1.4 C and 1.6 C, respectively. Curve 2423 corresponds to overlapping charge curves up to 1.6 C. Fig.24 All curves in (including 1.6C) look normal. Fig.25 , curves 2505, 2507, 2509, and 2511 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.4C, 0.6C, 0.8C, and 1C, respectively. Curve 2523 corresponds to overlapping charge curves for charging at 0.4C, 0.6C, and 0.8C, and curve 2525 corresponds to a charge curve for charging at 1C. Discharge curve 2511 shows irregularities, while charge curve 2525 indicates that a short circuit has occurred. Compare Figure 24-25 , a battery with a lithium metal anode heated at 330°C exhibits the same relationship between the surface roughness Ra of the second major surface as a battery with a lithium alloy anode (i.e., a second major surface with a higher roughness (1 micron or greater) is superior to a second major surface with a lower roughness (0.6 μm or less)).

[0183] Figure 26-27 The capacitance-voltage (CV) curves of comparative examples JJ-KK are shown respectively. Fig.26In FIG. 2 , curves 2605, 2607, and 2609 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.4C, 0.6C, and 0.8C, respectively. Curves 2623, 2625, and 2627 correspond to charge curves at 0.4C, 0.6C, and 0.8C, respectively. Curve 2609 shows irregularities, while curve 2627 indicates that a short circuit occurred at 0.8C. Fig. 27 In the embodiment, curves 2705, 2707, 2709 and 2711 correspond to discharge curves at 0.5C as part of a cycle of charging at 0.4C, 0.6C, 0.8C and 1C, respectively. Curve 2723 corresponds to overlapping charging curves charged at 0.4C, 0.6C and 0.8C, and curve 2725 corresponds to a charging curve at 1C. Discharge curve 2711 shows irregularities, while charging curve 2725 indicates a decrease in charge capacity at 1C. Comparing Example 4 and Comparative Example II with Comparative Examples JJ-KK, heating lithium metal at 330°C enables the battery to withstand a higher charging rate than the battery in which lithium metal is heated at 300°C, which can be attributed to the reduced wettability of lithium metal on the solid electrolyte at 300°C. Therefore, according to the present disclosure, heating the lithium metal anode at a temperature above 300°C (e.g., 330°C or higher) is critical to achieving improved performance of the battery (which is not the case with the lithium alloy anode).

[0184] The above observations can be combined to provide a solid electrolyte, a battery and a method for manufacturing the same, which includes one or more surfaces of a solid electrolyte having a predetermined surface roughness Ra. The surface roughness Ra of the first major surface (e.g., facing the anode) of the solid electrolyte can be about 0.6 μm or less (e.g., about 0.1 μm to about 0.5 μm), which can increase the charging rate that the battery can withstand. The surface roughness of the second major surface (e.g., facing the cathode) of the solid electrolyte can be about 1 μm or greater (e.g., about 1.2 μm to about 3 μm), which can reduce the interfacial resistance of the battery. The low surface roughness Ra of the first major surface (e.g., about 0.6 μm or less or about 0.1 μm to about 0.5 μm) is further combined with the high surface roughness Ra of the second major surface (e.g., about 1 μm or greater or about 1.2 μm to about 3 μm), which can unexpectedly increase the life of the battery and / or the capacity retention rate of the battery and as demonstrated in the embodiments herein. Without wishing to be bound by theory, it is believed that a low roughness of the first major surface (e.g., about 0.6 μm or less or about 0.1 μm to about 0.5 μm) increases the charging rate by providing a substantially uniform surface for the anode, which enables uniform contact with the anode, reduces current concentration on the surface, and / or reduces the formation of dendrites. Without wishing to be bound by theory, it is believed that a high roughness of the second major surface (e.g., about 1 μm or more or about 1.2 μm to about 3 μm) reduces the interface resistance by increasing the surface area of ​​the interface between the solid electrolyte and the liquid electrolyte.

[0185] The method of the present disclosure includes polishing the first main surface and / or the second main surface to achieve a predetermined surface roughness Ra. Polishing may include etching, mechanical polishing, or a combination thereof. Without wishing to be bound by theory, etching for a short time (e.g., about 4 minutes or less) can reduce surface irregularities without increasing the surface roughness of the first main surface (e.g., by etching the grain boundaries of the solid electrolyte). Without wishing to be bound by theory, etching for a short time (e.g., about 4 minutes or less) can reduce surface irregularities without increasing the surface roughness of the first main surface (e.g., by etching the grain boundaries of the solid electrolyte). Without wishing to be bound by theory, etching for a longer period of time (e.g., about 7 minutes or more) can increase the surface roughness of the second main surface, such as by etching the grain boundaries of the solid electrolyte and / or leaching a portion of the solid electrolyte. A high mesh number (or low median particle size) abrasive for mechanically polishing the first main surface can produce a low surface roughness of the first main surface.

