Indium-based oxyhalide solid electrolyte and preparation method and application thereof

By doping oxygen elements and using aqueous phase synthesis and specific atmosphere heat treatment, an indium-based oxyhalide solid electrolyte with high stability and high conductivity is prepared, which solves the problems of electrolyte safety hazards and material stability in lithium-ion batteries. , realizing the application prospects of all-solid-state batteries.

CN118782891APending Publication Date: 2024-10-15CHINA AUTOMOTIVE INNOVATION CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410748013.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The organic electrolytes used in existing lithium-ion batteries have safety risks, and halide solid electrolyte materials such as Li3InCl6 are easy to absorb water and are unstable to solvents and binders, which limits their application in all-solid-state batteries.

Method used

By doping oxygen elements, an indium-based oxyhalide solid electrolyte Li3InOxCl6-2x with high air stability, solvent stability and binder stability was prepared. The aqueous phase synthesis method and specific atmosphere heat treatment method were used to improve the electrolyte's stability. performance.

Benefits of technology

An indium-based oxyhalide solid electrolyte with high conductivity and good stability has been realized, which overcomes the problems of easy water absorption and unstable solvent binder, simplifies the production process of all-solid-state lithium secondary batteries, and expands its application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782891A_ABST
    Figure CN118782891A_ABST
Patent Text Reader

Abstract

The invention provides an indium-based oxyhalide solid electrolyte and a preparation method and application thereof.The indium-based oxyhalide solid electrolyte has the composition shown as Li3InOxCl6-2x, x is larger than 0 and smaller than 3, and the preparation method of the indium-based oxyhalide solid electrolyte comprises the steps that indium chloride tetrahydrate and lithium chloride are dissolved in deionized water and then dried to obtain precursor powder; and carrying out heat treatment on the precursor powder for 2-5 hours at the temperature of 400-600 DEG C in an anhydrous aerobic atmosphere. The novel oxygen-doped indium-based halide solid electrolyte Li3InOxCl6-2x with high conductivity, high air stability and high solvent and binder stability is simply synthesized by adopting a water-phase synthesis method assisted by heat treatment under specific conditions, the operation is convenient, the cost is low, the use of the halide solid electrolyte material in wet coating can be further realized, and the application prospect is wide. The production process of the all-solid-state lithium secondary battery is simplified, and the method is expected to have a certain application prospect in the field of all-solid-state batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to an indium-based oxyhalide solid electrolyte and a preparation method and application thereof. Background Art

[0002] Since its commercialization, lithium-ion secondary batteries have developed rapidly due to their advantages such as high energy density and long service life. However, the lithium-ion batteries commonly used at present contain flammable organic electrolytes, so there are serious safety hazards. In recent years, the frequent occurrence of safety accidents in liquid-phase lithium-ion power batteries has greatly restricted the further use of this system. The use of non-flammable inorganic solid materials as lithium-ion battery electrolytes can not only eliminate the safety hazards caused by organic electrolyte leakage and internal thermal runaway of the battery during the use of the battery, but also can be used under extreme conditions such as high temperature and low temperature, further enhancing the value of lithium secondary batteries and expanding their application areas. Therefore, the research and development of inorganic solid electrolytes with high stability and high lithium ion conductivity is the key to the development of lithium secondary batteries with high safety.

[0003] The halide solid electrolytes developed in recent years are considered to be one of the most promising candidate materials for all-solid-state batteries. Compared with oxide solid electrolytes, halide solid electrolytes are relatively light (the density of Li3InCl6 is 2.69 g cm -3 ;Li7La3Zr2O 12 The density is 5.01 g cm -3 ). In addition, oxide solid electrolytes require high-temperature sintering (>1000°C), while halide solid electrolytes can be sintered at low temperatures (<500°C), showing better mechanical flexibility. Compared with sulfide solid electrolytes, the radius of monovalent halogen ions is larger than that of divalent sulfur elements, and the interaction force with lithium ions is weak, which makes the lithium ion mobility of halide solid electrolytes high, the deformability is strong, and the mechanical softness is strong; in addition, the electrochemical window of halide solid electrolytes is wide, which can match the high-voltage positive electrode.

