Low melting point glass

By controlling the Sn and Zn content of the glass and the surrounding structure of the OH group, the problem of crystallization and hygroscopicity of low-melting point glass after low-temperature molding is solved, achieving high transparency and gas barrier properties, and is suitable for a variety of molding processes.

CN118786100APending Publication Date: 2024-10-15AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380024345.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2023-02-24
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing low-melting point glass easily crystallizes after low-temperature molding, has poor transparency and unstable gas barrier properties, making it difficult to apply to resin molding processes.

Method used

By controlling the composition range of glass, especially the content of Sn and Zn, the surrounding structure of the OH group can be reasonably adjusted to reduce the glass transition temperature Tg, inhibit crystallization, and improve moisture absorption resistance.

Benefits of technology

It achieves excellent transparency and moisture absorption resistance of the glass after low-temperature molding, expands the molding temperature margin, is suitable for extrusion, injection, blow molding and other processes, and improves gas barrier properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017163010000221
    Figure BDA0005017163010000221
  • Figure HDA0005017163030000011
    Figure HDA0005017163030000011
  • Figure HDA0005017163030000021
    Figure HDA0005017163030000021
Patent Text Reader

Abstract

The present invention relates to a glass containing, in mol% of elements, 12-16% of P, 16-21% of Sn, 50-60% of O, 5-15% of F, 0-3% of Zn, 0-1% of Si, 0-1% of B, and 0-3% of Al, in which (Sn + Zn) / P is 1.25-1.55, the glass transition temperature Tg is 80-200 DEG C or less, and in an infrared absorption spectrum, when the absorbance per 1 mm thickness at a wave number of 3100 cm <-1 > is A3100 and the absorbance per 1 mm thickness at a wave number of 3240 cm <-1 > is A3240, A3240 / A3100 is 0.6-1.2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to glass, and in particular to glass having a low glass transition temperature (Tg) and capable of low temperature molding, in which crystallization during molding is suppressed and which exhibits more excellent moisture absorption resistance, composite components of the glass and a resin, and sintered bodies and molded bodies thereof. Background Art

[0002] Although organic polymers (resins) are inferior to glass in heat resistance, light resistance, light transmittance, and gas barrier properties, they are used in various applications because of their low molding temperature and low cost. On the other hand, glass is excellent in heat resistance, light resistance, light transmittance, and gas barrier properties, but generally has a high Tg and is difficult to freely mold.

[0003] Low melting point glass refers to a glass material having a lower melting point than ordinary glass, and is used as a coating on metal surfaces or glass surfaces, as a bonding agent therebetween, or as a sealing material for electronic products that require higher airtightness than resin-based materials (e.g., Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application No. 2010-505727 Summary of the invention

[0007] However, conventional low-melting-point glass has the following problems: it is difficult to become transparent after low-temperature molding due to easy crystallization, and the molding temperature margin is narrow due to crystallization. Therefore, conventional low-melting-point glass is not suitable as a material for low-temperature molding processes such as extrusion, injection, blow molding, and press molding used in general resin molding.

[0008] In addition, since conventional low-melting-point glass is hygroscopic, it may absorb moisture in the air and cause the properties of the glass to become unstable. In addition, the gas barrier properties of the glass may be reduced.

[0009] Therefore, an object of the present invention is to provide a glass which has a low Tg, can be molded at a low temperature, can be crystallized during molding, and has excellent moisture absorption resistance.

[0010] The inventors of the present invention have studied the above-mentioned problems and found that the above-mentioned problems can be solved by making the glass into a specific composition range, especially making the total content of Sn and Zn into a specific range, and then controlling the structure around the OH group in the glass to achieve moisture absorption resistance and inhibit crystallization during molding, thereby completing the present invention.

[0011] The present invention relates to a glass, which contains, expressed by mole % of elements, P: 12-16%, Sn: 16-21%, O: 50-60%, F: 5-15%, Zn: 0-3%, Si: 0-1%, B: 0-1%, Al: 0-3%, (Sn+Zn) / P is 1.25-1.55, the glass transition temperature Tg is 80-200°C, and in the infrared absorption spectrum, the wave number 3100cm -1 The absorbance per 1 mm thickness at the point is set as A3100, and the wave number is 3240 cm -1 When the absorbance per 1 mm thickness at the position is defined as A3240, A3240 / A3100 is 0.6 to 1.2.

[0012] The glass of the present invention has a specific composition range, a Tg of 80 to 150°C, excellent moldability, and a wavelength of 3100 cm-1 in the infrared absorption spectrum. -1 The absorbance per 1 mm thickness at the point is set as A3100, and the wave number is 3240 cm -1 When the absorbance per 1 mm thickness is defined as A3240, A3240 / A3100 is in a specific range, and the structure around the OH group in the glass is controlled to suppress crystallization. Thus, the glass of the present invention has the advantages of showing excellent transparency and moisture absorption resistance after low-temperature molding. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 (A) and (B) are schematic cross-sectional views of one embodiment of the glass resin laminate. Figure 1 (C) is a schematic cross-sectional view of one embodiment of the glass resin sea-island composite.

[0014] Figure 2 (A) to (C) in FIG. 1 are schematic diagrams showing one embodiment of a method for producing a glass resin sea-island composite.

[0015] Figure 3 A DSC curve is shown.

[0016] Figure 4 (A) and (B) are schematic cross-sectional views showing a configuration example of a packaging material formed using the sintered body or the molded body of the present embodiment as a part thereof.

[0017] Figure 5 (A) to (C) are schematic cross-sectional views showing examples of the configuration of a fluorescent dispersion body formed using the sintered body or the molded body of the present embodiment as a part thereof.

[0018] Figure 6 1 is a schematic cross-sectional view showing a configuration example of an airtight sealing material 61 formed using the sintered body or the molded body of the present embodiment as a part thereof.

[0019] Figure 7 1 is a schematic cross-sectional view showing a configuration example of a vacuum multiple glass 71 formed using the sintered body or the molded body of the present embodiment as a part thereof.

[0020] Figure 8 (A) to (G) are schematic cross-sectional views showing configuration examples of a lens or a diffraction grating formed using the sintered body or the molded body of the present embodiment as a part thereof. DETAILED DESCRIPTION

[0021] In the present specification, “to” indicating a numerical range is used to mean that the numerical values ​​described before and after it are included as the lower limit and the upper limit, and unless otherwise specified, “to” is used in the present specification with the same meaning.

[0022] In this specification, the glass composition is expressed as the content of each element in mol % unless otherwise specified, and mol % is abbreviated as "%".

[0023] In addition, "substantially not containing" in this specification means that it is less than the level of impurities contained in raw materials, etc., that is, it is not intentionally added. In this specification, when it is stated that a certain component is substantially not contained, the content of the component is specifically, for example, less than 0.1%.

[0024] In this specification, "parallel light transmittance" refers to the ratio of parallel light beams emitted from a sample to parallel light beams incident on the sample, and does not include scattered light. In addition, "haze ratio" refers to a value measured using C light source in accordance with JIS K3761:2000.

[0025] <Glass>

[0026] (composition)

[0027] The glass of the present invention contains, expressed by mole % of elements, P: 12-16%, Sn: 16-21%, O: 50-60%, F: 5-15%, Zn: 0-3%, Si: 0-1%, B: 0-1%, Al: 0-3%, and (Sn+Zn) / P is 1.25-1.55.

[0028] Each composition range is described below.

[0029] The P content is 12% or more, preferably 13% or more, and more preferably 13.5% or more. By setting the P content to 12% or more, the glass transition temperature Tg and the molding temperature can be reduced. The P content is 16% or less, preferably 15.5% or less, and more preferably 15% or less. By setting the P content to 16% or less, the moisture absorption resistance and gas barrier properties can be improved.

[0030] The content of Sn is 16% or more, preferably 16.5% or more, and more preferably 17% or more. When the content of Sn is 16% or more, the moisture absorption resistance and gas barrier properties can be improved. The content of Sn is 21% or less, preferably 20% or less, and more preferably 19% or less. When the content of Sn is 21% or less, the glass transition temperature Tg and the molding temperature can be lowered.

[0031] The content of O is 50% or more, preferably 51% or more, and more preferably 52% or more. By setting the content of O to 50% or more, the glass manufacturing process can be simplified and the moisture absorption resistance can be improved. The content of O is 60% or less, preferably 58% or less, and more preferably 56% or less. By setting the content of O to 60% or less, the glass transition temperature Tg and the molding temperature can be lowered.