[0186] The method and battery may include a lithium-containing anode. In one aspect, the lithium-containing anode may be a lithium alloy, which may increase the wettability of the lithium-containing material on the first major surface of the solid electrolyte, which enables the battery to withstand high charging rates even when the lithium alloy is heated at 300°C and above. In one aspect, the lithium-containing anode may consist essentially of lithium metal. The method of the present disclosure includes heating the lithium metal at a temperature of about 330°C or above, which may wet or otherwise conform the lithium metal to the first major surface, which unexpectedly improves the charging rate that the battery can withstand, as demonstrated in the embodiments of the present invention, for example, by providing close and / or uniform contact between the lithium metal anode and the first major surface of the solid electrolyte.

[0187] Providing a solid electrolyte (e.g., in a solid-state battery) can address common safety issues, such as leakage, poor chemical stability, and flammability, that are common in batteries using liquid electrolytes. In addition, providing a solid-state electrolyte can also inhibit the shuttling of polysulfides from the cathode to the anode, resulting in improved electrode (e.g., anode, cathode) utilization and high discharge capacity and energy density. Providing a solid-state electrolyte can reduce the formation of dendrites (e.g., lithium dendrites) that would otherwise cause the battery to fail. Providing an intermediate layer comprising a liquid electrolyte can wet the interface between the cathode and the solid-state electrolyte, thereby reducing the interfacial resistance therebetween while minimizing the total amount of liquid electrolyte in the solid-state battery.

[0188] Directional terms used herein—eg, up, down, right, left, front, back, top, bottom—are used only with reference to the drawings in which they are drawn and are not intended to imply an absolute orientation.

[0189] It should be understood that the various aspects of the disclosure may relate to the features, elements or steps described in association with the aspect. It should also be understood that, although described in a form associated with one aspect, the features, elements or steps may be interchanged or combined with alternative aspects in various combinations or arrangements not illustrated.

[0190] It should also be understood that the terms "the," "a," or "an" as used herein mean "at least one," and should not be limited to "only one," unless clearly indicated to the contrary. For example, reference to a "component" includes aspects having two or more such components, unless the context clearly indicates otherwise. Likewise, "plurality" is intended to mean "more than one."

[0191] As used herein, the term "about" refers to that the amount, size, formula, parameter and other quantity and feature are not precise and need not be precise, but can be approximate and / or larger or smaller as needed, reflecting tolerances, conversion factors, rounding, measurement errors, etc., and other factors known to those skilled in the art. Herein, the range can be expressed as from "about" one specific value and / or to "about" another specific value. When such a range is stated, aspects include from the specific value and / or to the other specific value. Similarly, when the numerical value is indicated as an approximate value by using the antecedent "about", it should be understood that the specific value constitutes another aspect. Regardless of whether the numerical value or endpoint of the range in the specification is listed using "about", the numerical value or endpoint of the range is intended to include two aspects: one is modified with "about" and the other is not modified with "about". It should also be understood that the endpoint of each range is important when it is related to another endpoint and independent of another endpoint.

[0192] As used herein, the terms "substantially," "substantially," and variations thereof are intended to mean that the feature being described is equal to or approximately equal to the value being described. For example, a "substantially flat" surface is intended to mean that the surface is flat or approximately flat. Additionally, as defined above, "substantially similar" is intended to mean that two values ​​are equal or approximately equal. In aspects, "substantially similar" can mean values ​​that are within about 10% of each other, e.g., within about 5% of each other, or within about 2% of each other.

[0193] Unless otherwise stated, it is not intended that any method described herein be construed as requiring that its steps be performed in a specific order. Therefore, if a method claim does not actually state the order in which its steps are to be followed, or if the steps are not specifically indicated in any other way in the claims or description as being limited to a specific order, it is by no means intended to imply any specific order.

[0194] Although the transition phrase "comprising" may be used to disclose various features, elements, or steps of a particular aspect, it should be understood that it implicitly includes those alternative aspects that may be described using the transition phrases "consisting of" or "consisting essentially of. Thus, for example, implicit alternative aspects of a device comprising A+B+C include aspects wherein the device consists of A+B+C and aspects wherein the device consists essentially of A+B+C.

[0195] The above aspects and features of those aspects are exemplary and may be provided alone or in any combination with any one or more features of the other aspects provided herein without departing from the scope of the present disclosure.

[0196] It is obvious to those skilled in the art that various modifications and changes can be made to the present disclosure without departing from the scope of the present disclosure. Therefore, the present disclosure is intended to cover modifications and changes of the aspects described herein, as long as these modifications and changes are within the scope of the appended claims and their equivalents.

Claims

1. A battery, include: A lithium-containing anode; A solid electrolyte comprising a first major surface facing a lithium-containing anode and a second major surface opposite the first major surface, the first major surface comprising a surface roughness Ra of 0.6 micrometers or less, and the second major surface comprising a surface roughness of 1 micrometer or more; a liquid electrolyte disposed on the second major surface of the solid electrolyte; and A cathode is disposed over the second major surface of the solid electrolyte, with the liquid electrolyte located between the second major surface and the cathode.