[0004] Among them, halide electrolyte materials such as Li3YCl6 and Li3InCl6 have a wide voltage window, are stable with high-voltage positive electrodes, can be operated in a dry room, and are relatively soft and easy to shape and process, which are expected to be further applied in the industry. However, Li3InCl6 materials have disadvantages such as being extremely easy to absorb water and moisture, and being unstable to solvents and binders, which will have a greater impact on production processes such as wet coating. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides an indium-based oxyhalide solid electrolyte and a preparation method and application thereof. By doping oxygen element, a solid electrolyte with good air stability, solvent stability, binder stability and high conductivity is obtained, providing technical support for all-solid-state batteries.

[0006] In a first aspect, the present invention provides an indium-based oxyhalide solid electrolyte having Li3InO x Cl 6-2x In the composition shown, 0<x<3, more preferably 1<x<2.

[0007] In the chemical formula of the indium-based oxyhalide solid electrolyte of the present invention, x represents the proportion or content of the oxygen element. In the present invention, x is a range and can be derived from the XRD spectrum.

[0008] The present invention makes the hygroscopic halide solid electrolyte have good air stability by doping with oxygen elements, and the obtained indium-based oxyhalide solid electrolyte Li3InO x Cl 6-2x It has the advantages of high solvent and binder stability that general indium-based halide electrolytes do not have. The indium-based oxyhalide solid electrolyte of the present invention can overcome the defects of the existing Li3InCl6 material that is difficult to use in all-solid-state battery wet coating processes due to its easy water absorption and instability to solvents and binders, and has certain application prospects in the field of all-solid-state batteries.

[0009] In some embodiments of the present invention, the XRD characteristic peaks of the indium-based oxyhalide solid electrolyte are three strong peaks, specifically (001) peak 10.9°±0.2°, (003) peak 33.4°±0.2° and (004) peak 44.7°±0.2°. These characteristic peaks can help understand the crystal structure, chemical composition, etc. of the indium-based oxyhalide solid electrolyte.

[0010] In one embodiment of the present invention, the X-ray diffraction pattern of the indium-based oxyhalide solid electrolyte is as follows: Figure 1 shown.

[0011] The indium-based oxyhalide solid electrolyte of the present invention has solvent stability and binder stability. The solvent stability includes stability to isobutyl isobutyrate, xylene, dodecane, n-butyl ether and anisole. The binder stability includes stability to polyisobutylene and hydrogenated styrene-butadiene block copolymer.

[0012] It should be noted that the stability of the binder of the present invention can also be referred to as solvent binder stability. Because the binder itself is solid and the electrolyte is also solid and cannot be dissolved, the present invention first verifies whether the electrolyte powder is stable with the solvent during the experiment, and then verifies the corresponding binder stability based on the stability of the solvent (according to the stable solvent, the corresponding glue is prepared, and the glue is a uniform solution of a certain viscosity obtained by dissolving the binder in the solvent). Specifically, in the embodiment of the present invention, when judging whether the binder polyisobutylene and hydrogenated styrene-butadiene block copolymer are stable, the solvents used are xylene and dodecane, respectively. As a result, the two binders are stable under the condition that the solvents are selected from xylene and dodecane, respectively.

[0013] The ionic conductivity of the indium-based oxyhalide solid electrolyte of the present invention is not less than 1.4 mS / cm. Further, in some preferred embodiments of the present invention, the ionic conductivity of the indium-based oxyhalide solid electrolyte is not less than 1.8 mS / cm, and under preferred conditions, it can even reach 2.1 mS / cm.

[0014] The ionic conductivity of solid electrolytes is one of the key parameters for measuring their performance in solid-state batteries. The level of ionic conductivity directly affects the battery's charge and discharge performance, power density, and cycle stability. The present invention can achieve high ionic conductivity while ensuring high air stability, high solvent and binder stability, which is very beneficial for its application in all-solid-state batteries.

[0015] In a second aspect, the present invention provides a method for preparing an indium-based oxyhalide solid electrolyte.

[0016] The preparation method provided by the present invention comprises:

[0017] After dissolving indium trichloride tetrahydrate and lithium chloride in deionized water, the precursor powder is obtained by drying;

[0018] In an anhydrous oxygen atmosphere, the precursor powder is heat treated at 400-600° C. for 2-5 hours.

[0019] The heat treatment conditions may be any value within the above range, for example, heat treatment at 400°C for 2 hours, heat treatment at 400°C for 5 hours, heat treatment at 400°C for 4 hours, heat treatment at 500°C for 2 hours, heat treatment at 500°C for 3 hours, heat treatment at 500°C for 4 hours, heat treatment at 600°C for 2 hours, and heat treatment at 600°C for 3 hours.