[0032] The content of F is 5% or more, preferably 7% or more, more preferably 9% or more, and further preferably 11% or more. By making the content of F 5% or more, the glass transition temperature Tg and the molding temperature can be lowered, and crystallization can be suppressed. The content of F is 15% or less, preferably 14.5% or less, more preferably 14% or less, and further preferably 13.5% or less. By making the content of F 15% or less, the moisture absorption resistance can be improved. In addition, the glass manufacturing process can be simplified, and the generation of HF gas during melting and low-temperature molding can be suppressed.

[0033] The glass of the present invention contains 0 to 3% Zn. By containing Zn, crystallization can be suppressed while keeping the glass transition temperature Tg low, and the thermal expansion coefficient can be reduced. When Zn is contained, its content is preferably 0.1% or more, more preferably 0.5% or more, and further preferably 1% or more. From the viewpoint of hygroscopic resistance, the Zn content is 3% or less, preferably 2.5% or less, more preferably 2.2% or less, and further preferably 2% or less.

[0034] The glass of the present invention contains 0 to 1% Si. By containing Si, Si is introduced into the skeleton, thereby stabilizing it and improving the moisture absorption resistance. In addition, the thermal expansion coefficient can be reduced while keeping the glass transition temperature Tg low. When containing Si, its content is preferably 0.001% or more, more preferably 0.01% or more, and further preferably 0.05% or more. From the viewpoint of inhibiting crystallization, the Si content is 1% or less, preferably 0.5% or less, more preferably 0.3% or less, and further preferably 0.1% or less.

[0035] The glass of the present invention contains 0 to 1% B. By containing B, the moisture absorption resistance can be improved. In addition, the thermal expansion coefficient can be reduced while maintaining the glass transition temperature Tg low. When B is contained, its content is preferably 0.001% or more, more preferably 0.01% or more, and further preferably 0.05% or more. From the viewpoint of inhibiting crystallization, the content of B is 1% or less, preferably 0.5% or less, more preferably 0.3% or less, and further preferably 0.2% or less.

[0036] The glass of the present invention contains 0 to 3% Al. By containing Al, the moisture absorption resistance can be improved. In addition, the thermal expansion coefficient can be reduced while maintaining the glass transition temperature Tg at a low level. When Al is contained, the content is preferably 0.1% or more, more preferably 0.2% or more, and further preferably 0.5% or more. From the viewpoint of inhibiting crystallization, the content of Al is 3% or less, preferably 2% or less, more preferably 1.5% or less, and further preferably 1% or less.

[0037] The total content of Sn and the content of Zn, i.e., Sn+Zn, is preferably 18% or more. By making Sn+Zn 18% or more, crystallization, especially crystallization of tin phosphate, can be suppressed. Sn+Zn is preferably 18.2% or more, more preferably 18.4% or more, and further preferably 18.5% or more. Sn+Zn is preferably 21% or less, more preferably 20.5% or less, further preferably 20% or less, and particularly preferably 19.5% or less. By making Sn+Zn 21% or less, moisture absorption resistance can be improved.

[0038] The ratio of the total content of Sn and the content of Zn to the content of P, i.e. (Sn+Zn) / P, is 1.25 to 1.55. By making (Sn+Zn) / P greater than 1.25, crystallization, especially the precipitation of tin phosphate and zinc phosphate, can be suppressed. (Sn+Zn) / P is preferably greater than 1.30, more preferably greater than 1.32. By making (Sn+Zn) / P less than 1.55, the moisture absorption resistance of the glass can be improved, and the residual rate of F after melting and low-temperature forming can be improved. (Sn+Zn) / P is preferably less than 1.50, more preferably less than 1.40.

[0039] The glass of the present invention may contain any compound or additive used in glass in addition to the above components as long as the contents of the above components are within the above ranges, as long as the effects of the present invention are achieved. For example, the following components may be contained.

[0040] The glass of the present invention may contain 0 to 10% of Ba. By containing Ba, crystallization can be suppressed while the glass transition temperature Tg is kept low, and the moisture absorption resistance can be improved.

[0041] The glass of the present invention may contain 0 to 20% in total of Mg, Ca, and Sr. By containing Mg, Ca, or Sr, the moisture absorption resistance can be improved.

[0042] The glass of the present invention contains 0 to 20% in total of Li, Na, and K. By containing Li, Na, or K, the glass transition temperature Tg and the molding temperature can be lowered.

[0043] The glass of the present invention may contain 0 to 3% of Zr. By containing Zr, crystallization can be suppressed, and moisture absorption resistance and chemical resistance can be improved.

[0044] The glass of the present invention may contain 0 to 5% in total of Ce and Y. By containing Ce or Y, moisture absorption resistance and chemical resistance can be improved.

[0045] The glass of the present invention may contain 0 to 5% in total of Nb, W, Mo and Ta. By containing Nb, W, Mo or Ta, the moisture absorption resistance and chemical resistance can be improved.

[0046] The glass of the present invention may contain 0 to 10% in total of Fe, Ti, Mn, Cr, Cu and Ag. By containing Fe, Ti, Mn, Cr, Cu or Ag, crystallization can be suppressed and the glass transition temperature Tg can be lowered.

[0047] The glass of the present invention may contain 0 to 20% in total of Cl, Br, and I. By containing Cl, Br, or I, the moisture absorption resistance and chemical resistance can be improved, and crystallization can be suppressed.

[0048] (Glass transition temperature Tg)

[0049] The glass transition temperature Tg of the glass of the present invention is 80 to 200°C. By making the glass transition temperature Tg below 200°C, the glass becomes a low melting point and can be used as a material for low-temperature molding processes such as extrusion, injection, blow molding, and press molding used in general resin molding. In addition, for the purpose of sealing without thermally degrading the phosphor (especially quantum dot phosphor) and for the purpose of low-temperature sintering the glass without thermally degrading the surrounding components such as metals and organic substances, a low melting point is also preferred. The glass transition temperature Tg is preferably below 180°C, more preferably below 160°C, and further preferably below 140°C. In addition, by making the glass transition temperature Tg above 80°C, the thermal expansion coefficient can be reduced, and the durability and moisture absorption resistance can be improved. It is preferably above 100°C, more preferably above 110°C, and further preferably above 120°C.

[0050] (Infrared absorption spectrum)

[0051] For the glass of the present invention, in the infrared absorption spectrum, the wave number 3100 cm-1 The absorbance per 1 mm thickness at the point is set as A3100, and the wave number is 3240 cm -1 When the absorbance per 1 mm thickness at A3240 is set to A3240, A3240 / A3100 is 1.2 or less, preferably 1 or less, and more preferably 0.9 or less. By A3240 / A3100 being 1.2 or less, the structure around the OH group can be properly controlled, thereby suppressing crystallization. Moreover, foaming can be suppressed, thereby obtaining a transparent molded body. A3240 / A3100 is 0.6 or more, preferably 0.7 or more, and more preferably 0.8 or more. By A3240 / A3100 being 0.6 or more, the glass manufacturing process can be simplified.

[0052] Wave number 3100cm -1 and wave number 3240cm -1 The infrared absorption spectrum near represents the structure around the OH group in the glass. By using the PO-Sn-O structure as the structure of the glass skeleton, the F and OH attached to the glass skeleton are volatilized during low-temperature molding, and the elements are rearranged, which easily produces crystals of tin phosphate compounds. When the structure of the glass skeleton adopts the PO-Sn-O structure, the peak of A3240 in the infrared absorption spectrum is easy to stand out, and A3240 / A3100 is greater than 1.2. By making the structure of the glass skeleton preferably a POPO structure, A3240 / A3100 can be made less than 1.2. The F and OH attached to the POPO structure are difficult to volatilize during low-temperature molding, and even if they are volatilized, it is difficult to produce crystallization through the rearrangement of elements. Since the volatilization of F and OH can be suppressed, it is also difficult to produce foaming, and the transparency is improved.

[0053] By using ammonium dihydrogen phosphate (NH4H2PO4) as the phosphate raw material of the glass, the structure of the glass skeleton is made into a PO-Sn-O structure, and crystals of tin phosphate compounds are easily generated. In addition, when using ammonium dihydrogen phosphate, in addition to the large environmental load caused by the generation of a large amount of ammonia gas during glass melting, foaming also occurs during low-temperature molding due to the ammonia gas, so it is not preferred. On the other hand, by using orthophosphoric acid (H3PO4) or using orthophosphoric acid and stannous pyrophosphate (Sn2P2O7) together as the phosphate raw material of the glass, the structure of the glass skeleton is made into a POPO structure, and it is not easy to crystallize and foam after melting and low-temperature molding. Excellent transparency glass. In addition, the moisture contained in orthophosphoric acid plays a role in inhibiting crystallization during low-temperature molding in the glass, so it is preferred to use orthophosphoric acid as the phosphate raw material of the glass.

