Slurry composition and coating agent

By using a combination of La-based composite oxide particles with a median particle diameter of less than 800nm, dispersion media, binders and ultraviolet curable resins, the problem of fast settling speed of lanthanum and molybdenum composite oxide ceramic powders is solved and effective Improved coating and adhesion.

CN118786186APending Publication Date: 2024-10-15NITERRA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380014793.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The complex oxide ceramic powder containing lanthanum and molybdenum has high specific gravity, which leads to problems of fast settling speed and rapid solid-liquid separation, making it difficult to effectively coat.

Method used

La-type composite oxide particles with a median particle diameter of less than 800nm ​​are used, with a content rate of 0.1% to 10%, and are combined with a dispersion medium, a binder and an ultraviolet curable resin to form a slurry composition and coating agent that retards settling. .

Benefits of technology

It effectively delays the settling speed of La-based composite oxide particles, improves their dispersion and adhesion during the coating process, and ensures the coating effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786186A_ABST
    Figure CN118786186A_ABST
Patent Text Reader

Abstract

[Solution] This slurry composition contains particles of a composite oxide containing La and at least one element selected from the group consisting of Mo and W, and a dispersion medium, the particles having a median particle diameter of 800 nm or less, and the content of the particles being 0.1-10 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a slurry composition and a coating agent. Background Art

[0002] As shown in Patent Document 1, ceramics composed of composite oxides containing rare earths and molybdenum (Mo) are known as novel inorganic materials having antibacterial and antiviral properties. Among such ceramics, ceramics composed of composite oxides containing lanthanum (La) as a rare earth (e.g., La2Mo2O9) have attracted particular attention because lanthanum, which is cheap and easily available among rare earths, is used and is therefore advantageous for industrial production.

[0003] It should be noted that Patent Document 1 shows that a film containing a composite oxide ceramic can be formed by combining ceramic powder containing a composite oxide of lanthanum and molybdenum with a known binder resin, solvent, etc. to prepare ink or paste, and applying it on the surface of a desired article.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2020 / 017493

[0007] Problems to be solved by the invention

[0008] Conventionally, the antibacterial or antiviral property is imparted by making a powder having antibacterial or antiviral property such as silver powder into a slurry and using the slurry as a coating agent or mixing it into a paint or the like.

[0009] However, no such research has been conducted on ceramic powders such as the composite oxide containing lanthanum and molybdenum. The specific gravity of the composite oxide containing lanthanum and molybdenum is relatively large, at 5.5 / cm 3 , so there are problems such as fast powder sedimentation rate and fast solid-liquid separation. Summary of the invention

[0010] An object of the present invention is to provide a slurry composition and a coating agent in which the sedimentation rate of La-based composite oxide particles is slowed.

[0011] Means for solving problems

[0012] The present inventors have conducted intensive studies to achieve the above-mentioned purpose and have found that when the median particle size of particles of a composite oxide comprising at least one element selected from the group consisting of Mo and W is 800 nm or less and the content of the particles is 0.1% by mass to 10% by mass, the sedimentation rate of the particles is slowed down and the particles can be applied to an object, thereby completing the present invention.

[0013] The means for solving the above-mentioned problems are as follows.

[0014] <1> A slurry composition comprising particles of a composite oxide and a dispersion medium, wherein the composite oxide contains La and at least one element selected from the group consisting of Mo and W, wherein the median particle size of the particles is 800 nm or less and the content of the particles is 0.1 mass % to 10 mass %.

[0015] <2> According to the <1> The slurry composition described, wherein the composite oxide is La2Mo x W (2-X) O9(0≦x≦2).

[0016] <3> According to the <1> or <2> The slurry composition described herein contains a binder.

[0017] <4> According to the <1> ~ <3> The slurry composition according to any one of claims , wherein the slurry composition contains a dispersant.

[0018] <5> According to the <1> ~ <4> The slurry composition according to any one of the above, wherein the slurry composition contains an ultraviolet curable resin.

[0019] <6> A coating agent, the coating agent comprising <1> ~ <5> The slurry composition according to any one of the above.

[0020] Effects of the Invention

[0021] According to the present invention, a slurry composition and a coating agent in which the sedimentation rate of La-based composite oxide particles is slowed can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] [ Figure 1 ] is a diagram showing a SEM image of the La-Mo based composite oxide particles of Example 2.

[0023] [ Figure 2 ] is a diagram showing a photograph of the appearance of each slurry composition of Examples 1 and 2.

[0024] [ Figure 3 ] is a photograph showing the appearance of the slurry composition of Comparative Example 1 filled in a vial.

[0025] [ Figure 4 ] is a photograph showing the appearance of the slurry composition of Example 15.

[0026] [ Figure 5 ] is a graph showing the transmittance (%) curve of the slurry composition of Example 2.

[0027] [ Figure 6 is a diagram showing a SEM image of La-Mo composite oxide particles of Comparative Example 2. Detailed implementation mode

[0028] The slurry composition of the present implementation mode is a liquid composition containing particles of La-based composite oxide and a dispersion medium.