[0020] The present invention adopts an aqueous phase synthesis method supplemented by heat treatment under specific conditions to simply synthesize a new type of oxygen-doped indium-based halide solid electrolyte Li3InO with high conductivity, high air stability, high solvent and binder stability. x Cl 6-2x , easy to operate and low cost.

[0021] It should be noted that the first step of drying in the present invention is to obtain the precursor powder, which serves to remove most of the bound water in the precursor powder, and the second step of heat treatment is to remove the bound water between the electrolyte materials.

[0022] In some embodiments of the present invention, the anhydrous oxygen atmosphere uses compressed air or a nitrogen-oxygen mixture, and the volume ratio of nitrogen to oxygen in the nitrogen-oxygen mixture is 8:2 to 4:6.

[0023] The atmosphere conditions of the heat treatment of the present invention are critical. It cannot be conventional vacuum or inert gas (such as nitrogen, argon, helium), and must contain oxygen and be anhydrous. In particular, oxygen can be present but the oxygen content cannot be too high. If the oxygen content exceeds 60%, or even reaches 100% (in the case of pure oxygen), the solvent stability of the obtained electrolyte is not ideal. Considering the cost issue, compressed air is preferably used.

[0024] In a preferred embodiment of the present invention, the precursor powder is heat treated at 400-500° C. for 2-3 hours in a compressed air atmosphere.

[0025] Different heat treatment temperatures and times will affect the performance of the resulting electrolyte. If it is not within the above-mentioned 400-600°C heat treatment range for 2-5 hours of the present invention, the stability of the resulting electrolyte solvent binder is poor. If it is within the above-mentioned 400-600°C heat treatment range for 2-5 hours of the present invention, but not the preferred conditions of 400-500°C heat treatment for 2-3 hours, the ionic conductivity and air stability of the resulting electrolyte will be poor.

[0026] In some embodiments of the present invention, the molar ratio of the tetrahydrated indium trichloride to the lithium chloride is 1:3. The present invention has tried operating conditions with 1%, 2% and 5% excess lithium chloride, but the results are worse than the experimental data of the standard 1:3 molar ratio.

[0027] In a third aspect, the present invention provides a lithium-ion secondary battery comprising a positive electrode, a negative electrode and a solid electrolyte layer between the positive electrode and the negative electrode, wherein the solid electrolyte layer comprises the above-mentioned indium-based oxyhalide solid electrolyte.

[0028] It is understood that the solid electrolyte layer may include other electrolytes other than the above-mentioned indium-based oxyhalide solid electrolyte in addition to the above-mentioned indium-based oxyhalide solid electrolyte. Other solid electrolytes refer to solid electrolytes that can move ions inside them. As solid electrolytes, inorganic solid electrolytes are preferred. Since inorganic solid electrolytes are generally solid in a stable state, they are usually not dissociated or freed into cations and anions. As other solid electrolytes. Sulfide-based inorganic solid electrolytes, oxide-based inorganic solid electrolytes, halide-based inorganic solid electrolytes, and hydride-based solid electrolytes can be cited.

[0029] When the solid electrolyte layer includes other electrolytes in addition to the above-mentioned indium-based oxyhalide solid electrolyte, the content of the indium-based oxyhalide solid electrolyte is not particularly limited. Preferably, the content of the indium-based oxyhalide solid electrolyte accounts for more than 50% of the total mass of the solid electrolyte layer, more preferably more than 90%. The upper limit is not limited and can reach 100%.

[0030] In addition to the solid electrolyte, the solid electrolyte layer may also include auxiliary components such as a binder and a dispersion medium. The selection and content of the binder and the dispersion medium are not particularly limited, and those skilled in the art may select them according to their needs.

[0031] In the present invention, the method for forming the solid electrolyte layer is not particularly limited, and the method can be applied by coating followed by drying. The coating method is not particularly limited, and both wet coating and dry coating are possible.

[0032] Wet coating is a coating method that uses liquid coatings or solutions. In this method, the coating material is applied to the substrate in liquid form, and then the solvent is removed by evaporation or other means to leave a solid coating. Wet coating includes but is not limited to the following methods: spray coating, spin coating, dip coating, and shower coating. Dry coating is a coating method that does not use solvents or other carrier liquids. The coating material is usually applied directly to the substrate in powder, granular or other dry form, and then cured by heat treatment or other methods. Dry coating includes: powder coating, dry screen printing, etc.