[0054] The glass of the present invention has a wave number of 3100cm in the infrared absorption spectrum. -1The absorbance per 1 mm thickness at the wavelength of 3240 cm is preferably 0.2 to 4, more preferably 0.3 to 3, and even more preferably 0.5 to 2. -1 The absorbance per 1 mm thickness at the wavelength of 3100 cm is preferably 0.12 to 4.8, more preferably 0.18 to 3.6, and even more preferably 0.3 to 2.4. -1 The absorbance per 1 mm thickness and the wave number 3240 cm -1 When the absorbance per 1 mm thickness is within the above range, the structure of the glass is controlled, and crystallization and foaming are less likely to occur during low-temperature molding, thereby obtaining a molded body with excellent transparency.

[0055] The infrared absorption spectrum was measured using a Fourier transform infrared spectrophotometer. -1 The transmittance at T400 is set, and the wave number is set to 3100 cm -1 The transmittance at T3100 is set, and the wave number is set to 3240 cm -1 The transmittance at the point is set as T3240, and the thickness of the sample is measured as D (mm). According to A3100 = -log 10 (T3100 / T400) / D and calculate the wave number 3100cm -1 The absorbance per 1mm thickness is A3100, according to A3240 = -log 10 (T3240 / T400) / D and calculate the wave number 3240cm -1 The absorbance A3240 per 1 mm thickness at the measurement point is divided by T400 to correct the baseline in the measurement. It should be noted that the measurement sample is preferably processed into a flat plate with a thickness of 1 mm using cerium oxide free abrasive grains as a polishing agent.

[0056] (Refractive Index)

[0057] The refractive index nd of the glass of the present invention is 1.60 to 1.90, preferably 1.65 to 1.85, and more preferably 1.70 to 1.80. The refractive index nd of the glass of the present invention is higher than that of resins having the same viscosity characteristics, and when the glass of the present invention is used for optical components, the number of components can be reduced.

[0058] (Complex viscosity)

[0059] The glass of the present invention preferably has a temperature (T ) at which the complex viscosity measured in a dry nitrogen atmosphere at a dew point of -60°C reaches 1000 Pa·s. η=1000(-60℃) ) is 190~260℃. η=1000(-60℃) When the temperature is 190°C or higher, the stability and weather resistance of the glass at room temperature can be improved. η=1000(-60℃) It is more preferably 200°C or higher, and even more preferably 215°C or higher.η=1000(-60℃) The temperature is below 260°C, so that it is easy to melt at low temperature by calcination in a dry atmosphere and easy to form at low temperature. In addition, when used as a sealing material, low-temperature sintering can be performed without thermally degrading surrounding components such as phosphors (especially quantum dot phosphors), metals, and organic substances. η=1000(-60℃) The temperature is more preferably 250°C or lower, and even more preferably 240°C or lower.

[0060] The temperature at which the complex viscosity reaches 1000 Pa·s (T η=1000(0℃) ) is preferably higher than the temperature (T) at which the complex viscosity reaches 1000 Pa·s measured in a dry nitrogen atmosphere at a dew point of -60°C. η=1000(-60℃) ) is higher than 10℃. η=1000(0℃) With T η=1000(-60℃) The temperature difference is 10°C or more, which can improve the heat resistance when used in the atmosphere. η=1000(0℃) With T η=1000(-60℃) The temperature difference is more preferably 15°C or more, and further preferably 20°C or more. η=1000(0℃) With T η=1000(-60℃) The temperature difference is less than 100°C, and low-temperature molding or low-temperature sintering can be stably performed with respect to changes in the atmosphere. η=1000(0℃) With T η=1000(-60℃) The temperature difference is more preferably 50°C or less, further preferably 40°C or less.

[0061] The complex viscosity was determined from the viscoelasticity measured using a rheometer MCR502 manufactured by Anton Paar in accordance with JIS K 7244-10:2005 at a frequency of 1 Hz and a shear strain of 0.1%.

[0062] (moisture absorption capacity)

[0063] The weight increase per unit surface area of ​​the glass of the present invention when stored in an atmosphere of a temperature of 60° C. and a relative humidity of 90% for 5 hours is preferably 5 mg / cm 2 Below, more preferably 2 mg / cm 2 Below, more preferably 0.5 mg / cm 2 Below. The weight increase is 5 mg / cm 2 The lower limit of the weight increase is not particularly limited, but is usually 0.01 mg / cm 2 above.

[0064] (Differential Scanning Calorimetry)

[0065] The difference between the crystallization peak temperature Tc and the glass transition temperature Tg obtained by differential scanning calorimetry of the glass of the present invention is preferably 150°C or more, more preferably 160°C or more, and further preferably 170°C or more. It should be noted that it is most preferred that Tc is not observed, in which case the difference between Tc and Tg can be interpreted as infinite. By making the difference between Tc and Tg 150°C or more, the interval between the formable temperature and the crystallization temperature, i.e., the forming temperature margin, is expanded, and a glass with better transparency is obtained after low-temperature forming or low-temperature sintering. It should be noted that at a temperature above Tc, the viscosity rises sharply due to the crystallization of the glass, so it is difficult to form at low temperature.

[0066] The difference between the crystallization start temperature Tx and the glass transition temperature Tg obtained by differential scanning calorimetry of the glass of the present invention is preferably 140°C or more, more preferably 150°C or more, and further preferably 160°C or more. It should be noted that it is best not to observe Tx, in which case the difference between Tx and Tg can be interpreted as infinite. By making the difference between Tx and Tg 140°C or more, the interval between the moldable temperature and the crystallization start temperature is expanded, and a glass with better transparency is obtained after low-temperature molding or low-temperature sintering.

[0067] The differential scanning calorimetry analysis was performed by using a powder having a median particle size of less than 3 μm crushed in an agate mortar as a sample for measurement, and the temperature was raised from 25°C to 500°C at 2°C / min in an atmosphere. Figure 3 As shown, in the DSC curve, Tg is the temperature at which the curve first undergoes endothermic transition during the temperature rise process, Tx is the temperature at which heat release due to crystallization first begins during the temperature rise process, and Tc is the peak temperature of heat release due to crystallization first generated during the temperature rise process.

[0068] (Weight reduction rate during molding)

[0069] The weight loss rate of the glass of the present invention before and after heat treatment for 1 hour at (Tg+150)°C is preferably 2% or less, more preferably 1% or less, and further preferably 0.7% or less. (Tg+150)°C is the same temperature as the temperature during low-temperature molding. By keeping the weight loss rate below 2% and not too much water in the glass, foaming during low-temperature molding is suppressed, and a molded body with excellent transparency is obtained. The lower limit of the weight loss rate is preferably 0.1% or more, more preferably 0.2% or more, and further preferably 0.3% or more. By keeping the weight loss rate above 0.1%, crystallization during low-temperature molding is suppressed due to the presence of water in the glass, and a molded body with excellent transparency is obtained.

[0070] The weight loss before and after the heat treatment at (Tg+150)°C for 1 hour was measured under the following conditions.

[0071] The weight of the sample was measured using a thermogravimetric-differential thermal analyzer. As the sample for measurement, a powder with a median particle size of less than 3 microns was used, which was crushed in an agate mortar. The measurement conditions were to increase the temperature from 25°C to (Tg+150)°C at 2°C / min in an atmospheric atmosphere and to maintain it at (Tg+150)°C for 1 hour. The weight reduction rate relative to the initial weight at this time was evaluated.

[0072] (Parallel light transmittance)

[0073] The glass of the present invention preferably has an average value of 70% or more, more preferably 80% or more, and even more preferably 85% or more, of the parallel light transmittance at a wavelength of 400 to 700 nm measured in the thickness direction of a flat plate with a thickness of 1 mm. By having this average value of 70% or more, it becomes a glass with excellent transparency and suppressed crystallization. In addition, a molded body with high transparency is obtained by low-temperature molding using a glass with this average value of 70% or more. The upper limit of this average value is not particularly limited, and is typically 92% or less. It should be noted that the sample for measurement is preferably processed into a flat plate with a thickness of 1 mm using cerium oxide free abrasives as a polishing agent.

[0074] (Haze rate)

[0075] The glass of the present invention preferably has a haze ratio of 20% or less, more preferably 15% or less, and further preferably 10% or less, when measured in the thickness direction of a flat plate with a thickness of 1 mm. When the average value is 20% or less, the glass has excellent transparency and suppressed crystallization. The lower limit of the haze ratio is not particularly limited, but is typically 0.2% or more. It should be noted that the sample for measurement is preferably processed into a flat plate with a thickness of 1 mm using cerium oxide free abrasives as a polishing agent.