2. The battery according to claim 1, in, The surface roughness Ra of the first main surface is in the range of 0.1 micrometer to 0.5 micrometer.

3. The battery according to claim 1, in, The surface roughness Ra of the second main surface is in the range of 1.2 micrometers to 3 micrometers.

4. The battery according to claim 1, in, At 25°C, the interfacial resistance between the cathode and the lithium-containing anode is 60 Ωcm 2 or smaller.

5. The battery according to claim 1, in, The interfacial resistance of the battery is 50% or less of the interfacial resistance of another battery that is identical to the battery except that the first major surface and the second major surface are interchanged.

6. The battery according to any one of claims 1 to 5, in, The battery can withstand at least 10 cycles at 25°C with 1.6 mA / cm 2 or greater charging current density up to 1 mAh / cm 2 The capacity is 0.5 mA / cm 2 The discharge rate is the discharge cycle, where the area is based on the surface area of ​​the lithium-containing anode.

7. The battery according to claim 6, in, Another battery identical to the battery except that the first major surface and the second major surface are interchanged cannot withstand 10 cycles of 1.25 mA / cm2 at 25°C. 2 The charging current density is charged to 1 mAh / cm 2 The capacity is 0.5 mA / cm 2 The discharge rate is the discharge cycle.

8. The battery according to any one of claims 1 to 5, in, The battery was charged at a rate of 0.5C and discharged at a rate of 0.17C to 3 mAh / cm at a cut-off voltage of 4.5V and 60°C. 2 The maximum capacity after 60 cycles includes a capacity retention rate of 90% or higher, and the area is based on the surface area of ​​the lithium-containing anode.

9. The battery according to any one of claims 1-5, wherein the cathode comprises at least one of the following: lithium cobalt oxide (LCO), lithium manganese spinel (LMO), lithium nickel cobalt aluminate (NCA), lithium nickel manganese cobalt oxide (NCM) (LiNi d Co e Mn 1-d- e O 2 , where 0 < d < 1, 0 < e < 1), lithium iron phosphate (LiFePO 4 )(LFP), lithium cobalt phosphate (LCP), lithium titanate, lithium niobium tungstate, lithium nickel manganate, and lithium titanium sulfide (LiTiS 2 ) or a combination thereof.

10. The battery of any one of claims 1 to 5, wherein the solid electrolyte comprises at least one of: (i) Li 7-3a La 3 Zr 2 L a O 12 , in which L=Al, Ga or Fe and 0 <a<0.33; (ii) Li 7 La 3-b Zr 2 M b O 12 , where M=Bi or Y and 0 <b<1; (iii) Li 7-c La 3 (Zr 2-c ,N c )O 12 , where N=In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 <c<1; (iv) Protonated LLZO (e.g., H x Li 6.5-x La 3 Zr 1.5 I 0.5 O 12 , where I = In, Si, Ge, Sn, V, W, Te, Nb or Ta and 0 < x < 4, or H x Li 6.25-x E 0.25 La 3 Zr 2 O 12 , where E = Al, Ga or Fe and 0 < x < 4); or A combination of them.

11. A method of forming a battery, wherein include: polishing the first main surface of the solid electrolyte to form a surface roughness Ra of 0.6 micrometers or less; polishing a second main surface of the solid electrolyte to form a surface roughness Ra of 1 micrometer or more, the second main surface being opposite to the first main surface; heating the lithium-containing precursor to a temperature of 300° C. or greater to form a lithium-containing anode disposed on the first major surface; and A solid electrolyte is disposed above the cathode with a second major surface of the solid electrolyte facing the cathode.

12. The method of claim 11, wherein heating the lithium-containing precursor comprises heating it to a temperature of 330°C to 400°C for 5 minutes to 10 minutes, and the lithium-containing anode consists essentially of lithium metal.

13. The method of claim 11, wherein polishing the first major surface comprises mechanical polishing using a grit of 1000 or greater.

14. The method of any one of claims 11-13, wherein polishing the second major surface comprises mechanical polishing using a grit of 600 or less.

15. The method of any one of claims 11-13, wherein polishing the first major surface comprises etching in an acidic solution comprising a concentration of 0.1 molar to 3 molar for 4 minutes or less.

16. The method of any one of claims 11-13, wherein polishing the second major surface comprises etching in an acidic solution comprising a concentration of 0.1 molar to 3 molar for 7 minutes to 30 minutes.

17. The method of any one of claims 11-13, further comprising disposing a liquid electrolyte on the cathode such that the liquid electrolyte is between the cathode and the second major surface, the liquid electrolyte comprising a lithium-containing salt.

18. The method according to any one of claims 11 to 13, in, The surface roughness Ra of the first main surface is in the range of 0.1 micrometer to 0.5 micrometer.

19. The method of any one of claims 11 to 13, wherein the surface roughness Ra of the second major surface is in the range of 1.2 microns to 3 microns.

20. The battery according to any one of claims 11 to 13, in, The interfacial resistance of the battery is 50% or less of the interfacial resistance of another battery that is identical to the battery except that the first major surface and the second major surface are interchanged.