[0033] Since the indium-based oxyhalide solid electrolyte of the present invention has high air stability, high solvent and binder stability, wet coating can be used. The coating formula of wet coating is flexible, and the viscosity and performance of the coating can be adjusted as needed. In addition, wet coating is suitable for substrates of various shapes and sizes, and a thicker coating can be applied, so the application range is wider and the practical operation is easier.

[0034] It is understood that after the solid electrolyte layer is formed by coating, the coating needs to be dried. The drying temperature is not particularly limited, but is preferably above 30°C, and more preferably 60-200°C.

[0035] In the present invention, the positive electrode preferably includes a positive electrode current collector and an active material layer formed on the positive electrode current collector.

[0036] In some preferred embodiments of the present invention, the positive electrode has an active material layer, and the active material layer includes the above-mentioned indium-based oxyhalide solid electrolyte.

[0037] Specifically, the positive electrode active material layer includes a positive electrode active material and the above-mentioned indium-based oxyhalide solid electrolyte. The positive electrode active material is preferably capable of reversibly inserting or releasing lithium ions and the like, and a transition metal oxide is further preferred. Exemplarily, it can be a transition metal oxide having a layered rock salt structure, a transition metal oxide having a spinel structure, a lithium-containing transition metal phosphate compound, a lithium-containing transition metal halide phosphate compound, or a lithium-containing transition metal silicate compound. For example, lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese cobalt oxide, etc.

[0038] In the present invention, the negative electrode preferably includes a negative electrode current collector and an active material layer formed on the negative electrode current collector.

[0039] In some preferred embodiments of the present invention, the negative electrode has an active material layer, and the active material layer includes the above-mentioned indium-based oxyhalide solid electrolyte.

[0040] Specifically, the negative electrode active material layer includes a negative electrode active material and the above-mentioned indium-based oxyhalide solid electrolyte. The negative electrode active material is preferably capable of reversibly inserting or releasing lithium ions and the like. Exemplarily but not restrictively, carbonaceous materials, oxides of metals or metalloid elements, lithium monomers, lithium alloys, and negative electrode active materials capable of forming alloys with lithium. Among them, the carbonaceous material used as the negative electrode active material refers to a material substantially composed of carbon, for example, it can be a carbonaceous material calcined by various synthetic resins such as petroleum asphalt, acetylene black and other carbon blacks, graphite and polyacrylonitrile resins. Metalloid elements refer to elements that show properties intermediate between metal elements and non-metallic elements, and generally include boron, silicon, germanium, arsenic, antimony and tellurium, and also include selenium, polonium and astatine. The negative electrode active material can be used alone or as a mixture of multiple types.

[0041] It is well known in the art that the active material layer may include one or more of a conductive aid, a binder, and a dispersion medium in addition to the active material and the above-mentioned indium-based oxyhalide solid electrolyte. The conductive aid may be a commonly used conductive aid known in the art, such as graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black and Ketjen black, and carbonaceous materials such as graphene and fullerene. The binder and the dispersion medium may also be commonly used substances in the art, which will not be described here.

[0042] The lithium ion secondary battery obtained by the present invention is preferably an all-solid-state lithium secondary battery, which can be used in various applications, such as laptop computers, mobile phones, electric shavers, calculators, cars, electric vehicles, lighting equipment, toys, game consoles, cameras and other equipment.

[0043] The present invention provides an indium-based oxyhalide solid electrolyte and a preparation method and application thereof. Compared with the poor air stability and initial instability to solvents and binders of Li3InCl6, the present invention uses an aqueous phase synthesis method supplemented by a specific atmosphere heat treatment to simply synthesize a novel oxygen-doped indium-based halide solid electrolyte Li3InO with high electrical conductivity, high air stability, high solvent and binder stability. x Cl 6-2x It is easy to operate and low in cost. It can further realize the use of halide solid electrolyte materials in wet coating and simplify the production process of all-solid-state lithium secondary batteries. It is expected to have certain application prospects in the field of all-solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0045] Figure 1 is the XRD pattern of the product of Example 1 of the present invention;

[0046] Figure 2 This is the XRD diagram of the product of Comparative Example 1 of the present invention;

[0047] Figure 3 This is the EIS spectrum of the product of Example 1 of the present invention;

[0048] Figure 4 This is the EIS spectrum of the product of Comparative Example 1 of the present invention;

[0049] Figure 5 It is a SEM picture of the product of Example 1 of the present invention. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0052] In the following examples and comparative examples, the heat treatment with compressed air and special gases (nitrogen, argon, helium, oxygen, nitrogen-oxygen mixture) is free of water (the moisture content can be regarded as 0). Only in comparative example 2, which is connected to the outside air, water is present (because the outside air has a certain amount of humidity).