[0076] (Manufacturing method)

[0077] The glass of the present invention can be manufactured by a method of modulating glass raw materials, melting and cooling. The glass of the present invention preferably uses orthophosphoric acid (H3PO4) as the phosphate raw material of the glass. When using orthophosphoric acid, in order to remove the moisture of orthophosphoric acid, it can be used after drying at a temperature of 100 to 500°C for about 10 minutes to 50 hours before melting. Only orthophosphoric acid can be dried and mixed with other raw materials, or orthophosphoric acid can be mixed with part or all of other raw materials and then dried. The raw materials are placed in a container such as platinum, carbon, quartz, alumina or nickel and melted at a temperature of 400 to 700°C for about 10 minutes to 10 hours. All raw materials can be melted together, or only a part or specific raw materials can be melted first, and then the remaining part can be melted. The molten glass can be formed into a specified shape such as glass material, pellets, fragments, etc. by various methods as needed.

[0078] <Glass Frit>

[0079] The glass of the present invention can be a glass material having a powdered form. By making it into a glass material shape, it can be used for processes such as printing, dispensing, coating, and powder pressing. The average particle size (d50) of the glass material is preferably 0.5 μm or more. By making the average particle size (d50) be 0.5 μm or more, it is possible to suppress the mixing of excessive bubbles into the low-temperature sintered body. The average particle size (d50) is preferably 1 μm or more, and more preferably 1.5 μm or more. In addition, the average particle size (d50) is preferably 10 μm or less. By making the average particle size (d50) be 10 μm or less, the surface roughness of the low-temperature sintered body can be reduced, and the printed film thickness can be thinned. The average particle size (d50) is more preferably 5 μm or less, and further preferably 3 μm or less. The average particle size (d50) is obtained by laser diffraction.

[0080] The manufacturing method of the glass frit is not particularly limited, and for example, the glass of the present invention is obtained by pulverizing. Therefore, the particle size of the glass is determined by the pulverizing conditions. For example, the pulverizing method includes a rotary ball mill, a vibrating ball mill, a planetary grinder, a jet mill, a grinding mill, a medium stirring mill (bead mill), a jaw crusher, a roll crusher, etc.

[0081] <Glass paste>

[0082] The glass of the present invention can be made into a glass paste by dispersing powdered glass in a solvent and mixing a resin component to adjust the viscosity. Examples of the resin used in the glass paste include ethyl cellulose, nitrocellulose, acrylic resin, vinyl acetate, butyral resin, melamine resin, alkyd resin, and rosin resin.

[0083] In addition, as the solvent used for the glass frit paste, for example, ether solvents (butyl carbitol (BC), butyl carbitol acetate (BCA), diethylene glycol di-n-butyl ether, dipropylene glycol butyl ether, tripropylene glycol butyl ether, butyl cellosolve acetate, ethylene glycol monophenyl ether, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether), alcohol solvents (α-terpineol, pine oil, DOWANOL), glycol solvents (propylene glycol, ethylene glycol, diethylene glycol, dipropylene glycol, tripropylene glycol), ketone solvents (isophorone, cyclohexanone), ester solvents (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate), phthalate solvents (DBP (dibutyl phthalate), DMP (dimethyl phthalate), DOP (dioctyl phthalate)).

[0084] The content of glass in the glass frit paste is preferably 55 to 90% by mass, more preferably 65 to 85% by mass, and further preferably 70 to 80% by mass. The content of resin in the glass frit paste is preferably 0 to 10% by mass, more preferably 1 to 7% by mass, and further preferably 2 to 5% by mass. The content of solvent in the glass frit paste is preferably 10 to 45% by mass, more preferably 15 to 40% by mass, and further preferably 20 to 35% by mass.

[0085] The glass paste may contain inorganic powder and phosphor. Inorganic powder is added for the purpose of imparting scattering properties, improving strength, reducing thermal expansion, etc. Examples of inorganic powder include silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zirconium phosphate, zirconium tungstate phosphate, and cordierite. The content of the inorganic powder is preferably 0.01 to 30% by mass, more preferably 1 to 20% by mass, and further preferably 5 to 10% by mass.

[0086] As the phosphor, for example, oxides, oxynitrides, nitrides, semiconductor nanoparticles (quantum dots), etc. can be cited. The content of the phosphor is preferably 0.01 to 30% by mass, more preferably 1 to 20% by mass, and further preferably 5 to 10% by mass. By low-temperature sintering or low-temperature molding the glass frit paste containing the phosphor, the phosphor can be sealed and dispersed in the glass.

[0087] <Glass Granules>

[0088] The glass of the present invention may be a glass pellet in the form of a pellet. By forming the glass pellet in the form of a pellet, it is easy to put into a low temperature forming machine. The major diameter of the glass pellet is preferably 0.1 mm to 5 mm. The lower limit of the major diameter of the glass pellet is more preferably 1 mm or more, and more preferably 2 mm or more. In addition, the upper limit of the major diameter of the glass pellet is more preferably 4.5 mm or less, and more preferably 4 mm or less.

[0089] The minor diameter of the glass pellets is preferably 0.1 mm to 5 mm. The lower limit of the minor diameter of the glass pellets is more preferably 0.5 mm or more, and more preferably 1.5 mm or more. In addition, the upper limit of the minor diameter of the glass pellets is more preferably 4.5 mm or less, and more preferably 4 mm or less. If the diameter and minor diameter of the glass pellets are within the above range, it is easy to carry out screw conveying in the molding machine and is not easy to break in the molding machine. In addition, it is not easy to crystallize during low-temperature molding.

[0090] From the viewpoint of preventing breakage in a molding machine, the ratio of the major axis to the minor axis of the glass pellets is preferably 0.2 to 1, more preferably 0.5 to 1, and even more preferably 0.7 to 0.95.

[0091] The method for producing glass pellets is not particularly limited, and examples thereof include a method of pressing using a mold, a method of crushing glass using water, a drop forming method, a method of remelting glass powder, a method of finely crushing the melt and then dispersing it, a method of extruding glass into a rope shape and then cutting it using a pelletizer, a method of finely cutting flat glass, etc.

[0092] Glass pellets may contain inorganic powders and phosphors. Inorganic powders are added for the purpose of imparting scattering, improving strength, and reducing thermal expansion. As inorganic powders, silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zirconium phosphate, zirconium tungstate phosphate, cordierite, etc. may be used. The content of inorganic powders is preferably 0.01 to 50% by volume, more preferably 1 to 30% by volume, and further preferably 10 to 25% by volume. As phosphors, oxides, nitrogen oxides, nitrides, semiconductor nanoparticles (quantum dots), etc. may be used. The content of phosphors is preferably 0.01 to 50% by volume, more preferably 1 to 30% by volume, and further preferably 10 to 25% by volume. By low-temperature sintering or low-temperature molding of glass pellets containing phosphors, the phosphors can be sealed and dispersed in the glass.

[0093] The glass pellets may contain bubbles. The bubbles are added for the purpose of imparting scattering properties, etc. The content of the bubbles is preferably 0.01 to 50% by volume, more preferably 1 to 30% by volume, and further preferably 5 to 20% by mass.

[0094] (Low temperature forming and low temperature sintering)

[0095] The glass of the present invention is preferably used for low-temperature molding or low-temperature sintering of at least any one of extrusion molding, injection molding, blow molding and press molding, preferably at 400° C. or less, more preferably at 300° C. or less, and further preferably at 250° C. or less. As described above, the glass of the present invention has a Tg of 80 to 150° C. and an A3240 / A3100 of 1.2 or less. Therefore, even when used in a low-temperature molding process preferably at 400° C. or less, a molded body or sintered body having excellent transparency and suppressed crystallization can be obtained.

[0096] <<Glass resin mixed glass frit>>

[0097] The glass frit may be a glass-resin mixed glass frit obtained by mixing the glass frit of the present invention with a resin. As the resin, both thermosetting resins and thermoplastic resins can be used. From the viewpoint of easy composite with glass, a thermoplastic resin is preferred, and a resin having an acid group and an amino group is preferred. The resin having an acid group and an amino group is easy to chemically bond with the low melting point glass of the present invention. The resin may be a powder, in which case the average particle size (d50) is preferably 0.5 μm to 10 μm.

[0098] Examples of the thermosetting resin include epoxy resins, phenolic resins, urea resins, melamine resins, silicone resins, unsaturated polyester resins, and polyurethane resins.

[0099] In addition, examples of thermoplastic resins include nylon, polyacetal, polysulfone, polyetherimide, polyamideimide, liquid crystal polymer, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, aromatic polyether, polyphenylene ether, polyetheretherketone, polyphenylene ether, polycarbonate, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethersulfone, polypropylene, polystyrene, acrylonitrile-butadiene-styrene, acrylic acid, polyvinyl chloride, polyarylate, polyoxybenzoyl polyester, cycloolefin polymer, cycloolefin copolymer, and the like.