[0053] Example 1

[0054] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2.

[0055] This embodiment also provides a method for preparing the above-mentioned indium-based oxyhalide solid electrolyte, and the specific steps are as follows:

[0056] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce compressed air during the heat treatment to obtain the target product.

[0057] Example 2

[0058] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0059] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce nitrogen and oxygen mixed gas during the heat treatment process, with a nitrogen-oxygen ratio of 8:2, to obtain the target product.

[0060] Example 3

[0061] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0062] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce nitrogen and oxygen mixed gas during the heat treatment process, with a nitrogen-oxygen ratio of 6:4, to obtain the target product.

[0063] Example 4

[0064] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0065] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce nitrogen and oxygen mixed gas during the heat treatment process, with a nitrogen-oxygen ratio of 5:5, to obtain the target product.

[0066] Example 5

[0067] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0068] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce nitrogen and oxygen mixed gas during the heat treatment process, with a nitrogen-oxygen ratio of 4:6, to obtain the target product.

[0069] Example 6

[0070] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0071] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders in a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 600°C in an atmosphere furnace for 2h, and introduce compressed air during the heat treatment to obtain the target product.

[0072] Example 7

[0073] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0074] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders in a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 4 hours, and introduce compressed air during the heat treatment to obtain the target product.

[0075] Example 8

[0076] This embodiment provides an indium-based oxyhalide solid electrolyte, the composition of which is Li3InO x Cl 6-2x , 1<x<2, and the preparation method is as follows:

[0077] In a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 500°C in an atmosphere furnace for 3h, and introduce compressed air during the heat treatment to obtain the target product.

[0078] Comparative Example 1

[0079] This comparative example provides a preparation method different from that of Example 1, the difference being that vacuum is applied during the heat treatment process.

[0080] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders in a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C for 2h in an atmosphere furnace, and evacuate during the heat treatment.

[0081] Comparative Example 2

[0082] This comparative example provides a preparation method different from that of Example 1, the difference being that the heat treatment process is connected to the outside air, that is, there is no gas protection and the heat treatment process is connected to the outside air.

[0083] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C for 2h in an atmosphere furnace, and connect to the outside air during the heat treatment.

[0084] Comparative Example 3

[0085] This comparative example provides a preparation method different from that of Example 1, the difference being that nitrogen is introduced during the heat treatment process.

[0086] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce nitrogen during the heat treatment.

[0087] Comparative Example 4

[0088] This comparative example provides a preparation method different from that of Example 1, the difference being that argon gas is introduced during the heat treatment process.

[0089] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce argon gas during the heat treatment.

[0090] Comparative Example 5

[0091] This comparative example provides a preparation method different from that of Example 1, the difference being that helium is introduced during the heat treatment process.

[0092] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce helium during the heat treatment.

[0093] Comparative Example 6

[0094] This comparative example provides a preparation method different from that of Example 1, the difference being that oxygen is introduced during the heat treatment process.

[0095] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce oxygen during the heat treatment process.

[0096] Comparative Example 7

[0097] This comparative example provides a preparation method different from that of Example 1, the difference being that a nitrogen-oxygen mixed gas is introduced during the heat treatment process, and the ratio of nitrogen to oxygen is 2:8.

[0098] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add an appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 2h, and introduce nitrogen and oxygen mixed gas during the heat treatment process, with a nitrogen to oxygen ratio of 2:8.

[0099] Comparative Example 8

[0100] This comparative example provides a preparation method different from that of Example 1, the difference being that the heat treatment temperature is 200°C.

[0101] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 200°C for 2h in an atmosphere furnace, and introduce compressed air during the heat treatment.

[0102] Comparative Example 9

[0103] This comparative example provides a preparation method different from that of Example 1, the difference being that the heat treatment time is 1 h.

[0104] The specific steps are as follows: in a nitrogen glove box, weigh indium trichloride tetrahydrate and lithium chloride powders at a molar ratio of 1:3, transfer to a fume hood, add appropriate amount of deionized water to completely dissolve, and then collect the white precursor powder by rotary drying at 120°C. Heat treat at 400°C in an atmosphere furnace for 1h, and introduce compressed air during the heat treatment.

[0105] Performance Testing

[0106] The solid electrolytes obtained in each embodiment and comparative example were subjected to performance tests, and the specific test items and methods are as follows:

[0107] a. Ionic conductivity test of halide solid electrolyte:

[0108] The Swiss Metrohm PGSTAT302 electrochemical workstation was used, with a test frequency range of 10MHz-1Hz and a bias voltage of 10mV. During the test, 200mg of powder was weighed and pressed into sheets at 350MPa using a φ10mm mold, with stainless steel as the blocking electrode. The ionic conductivity was calculated according to the conductivity calculation formula σ=L / (R*S) (L is the thickness of the sample, R is the total impedance, and S is the effective area of ​​contact between the sample and the electrode).

[0109] b. Air stability test of halide solid electrolyte:

[0110] In a nitrogen glove box, weigh 300 mg of the halide solid electrolyte material and put it into a 5 ml open glass bottle. Then, place the glass bottle containing the halide solid electrolyte material in a reaction box with an air flow of 10% relative humidity and 100 ml / min, and let it stand at room temperature for 24 hours. After standing, take out the sample for ion conductivity test.

[0111] In the test results shown in Table 1, "original" refers to the sample "not treated in a reaction box with air flow", and "after 24h exposure" refers to the sample "treated in a reaction box with air flow". By comparing the ion conductivity of "after 24h exposure" and "original", the retention rate is obtained, which reflects the air stability. The higher the retention rate, the higher the air stability.

[0112] c. Solvent stability and binder stability test of halide solid electrolyte:

[0113] In a nitrogen glove box, weigh 1 g of a halide solid electrolyte material, dissolve it in 10 g of an organic solvent, and observe whether the halide solid electrolyte material is stable with the solvent (if there is no color change reaction within ten minutes of standing, it is judged to be stable).

[0114] In a nitrogen glove box, based on the organic solvent that is in a stable state after the above screening, a certain amount of binder is prepared and dissolved in the organic solvent, 1g of halide solid electrolyte material is added, and it is observed whether the halide solid electrolyte material is stable with the binder (if there is no color change reaction within ten minutes of standing, it is judged to be stable).

[0115] The test results are shown in Table 1.

[0116] Table 1

[0117]

[0118] Note: PIB: polyisobutylene; SEBS: hydrogenated styrene-butadiene block copolymer; PVDF: polyvinylidene fluoride; PAA: polyacrylic acid; PMMA: polymethyl methacrylate.

[0119] "PIB / SEBS-xylene / dodecane stable" means that the two binders can be arbitrarily matched with the two solvents, that is, PIB and xylene, PIB and dodecane, SEBS and xylene, SEBS and dodecane are all stable, and so on.

[0120] In addition, the XRD pattern of the product of Example 1 is as follows Figure 1 As shown; the XRD pattern of the product of Comparative Example 1 is as shown Figure 2 As shown; the EIS spectrum of the product of Example 1 is as shown Figure 3 As shown; the EIS spectrum of the product of Comparative Example 1 is as follows Figure 4As shown; the SEM picture of the product of Example 1 is as shown Figure 5 It can be seen that there is O element in the product of Example 1 of the present invention, so it is inferred that it is an oxygen-doped halide solid electrolyte Li3InO x Cl 6-2x , which has three strong peaks, (001) peak 10.9°, (003) peak 33.4° and (004) peak 44.7°. The XRD of Comparative Example 1 is basically consistent with the PDF standard card of Li3InCl6 (PDF#44-0287), that is, it has not been successfully doped with oxygen.