[0100] From the viewpoint of facilitating composite formation with glass, it is preferred that the viscosities of the glass and the resin in the molding temperature range be substantially the same.

[0101] In the glass-resin mixed glass frit of the present invention, the mixing ratio of glass to resin can be appropriately set in consideration of the use of the composite material composition, and is not particularly limited. For example, it can be mixed and composited in the range of glass:resin = 1:99 to 99.9:0.1 (volume ratio).

[0102] <<Glass-resin composite granules>>

[0103] The glass granules can be glass-resin composite granules obtained by composite the glass of the present invention with a resin. As the resin, both thermosetting resins and thermoplastic resins can be used. From the viewpoint of being easy to composite with glass, thermoplastic resins are preferred, and resins having acid groups and amino groups are preferred. Resins having acid groups and amino groups are easy to chemically bond with the low melting point glass of the present invention.

[0104] Examples of the thermosetting resin include epoxy resins, phenolic resins, urea resins, melamine resins, silicone resins, unsaturated polyester resins, and polyurethane resins.

[0105] In addition, examples of thermoplastic resins include nylon, polyacetal, polysulfone, polyetherimide, polyamideimide, liquid crystal polymer, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, aromatic polyether, polyphenylene ether, polyetheretherketone, polyphenylene ether, polycarbonate, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethersulfone, polypropylene, polystyrene, acrylonitrile-butadiene-styrene, acrylic acid, polyvinyl chloride, polyarylate, polyoxybenzoyl polyester, cycloolefin polymer, cycloolefin copolymer, and the like.

[0106] From the viewpoint of facilitating composite formation with glass, it is preferred that the viscosities of the glass and the resin in the molding temperature range be substantially the same.

[0107] The method for producing the glass-resin composite pellets is not particularly limited, and examples thereof include a method of granulating a melt obtained by melt-kneading a glass component and a resin component and other components as required using a twin-screw kneading extruder, or a method of hot-pressing glass pellets and resin pellets.

[0108] In the glass-resin composite pellets of the present invention, the ratio of glass to resin can be appropriately set in consideration of the use of the composite material composition, and is not particularly limited. For example, glass:resin can be mixed and composited in the range of 1:99 to 99:1 (volume ratio).

[0109] <<Other ingredients>>

[0110] In the present invention, the glass resin mixed glass frit, glass frit paste and glass granules may contain one or more fillers, additives, etc. as required. As the filler, it may be a plate-like filler, a spherical filler and other granular fillers. The filler may be an inorganic filler or an organic filler. As the additive, for example, flame retardants, conductivity imparting materials, crystal nuclei, ultraviolet absorbers, antioxidants, vibration dampers, antibacterial agents, insect repellents, deodorants, anti-colorants, heat stabilizers, release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, viscosity modifiers, surfactants may be cited.

[0111] <Sintered body>

[0112] The sintered body of the present invention is obtained by low-temperature calcining the above-mentioned glass frit (glass frit alone or glass resin mixed glass frit) composed of the glass of the present invention or the above-mentioned glass frit paste containing the glass of the present invention. If the glass crystallizes during calcination, the sintered body loses transparency and loses fluidity during calcination, so shape control becomes difficult and airtight sealing is difficult. Since the glass of the present invention suppresses crystallization and foaming during calcination, a sintered body with excellent shape stability and gas barrier properties is obtained. In addition, since crystallization and foaming are suppressed during calcination, a sintered body with excellent transparency is obtained.

[0113] Examples of methods for forming the sintered body of the present invention include a method of calcining glass frit in a powder state, a method of calcining the glass frit after forming a powder compact, and a method of applying a glass frit paste to a member such as glass, resin, or metal and then calcining the compact.

[0114] The sintered body of the present invention preferably has good gas barrier properties. Specifically, the water vapor permeability is preferably 1 g / m at a temperature of 40° C. and a relative humidity of 90%. 2 / day or less, more preferably 0.1g / m2 / day or less, more preferably 0.01g / m 2 / day or less, particularly preferably 0.001g / m 2 / day or less.

[0115] As the form of the sintered body involved in the present invention, for example, a glass sintered body and a glass resin composite can be cited. In addition, the shape of the sintered body can be a shape obtained by directly calcining glass powder without molding the glass frit. In addition, it can also be a shape obtained by coating the glass frit paste into a film shape and then calcining it. In addition, the surface can be smooth or have unevenness.

[0116] <Molding body>

[0117] The molded body involved in the present invention comprises the glass of the present invention, and is obtained by molding the above-mentioned glass material or the above-mentioned glass granules (glass material, granules, glass resin composite glass material or glass resin composite granules of glass alone) into a desired shape by low-temperature molding such as extrusion, injection, blow molding, and press molding. If the glass crystallizes and foams during molding, molding becomes difficult, and the molded body loses transparency. Since the glass of the present invention is inhibited from crystallizing and foaming during molding, a molded body with excellent bonding strength and transparency when composited with a resin is obtained. From the perspective of ensuring transparency, the average value of the parallel light transmittance in the thickness direction of the molded body at a wavelength of 400 to 700 nm is preferably 60% or more, more preferably 70% or more, and further preferably 80% or more. The upper limit of the parallel light transmittance is not particularly limited, and is typically 92% or less. In addition, from the perspective of ensuring transparency, the haze rate in the thickness direction of the molded body is preferably 20% or less, more preferably 15% or less, and further preferably 10% or less. The lower limit of the haze rate is not particularly limited, and is typically 0.2% or more.

[0118] The molded article of the present invention preferably has good gas barrier properties. Specifically, the water vapor permeability is preferably 1 g / m at a temperature of 40° C. and a relative humidity of 90%. 2 / day or less, more preferably 0.1g / m 2 / day or less, more preferably 0.01g / m 2 / day or less, particularly preferably 0.001g / m 2 In addition, when the moisture absorption resistance of glass is poor, the glass absorbs moisture and deteriorates, and as a result, the gas barrier properties are greatly reduced.

[0119] As the form of the molded body of the present invention, for example, a glass molded body and a glass resin composite body can be mentioned. The shape of the molded body can be plate-like or film-like, and can also have a three-dimensional shape such as a cylinder, a column, a prism, a bottle, a syringe, a container, etc. In the case of a plate-like or film-like shape, it is not limited to a rectangle, and can also be a polygon, a circle, or an ellipse. In addition, the surface can be smooth or have concavoconvexity.

[0120] The thickness of the molded body is not particularly limited, but is preferably 0.01 to 10 mm, more preferably 0.02 to 3 mm, and further preferably 0.05 to 1 mm. When the thickness of the molded body is 0.01 mm or more, the strength can be improved, and the gas barrier properties can be improved. When the thickness of the molded body is 5 mm or less, light weight can be achieved.

[0121] The sintered body and the molded body of the present invention may contain an inorganic substance as a filler. Examples of the filler include silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zirconium phosphate, zirconium tungstate phosphate, and cordierite.

[0122] The content ratio of the filler is preferably 0.01 to 50 volume %, more preferably 1 to 30 volume %, and further preferably 10 to 25 volume % relative to the total volume of the glass component and the filler. If the content ratio of the filler is 0.01 volume % or more, the strength of the sintered body and the molded body or the adhesion to other components is improved. In addition, if the content ratio of the filler is 50 volume % or less, the fluidity during low temperature sintering and low temperature molding can be maintained. Preferably, it is 0.01 to 50 volume %, more preferably 1 to 30 volume %, and further preferably 10 to 25 volume %.

[0123] The sintered body and the molded body of the present invention can contain a fluorescent body because they show excellent transparency. In addition, the glass of the present invention has a low viscosity during molding, so it is easy to disperse the fluorescent body in the glass. As fluorescent body, for example, quantum dot fluorescent body, oxide, nitrogen oxide, nitride, semiconductor nanoparticle (quantum dot) etc. can be cited. Although these fluorescent bodies exist due to oxygen, water and deterioration over time, they can be suppressed by being dispersed in the glass.

[0124] The content ratio of the phosphor is preferably 0.01 to 50 volume %, more preferably 1 to 30 volume %, and further preferably 10 to 25 volume % relative to the total volume of the glass component and the phosphor. If the content ratio of the phosphor is 0.01 volume % or more, color conversion can be effectively performed. In addition, if the content ratio of the phosphor is 50 volume % or less, fluidity during low temperature sintering and low temperature molding can be maintained.

[0125] Examples of methods for making the sintered body or molded body of the present invention contain a phosphor include low-temperature molding of glass pellets containing a phosphor, calcining a glass paste containing a phosphor, and calcining a glass frit mixed with a phosphor.