[0121] From the above results, it can be seen that the oxygen-doped indium-based halide solid electrolyte Li3InO can be obtained by heat treating the precursor in an anhydrous oxygen atmosphere. x Cl 6-2x , the electrolyte has excellent air stability and solvent and binder stability. Among them, the anhydrous oxygen atmosphere can use compressed air or nitrogen-oxygen mixed gas. When it is a nitrogen-oxygen mixed gas, the volume ratio of nitrogen and oxygen should be controlled in the range of 8:2 to 4:6, as shown in Examples 2-5. If the oxygen content is too high, or even pure oxygen conditions, the solvent stability of the resulting electrolyte is not ideal, as shown in Comparative Examples 6 and 7. If the oxygen content is too low, or even oxygen-free, and conventional inert gases such as nitrogen, argon, and helium are used, the ionic conductivity of the resulting electrolyte is low and the solvent stability is also not ideal, as shown in Comparative Examples 3-5. Comparative Example 1 synthesizes pure phase Li3InCl6 under vacuum conditions. Compared with Example 1, the conductivity, air stability, and solvent binder stabilizer of the material are all poor. Comparative Example 2 uses outside air. Due to the presence of moisture in the air, the performance of the synthesized material is extremely poor.

[0122] Compared with Example 1, Example 2 has similar performance, which is attributed to the fact that the ratio of nitrogen to oxygen in the compressed air is about 8:2, but the advantage of Example 1 lies in the low cost of compressed air and more convenient operation.

[0123] In the preparation method of the present invention, not only the atmosphere conditions of the heat treatment are critical, but also the temperature and time of the heat treatment affect the product performance. By comparing Example 1, Example 6, Example 7, Example 8 and Comparative Examples 8-9, it can be seen that the indium-based halide solid electrolyte Li3InO x Cl 6-2x The synthesis performance is optimal under the specific heat treatment temperature and insulation time conditions of the present invention.

[0124] In summary, the present invention uses an aqueous phase synthesis method supplemented by heat treatment under specific conditions to simply synthesize a new type of oxygen-doped indium-based halide solid electrolyte with high conductivity, high air stability, and high solvent binder stability. The operation is convenient and the cost is low. The use of halide solid electrolyte materials in wet coating can be further realized, and the production process of all-solid-state lithium secondary batteries is simplified. It is expected to have certain application prospects in the field of all-solid-state batteries.

[0125] It should be noted that the endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.

[0126] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "specific implementations", or "some specific implementations" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. Indium-based oxyhalide solid electrolyte, characterized in that: With Li3InO x Cl 6-2x The composition shown, wherein 0<x<3.

2. The indium-based oxyhalide solid electrolyte according to claim 1, characterized in that: 1<x<2。 3. The indium-based oxyhalide solid electrolyte according to claim 1, characterized in that: The XRD characteristic peaks of the indium-based oxyhalide solid electrolyte are three strong peaks, namely (001) peak 10.9°±0.2°, (003) peak 33.4°±0.2° and (004) peak 44.7°±0.2°.

4. A method for preparing an indium-based oxyhalide solid electrolyte, characterized in that: include: After dissolving indium trichloride tetrahydrate and lithium chloride in deionized water, the precursor powder is obtained by drying; In an anhydrous oxygen atmosphere, the precursor powder is heat treated at 400-600° C. for 2-5 hours.

5. The method for preparing an indium-based oxyhalide solid electrolyte according to claim 4, characterized in that: The anhydrous oxygen atmosphere is compressed air or a nitrogen-oxygen mixed gas, and the volume ratio of nitrogen to oxygen in the nitrogen-oxygen mixed gas is 8:2 to 4:

6.

6. The method for preparing an indium-based oxyhalide solid electrolyte according to claim 5, characterized in that: The precursor powder is heat treated at 400-500° C. for 2-3 hours in a compressed air atmosphere.

7. The method for preparing an indium-based oxyhalide solid electrolyte according to any one of claims 4 to 6, characterized in that: The molar ratio of the indium chloride tetrahydrate to the lithium chloride is 1:

3.

8. A lithium ion secondary battery, characterized in that It comprises a positive electrode, a negative electrode and a solid electrolyte layer between the positive electrode and the negative electrode, wherein the solid electrolyte layer comprises the indium-based oxyhalide solid electrolyte according to any one of claims 1 to 3.

9. The lithium ion secondary battery according to claim 8, characterized in that: The positive electrode and / or the negative electrode has an active material layer, and the active material layer includes the indium-based oxyhalide solid electrolyte according to any one of claims 1 to 3.

10. The lithium ion secondary battery according to claim 8 or 9, characterized in that: The lithium ion secondary battery is prepared by wet coating.