[0126] <<Glass-resin composite>>

[0127] As glass resin composites, for example, there can be mentioned 1) glass resin laminates and 2) glass resin sea island composites. If the glass component crystallizes and foams, low-temperature molding of the composite molded body becomes difficult, and the bonding strength and transparency between the resin and the glass are reduced. Since the glass of the present invention suppresses crystallization and foaming during low-temperature molding, a composite having excellent bonding strength and transparency when compounded with a resin is obtained. From the perspective of ensuring transparency, the average value of the parallel light transmittance in the thickness direction of the composite at a wavelength of 400 to 700 nm is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. There is no particular limit to the upper limit of the parallel light transmittance, and it is typically 92% or less.

[0128] 1) Glass resin laminate

[0129] A schematic cross-sectional view of one embodiment of a glass resin laminate is shown in Figure 1 (A) and (B). Figure 1 As shown in (A) and (B), the glass resin laminate 11 is a laminate composed of two or more layers, preferably three or more layers, of a resin layer 13 laminated on one or both sides of a glass layer 12. From the viewpoint of moldability and strength, the outermost layer is preferably a resin.

[0130] The content ratio (mass ratio) of the glass layer to the resin layer in the glass resin laminate is preferably 1:99 to 80:20, and more preferably 10:90 to 60:40, from the viewpoint of gas barrier properties and weight reduction.

[0131] The glass resin laminate can be obtained by melting the glass component (e.g., the above-mentioned glass frit and glass granules) and the resin component (e.g., resin granules) separately, stacking and compounding them, and then low-temperature molding them by extrusion molding, injection molding, blow molding, press molding, etc.

[0132] The interface between the glass layer and the resin layer in the glass resin laminate is preferably a mixed phase of glass and resin, because the interface strength between the glass layer and the resin layer can be increased and optical scattering can be suppressed by having a refractive index intermediate between that of glass and that of resin.

[0133] 2) Glass resin island complex

[0134] A schematic cross-sectional view of one embodiment of a glass resin sea-island composite is shown in FIG. Figure 1 (C). Figure 1 As shown in (C), the glass resin sea-island composite 21 has a structure in which a particulate glass phase 23 which is a non-continuous phase having a closed interface exists in a resin phase 22 which is a continuous phase composed of a resin. Figure 1 Although (C) shows a schematic cross-sectional view of a single-layer glass resin sea-island composite, a structure consisting of two or more layers may be used. From the viewpoint of moldability and strength, the outermost layer is preferably a resin.

[0135] The term "sea-island structure" as used herein refers to a structure in which a discontinuous phase of a component constituting a particle-like island phase having a closed interface (boundary between phases) exists in a continuous phase of a component forming a sea phase.

[0136] From the viewpoint of gas barrier properties and weight reduction, the content ratio (mass ratio) of the glass phase to the resin phase in the glass resin sea-island composite is preferably 1:99 to 70:30, more preferably 10:90 to 60:40.

[0137] The interface between the glass phase and the resin phase in the glass-resin sea-island composite is preferably a mixed phase of glass and resin, because the interface strength between the glass phase and the resin phase can be increased and optical scattering can be suppressed by having a refractive index intermediate between that of glass and that of resin.

[0138] As a method for manufacturing a glass resin island composite, for example, the following method can be cited: a glass component (for example, the above-mentioned glass material and glass pellets) is mixed with a resin component (for example, resin pellets) to obtain a composite material (for example, glass-resin composite glass material and glass-resin composite pellets), the composite material and the resin component (for example, resin pellets) are melted separately, stacked and composited, and after low-temperature molding by extrusion molding, injection molding, blow molding, press molding, etc., biaxial stretching is performed.

[0139] Figure 2 Schematic diagram of one embodiment of a method for producing a glass resin sea-island composite is shown in FIG. Figure 2 (A) shows a lamination step. The lamination step is a step of laminating resin layers 27 on both surfaces of a layer 26 in which a glass component 24 and a resin component 25 are composited to obtain a laminate 28 . Figure 2 (B) shows the stretching and extending step. The stretching and extending step is a step of stretching and extending the laminate obtained in the lamination step by biaxial stretching. Thus, Figure 2 The glass resin sea island composite shown in (C).

[0140] <Application>

[0141] The sintered body or molded body of the present invention has excellent transparency, moisture absorption resistance and gas barrier properties. As its use, for example, packaging materials for foods such as high-functional foods or medicines, pharmaceutical containers such as syringes and ampoules, flexible displays such as organic field effect transistor (OLET) covers, and high-frequency films / substrates for wearable devices or mobile phones or 5G can be cited. In addition, for example, color conversion components dispersed with fluorescent materials (particularly preferably quantum dot fluorescent materials) for displays (for example, liquid crystals, organic EL televisions), airtight sealing materials for MEMS or electronic circuits, sealing materials for vacuum multilayer glass, or lenses (for example, aspherical lenses, prismatic lenses) and diffraction gratings made by press molding or injection molding can be cited.

[0142] (Packaging Materials)

[0143] The packaging material for foods such as highly functional foods or pharmaceuticals is an example of PTP (Press Through Package), which can be produced by simultaneously extruding or laminating a resin and glass. Figure 4 (A) and (B) are schematic cross-sectional views showing a configuration example of a packaging material formed using the sintered body or the molded body of the present embodiment as a part thereof.

[0144] like Figure 4 As shown in (A) and (B) of FIG. 4 , the packaging material 41 is a laminated body in which a resin layer 43 is laminated on a glass layer 42. The number of laminated layers is not particularly limited and may be as follows: Figure 4 The structure in which the resin layer 43 is laminated on both sides of the glass layer 42 as shown in (B) may also be as follows Figure 4 The structure formed by multiple layers is shown in (A). Figure 4 In the case of the structure shown in (A), the thickness of the glass layer 42 is preferably 1 to 50 μm, for example. Figure 4 In the case of the configuration shown in (B), the thickness of the glass layer 42 is preferably, for example, 10 μm to 3 mm.

[0145] (Color conversion member in which phosphor is dispersed)

[0146] The color conversion member dispersed with the phosphor (hereinafter also referred to as the fluorescent dispersion) is used for displays such as liquid crystal televisions or organic EL televisions, or lighting. As a method for preparing the fluorescent dispersion, for example, a method of low-temperature molding (extrusion molding or injection molding, etc.) using glass pellets in which the phosphor is pre-dispersed, a method of mixing the phosphor with glass material and then sintering, and a method of mixing the glass-coated phosphor with resin pellets and then low-temperature molding, etc. can be cited.

[0147] Figure 5(A) to (C) are schematic cross-sectional views of configuration examples of a fluorescent dispersion body formed using the sintered body or the molded body of the present embodiment as a part thereof. Figure 5 The fluorescent dispersion 51 shown in (A) is composed of a layer in which a fluorescent substance 53 is dispersed in a glass or glass resin composite 52. Figure 5 In the configuration shown in (A), the thickness of the layer in which the phosphor 53 is dispersed in the glass or glass resin composite 52 is preferably, for example, 10 μm to 3 mm.

[0148] Figure 5 The fluorescent dispersion 51 shown in (B) is a structure in which a layer in which a fluorescent substance 53 is dispersed in a glass 54 is laminated with a resin layer 55 on both sides. Figure 5 In the case of the structure shown in (B), the thickness of the layer in which the fluorescent substance 53 is dispersed in the glass 54 is preferably 10 μm to 3 mm, for example.

[0149] Figure 5 The fluorescent dispersion 51 shown in (C) is a layer in which the fluorescent body 53 covered by the coating layer 56 is dispersed in the resin 57. Figure 5 In the case of the structure shown in (C), the thickness of the layer obtained by dispersing the phosphor 53 covered by the covering layer 56 in the resin 57 is preferably 10 μm to 3 mm, for example. Figure 5 In the case of the structure shown in (C), the thickness of the coating layer 56 covering the phosphor 53 is usually preferably 0.001 μm to 1 mm. The coating layer 56 may be either organic or inorganic. In order to protect the phosphor 53 from oxygen and moisture and to improve the heat resistance of the phosphor 53, the coating layer 56 is preferably an inorganic material, and metal, silicon dioxide, aluminum oxide, zirconium oxide, or glass (especially the low melting point glass of the present invention) may be used.

[0150] (Airtight sealing material)

[0151] Figure 6 It is a schematic cross-sectional view showing a configuration example of an airtight sealing material formed using the sintered body or the molded body of the present embodiment as a part thereof. Figure 6 This is a configuration example in which glass or a glass-resin composite is used as a sealing material 61 for encapsulating a MEMS or an electronic circuit 62 in a member 63 such as metal or ceramic.

[0152] (Sealing material for vacuum multi-layer glass)

[0153] Figure 7 This is a schematic cross-sectional view showing a configuration example of a vacuum multiple glass formed using the sintered body or the molded body of the present embodiment as a part thereof. Figure 7 The vacuum multi-layered glass 71 shown has a structure in which a column 73 and a glass or glass-resin composite 74 are arranged between two sheets of glass 72 .

[0154] (Lens and Diffraction Grating)

[0155] Figure 8 (A) to (G) are schematic cross-sectional views showing a configuration example of a lens or diffraction grating 81 formed by using the sintered body or molded body of the present embodiment as a part thereof. The lens or diffraction grating 81 may be formed as follows: Figure 8 (A), (B) and (F) show a structure formed by a glass or glass resin composite 82 having a curved surface or a protruding shape according to the application. Figure 8 (C), (D) and (G) show a structure including a glass layer 83 and a resin layer 84. Figure 8 (E) shows a structure in which resin layers 84 are laminated on both surfaces of a glass layer 83. The resin layer 84 is not limited to a resin layer, and may be a layer containing an inorganic substance (for example, an AR film, etc.).

[0156] Example

[0157] Hereinafter, the present invention will be described based on Examples, but the present invention is not limited thereto.

[0158] <Glass production>

[0159] As described below, based on the glass composition as a matrix, glass raw materials were weighed, melted, and cast into a mold to obtain a glass block. The glass composition as a matrix: a composition containing 15% P, 17.5% Sn, 42.5% O, and 25% F expressed in mol%.

[0160] [Examples 1 to 12, 14]

[0161] H3PO4 (concentration 85%), SnF2, SnO, ZnF2, SiO2, BPO4, and AlF3 are used as raw materials. Each raw material is weighed in such a way that the composition of the glass obtained after the raw materials are melted becomes each composition in the table. In Examples 1 to 10, only H3PO4 is dried at 150°C for 2 hours, and in Example 12, only H3PO4 is dried at 170°C for 4 hours. Then, all the remaining raw materials are mixed in H3PO4. The mixed raw materials are melted at 500°C for 2 hours using a platinum crucible. The molten liquid is cast in a mold to obtain a glass block. For the obtained glass block, the F concentration is quantified by the ion electrode method, and the concentration of each element except F and O is quantified by the ICP emission spectrometry method. The O concentration is calculated from the difference between the total concentration of other elements and the total. The quantitative results of the composition are expressed as molar % of the element and are shown in Table 1.

[0162] [Example 13]

[0163] A glass block was obtained by the same method as in Example 1 except that NH4H2PO4, SnO and SnF2 were used as raw materials. Table 1 shows the quantitative results of the composition obtained by the same method as in Example 1.

[0164] <Evaluation>

[0165] (Tx, Tg, Tc)

[0166] The above glass block was crushed with an agate mortar to obtain a powder with a median particle size of 0.3 microns. 50 mg of the powder was measured in an aluminum pan, and the temperature was raised from 25°C to 500°C at 2°C / min in an atmospheric atmosphere using a differential scanning calorimeter (DSC3300SA manufactured by Bruker). In the DSC curve, Tg is the temperature at which the curve first endothermically changes during the heating process, Tx is the temperature at which heat is first released due to crystallization during the heating process, and Tc is the peak temperature of the heat generated by crystallization for the first time during the heating process. It should be noted that when Tx and Tc are not observed, it is recorded as "none".

[0167] (moisture absorption capacity)

[0168] The glass block was placed in an atmosphere of 60°C and 90% relative humidity for 5 hours. The weight before and after the placement was measured, and the weight increase per unit surface area was calculated as the moisture absorption. The results are shown in Table 1 as "Moisture Absorption".

[0169] (T η=1000(-60℃) , T η=1000(0℃) )

[0170] The glass block was placed in a dry nitrogen atmosphere with a dew point of -60°C using a rheometer (MCR502 manufactured by Anton Paar) to measure the temperature (T) at which the complex viscosity reached 1000 Pa·s. η=1000(-60℃) ).

[0171] The temperature (T) at which the complex viscosity reaches 1000 Pa·s was measured using a rheometer (MCR502 manufactured by Anton Paar). η=1000(0℃) ). It should be explained that

[0172] (Weight reduction rate at (Tg+150)℃)

[0173] The glass block was crushed with an agate mortar to obtain a powder with a median particle size of 0.3 microns. 50 mg of the powder was weighed in an aluminum pan and measured using a thermogravimetric-differential thermal analyzer (TG-DTA20000SA manufactured by Bruker) under the conditions of heating from 25°C to (Tg+150)°C at 2°C / min in an atmospheric atmosphere and maintaining at (Tg+150)°C for 1 hour. The weight reduction rate relative to the initial weight at this time was evaluated, and the results are shown as "loss(Tg+150)" in Table 1. It should be noted that in Table 1, blank columns indicate no evaluation.

[0174] (Infrared absorption spectrum)

[0175] The glass block was processed into a 1 mm thick plate using cerium oxide free abrasive as a polishing agent, and then the glass block was processed into a 1 mm thick plate using a Fourier transform infrared spectrophotometer (Nicolet iS10 manufactured by Thermo Fisher Scientific) at a wave number of 400 to 4000 cm -1 The range of measurement is 400 cm -1 The transmittance at T400 is set, and the wave number is set to 3100 cm -1 The transmittance at T3100 is set, and the wave number is set to 3240 cm -1 When the transmittance at is set to T3240, according to A3100 = -log 10 (T3100 / T400) Calculate the wave number 3100cm -1 The absorbance per 1mm thickness is A3100, according to A3240 = -log 10 (T3240 / T400) Calculate the wave number 3240cm -1 The absorbance A3240 per 1mm thickness.

[0176] (Parallel light transmittance)

[0177] The glass block was processed into a 1 mm thick flat plate using cerium oxide free abrasive as a polishing agent, and then the parallel light transmittance at a wavelength of 400 to 700 nm was measured using an ultraviolet-visible-near-infrared spectrophotometer (manufactured by Hitachi High-Technologies Corporation: U4100).

[0178] The results are shown in Table 1. In Table 1, Examples 1 to 8, 15, and 16 are Examples, and Examples 9 to 14 are Comparative Examples.

[0179] [Table 1]

[0180]

[0181] As shown in Table 1, the total content of Sn and Zn in Examples 1 to 8, 15 and 16 as embodiments is 18 to 21%, and the moisture absorption is lower than that in Example 9. In addition, A3240 / A3100 of Example 6 is 1.2 or less, the moisture content is controlled, and crystallization is not easy, so a transparent glass is obtained. It is estimated that Examples 1 to 5, 7, 8, 15 and 16 in which A3240 / A3100 is 1.2 or less also obtain glass with excellent transparency. In addition, since Tc is not observed in Examples 1 to 8, 15 and 16, the margin between the molding temperature and the crystallization temperature is expanded, and a glass with better transparency is obtained even when molding at a low temperature.

[0182] As a comparative example, Example 9 has Sn less than 16%, Zn more than 3%, (Sn+Zn) / P less than 1.25, and high moisture absorption. As a comparative example, Example 10 has (Sn+Zn) / P more than 1.55, and high moisture absorption. As a comparative example, Example 11 has (Sn+Zn) / P less than 1.25, and moisture absorption and T η=1000(-60℃) Higher than Examples 1 to 8. As a comparative example, Example 12 has O less than 50%, F more than 15%, and moisture absorption higher than Examples 1 to 8. As a comparative example, Example 13 has A3240 / A3100 greater than 1.2, and crystallization is not controlled, so transparent glass cannot be obtained. As a comparative example, Example 14 has P more than 16%, F less than 11%, and the differences between Tc and Tg and between Tx and Tg are narrower than those in the examples.

[0183] <Production of glass-resin composites and gas barrier properties>

[0184] A small piece of 5 mm square and 4 mm thick was cut from the glass produced in Example 6, and sandwiched between two pieces of 90 mm square and 125 μm thick polyimide resin, and pressurized at 260°C to produce a composite sheet. As a result, the bonding strength between the glass and the resin was good, and the thickness of the glass layer was 16 μm. The gas barrier properties of the composite sheet were measured using a water vapor permeability measuring device (AQUATRAN Model 1 manufactured by MOCON). As a result, the water vapor permeability was 0.8 g / m 2 / day, indicating high gas barrier properties.

[0185] A small piece of 5 mm square and 4 mm thick was cut from the glass prepared in Example 11 as a comparative example, and sandwiched between two pieces of 90 mm square and 125 micrometer thick polyimide resin, and pressurized at 260°C to prepare a composite sheet. As a result, the bonding strength between the glass and the resin was good, and the thickness of the glass layer was 10 micrometers. The gas barrier properties of the composite sheet were measured using a water vapor permeability measuring device (AQUATRAN Model 1 manufactured by MOCON). As a result, the water vapor permeability was 8.0 g / m 2 / day, indicating low gas barrier properties.

[0186] A small piece of 50 mm square and 2 mm thick was cut from the glass prepared in Example 1, and the small piece was pressed at 260°C to obtain a circular glass plate with a diameter of 90 mm and a thickness of 757 micrometers. The gas barrier properties of the glass plate were measured using a water vapor permeability measuring device (AQUATRAN Model 1 manufactured by MOCON). The water vapor permeability was 0.006 g / m 2 / day, indicating high gas barrier properties.

[0187] The glass prepared in Example 6 was pressed with a carbon mold to prepare glass pellets with a long diameter of 3 mm and a short diameter of 2.5 mm. The glass pellets and resin pellets composed of cycloolefin copolymer were extruded at 240°C using an extruder (manufactured by Soken Co., Ltd.) equipped with a T-die with a gap of 0.3 mm. As a result, a glass-resin composite sheet with a thickness of 0.1 mm was obtained. The composite sheet has high transparency, and the average value of the parallel light transmittance in the thickness direction at a wavelength of 400 to 700 nm is 75%.

[0188] As described above, this specification discloses the following matters.

[0189] 1. A glass comprising, expressed in mole percent of the elements, 12 to 16% P, 16 to 21% Sn, 50 to 60% O, 5 to 15% F, 0 to 3% Zn, 0 to 1% Si, 0 to 1% B, 0 to 1% Al, (Sn+Zn) / P being 1.25 to 1.55,

[0190] The glass transition temperature Tg is 80~200℃,

[0191] In infrared absorption spectroscopy, the wave number 3100cm -1 The absorbance per 1 mm thickness at the point is set as A3100, and the wave number is 3240 cm -1 When the absorbance per 1 mm thickness at the position is defined as A3240, A3240 / A3100 is 0.6 to 1.2.

[0192] 2. The glass according to item 1 above, wherein a temperature at which the complex viscosity reaches 1000 Pa·s measured in a dry nitrogen atmosphere at a dew point of -60°C is 190 to 260°C.

[0193] 3. The glass according to 1 or 2 above, wherein the weight increase per unit surface area when stored in an atmosphere at a temperature of 60° C. and a relative humidity of 90% for 5 hours is 5 mg / cm 2 the following.

[0194] 4. The glass according to any one of 1 to 3 above, wherein A3100 is 0.2 to 4, and A3240 is 0.12 to 4.8.

[0195] 5. The glass according to any one of 1 to 4 above, wherein the temperature at which the complex viscosity reaches 1000 Pa·s when measured in an air atmosphere with a dew point of 0°C is 10°C or more higher than the temperature at which the complex viscosity reaches 1000 Pa·s when measured in a dry nitrogen atmosphere with a dew point of -60°C.

[0196] 6. A glass frit comprising the glass according to any one of 1 to 5 above, wherein the glass has an average particle size (d50) of 0.5 to 10 μm.

[0197] 7. A pellet comprising the glass according to any one of 1 to 5 above, wherein the major diameter is 0.1 mm to 5 mm.

[0198] 8. The pellets according to item 7 above, wherein the minor diameter is 0.1 mm to 5 mm, and the ratio of the major diameter to the minor diameter is 0.2 to 1.

[0199] 9. The pellets according to item 7 or 8 above, wherein the pellets are glass-resin composite pellets obtained by composite glass and resin.

[0200] 10. A sintered body or a molded body obtained by sintering or molding the glass material or granules described in any one of 6 to 9 above.

[0201] 11. The sintered body or molded body according to 10 above, which contains an inorganic substance.

[0202] 12. The sintered body or molded body according to 10 or 11 above, which contains a phosphor.

[0203] 13. The sintered body or molded body according to any one of 10 to 12 above, which is a glass resin composite.

[0204] 14. The sintered body or molded body according to any one of 10 to 13 above, wherein the moisture absorption per unit surface area when stored in an atmosphere at a temperature of 60° C. and a relative humidity of 90% for 5 hours is 5 mg / cm 2 the following.

[0205] 15. A pharmaceutical packaging material comprising the sintered body or molded body according to any one of 10 to 14 above.

[0206] 16. A food packaging material comprising the sintered body or the molded body according to any one of 10 to 14 above.

[0207] 17. A fluorescent dispersion comprising the sintered body or the molded body according to any one of 10 to 14 above.

[0208] 18. A hermetic sealing material for MEMS or electronic circuits, comprising the sintered body or molded body according to any one of 10 to 14 above.

[0209] 19. A sealing material for vacuum multi-layer glass, comprising the sintered body or the molded body according to any one of 10 to 14 above.

[0210] 20. A lens or a diffraction grating comprising the sintered body or the molded body according to any one of 10 to 14 above.

[0211] Although the present invention is described in detail with reference to a specific mode, it is obvious that those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. It should be noted that this application is based on the Japanese patent application (Japanese Patent Application 2022-032183) filed on March 2, 2022, which is cited as a whole. In addition, all references cited are incorporated herein as a whole.

Claims

1. A glass comprising, expressed in mole percent of the elements, 12 to 16% P, 16 to 21% Sn, 50 to 60% O, 5 to 15% F, 0 to 3% Zn, 0 to 1% Si, 0 to 1% B, 0 to 1% Al, (Sn+Zn) / P being 1.25 to 1.55, having a glass transition temperature Tg of 80 to 200°C, and having a wave number of 3100 cm -1 The absorbance per 1 mm thickness at the point is set as A3100, and the wave number is 3240 cm -1 When the absorbance per 1 mm thickness at the position is defined as A3240, A3240 / A3100 is 0.6 to 1.

2.

2. The glass according to claim 1, wherein: The temperature at which the complex viscosity reaches 1000 Pa·s measured in a dry nitrogen atmosphere with a dew point of -60°C is 190 to 260°C.

3. The glass according to claim 1, wherein: The weight increase per unit surface area when stored in an atmosphere of 60°C and 90% relative humidity for 5 hours is 5 mg / cm 2 the following.

4. The glass according to claim 1, wherein: The A3100 is 0.2 to 4, and the A3240 is 0.12 to 4.

8.

5. The glass according to claim 1, wherein: The temperature at which the complex viscosity measured in an air atmosphere with a dew point of 0°C reaches 1000 Pa·s is 10°C or more higher than the temperature at which the complex viscosity measured in a dry nitrogen atmosphere with a dew point of -60°C reaches 1000 Pa·s. 6 . A glass frit comprising the glass according to claim 1 , wherein the average particle size d50 is 0.5 to 10 μm.

7. A pellet comprising the glass according to claim 1, wherein the major diameter is 0.1 mm to 5 mm.

8. The pellet according to claim 7, wherein: The short diameter is 0.1 mm to 5 mm, and the ratio of the long diameter to the short diameter is 0.2 to 1.

9. The pellet according to claim 7, wherein: The granules are glass-resin composite granules formed by compounding glass and resin.

10. A sintered body or a molded body obtained by sintering or molding the glass material or granules according to claim 6.

11. The sintered body or molded body according to claim 10, wherein: Contains inorganic substances.

12. The sintered body or molded body according to claim 10, wherein: Contains fluorescent material.

13. The sintered body or molded body according to claim 10, which is a glass-resin composite body.

14. The sintered body or molded body according to claim 10, wherein: When stored in an atmosphere of 60°C and 90% relative humidity for 5 hours, the moisture absorption per unit surface area is 5 mg / cm 2 the following. 15 . A packaging material for pharmaceuticals, comprising the sintered body or molded body according to claim 10 .

16. A food packaging material comprising the sintered body or molded body according to any one of claims 10 to 14. 17 . A fluorescent dispersion comprising the sintered body or the molded body according to claim 10 .

18. A hermetic sealing material for MEMS or electronic circuits, comprising the sintered body or molded body according to any one of claims 10 to 14.

19. A sealing material for vacuum multi-layer glass, comprising the sintered body or the molded body according to any one of claims 10 to 14.

20. A lens or a diffraction grating comprising the sintered body or the molded body according to any one of claims 10 to 14.

Citation Information

Patent Citations

  • Durable tungsten-doped tin-fluorophosphate glasses

    CN101522585A

  • Fluorinated tin-based glass frit and method for manufacturing same

    CN108473363A

  • Low melting point glass

    JP2001048574A

  • SnO-P2O5-B2O3-BASED PHASE-SEPARATED GLASS

    JP2011121818A

  • Phosphor composite member, LED device and method for manufacturing phosphor composite member

    WO2012008306A1