[0029] In this specification, a composite oxide containing La and at least one element selected from the group consisting of Mo and W is represented as "La-based composite oxide". Such La-based composite oxides have excellent antibacterial and antiviral properties.

[0030] The La-based composite oxide is, for example, composed of La2Mo x W (2-X) O9 (0 ≦ x ≦ 2).

[0031] As specific La-based composite oxides, for example, La-Mo composite oxides, La-Mo-W composite oxides, and La-W composite oxides can be cited.

[0032] As the La-Mo composite oxide, from the viewpoints of antibacterial and antiviral properties, etc., it is preferable to contain Mo as the element. That is, as the La-based composite oxide, it is preferably a composite oxide represented by La2Mo x W (2-X) O9 (0 < x ≦ 2).

[0033] It should be noted that in this specification, particles of La-based composite oxide (i.e., particulate La-based composite oxide) are represented as "La-based composite oxide particles".

[0034] In this specification, a composite oxide of lanthanum (La) and molybdenum (Mo) is represented as "La-Mo composite oxide", and in addition, particles of La-Mo composite oxide (i.e., particulate La-Mo composite oxide) are represented as "La-Mo composite oxide particles".

[0035] In addition, in this specification, a composite oxide of lanthanum (La), molybdenum (Mo), and tungsten (W) is represented as "La-Mo-W composite oxide", and in addition, particles of La-Mo-W composite oxide (i.e., particulate La-Mo-W composite oxide) are represented as "La-Mo-W composite oxide particles".

[0036] In addition, in this specification, a composite oxide of lanthanum (La) and tungsten (W) is represented as "La-W composite oxide", and in addition, particles of La-W composite oxide (i.e., particulate La-W composite oxide) are represented as "La-W composite oxide particles".

[0037] The median particle size of the La-based composite oxide particles is 800 nm or less, preferably 600 nm or less, more preferably 150 nm or less, and further preferably 100 nm or less. When the median particle size of the La-based composite oxide particles is within such a range, the sedimentation rate of the La-based composite oxide particles in the dispersion medium is sufficiently slowed, thereby improving the dispersibility of the La-based composite oxide particles and enabling the slurry composition to be applied to an object.

[0038] The median particle size of the La-based composite oxide particles is determined as the particle size (D50) when the cumulative frequency based on the laser diffraction method reaches 50%. The specific method for measuring the median particle size using a laser diffraction particle size distribution analyzer will be described later.

[0039] It should be noted that in the determination of the median particle size using the particle size distribution measuring device, when the measurement result is lower than the lower limit of the measurement limit, the correct particle size (median particle size) cannot be obtained. Therefore, when the measurement result based on the particle size distribution measuring device is less than 100nm, on the basis of the measurement method using the particle size distribution measuring device, FE-SEM (Field Emission-Scanning Electron Microscope) is also used to measure the particle size. As a measurement method using FE-SEM, for example, the La-based composite oxide powder in the slurry composition can be attached to the surface of an appropriate object, and the La-based composite oxide powder contained in the attachment can be obtained. It should be noted that the specific particle size measurement method using FE-SEM is described later.

[0040] The La-Mo composite oxide is not particularly limited unless the purpose of the present invention is impaired, and examples thereof include La 2 Mo 2 O 9 . The La-Mo composite oxide may consist of only La 2 Mo 2 O 9 , or may contain substances other than La 2 Mo 2 O 9 .

[0041] The La-Mo-W composite oxide is not particularly limited unless the purpose of the present invention is impaired. Examples thereof include La2MoWO9, La2Mo 1.5 W 0.5 O9, La2Mo 0.5 W 1.5 O9, etc. These composite oxides may be used alone or in combination of two or more.

[0042] The La-W composite oxide is not particularly limited unless the purpose of the present invention is impaired, and examples thereof include La 2 W 2 O 9 . The La-W composite oxide may be composed of La 2 W 2 O 9 alone, or may contain substances other than La 2 W 2 O 9 .

[0043] La-based composite oxide particles such as La—Mo-based composite oxide particles are produced, for example, through a preparation step, a first calcination step, and a pulverization step.

[0044] When the La-based composite oxide particles are La-Mo-based composite oxide particles, the preparation step is a step of mixing a lanthanum compound and a molybdenum compound to prepare a mixed powder.

[0045] When the La-based composite oxide particles are La-Mo-W-based composite oxide particles, the preparation step is a step of mixing a lanthanum compound, a molybdenum compound, and a tungsten compound to prepare a mixed powder.

[0046] When the La-based composite oxide particles are La-W-based composite oxide particles, the preparation step is a step of mixing a lanthanum compound and a tungsten compound to prepare a mixed powder.

[0047] Lanthanum compounds are compounds containing lanthanum (La) necessary for producing La-based composite oxides such as La-Mo-based composite oxides, and examples thereof include La(OH)3, La2O3, La2(CO3)3, etc. As the lanthanum compound, for example, at least one selected from the group consisting of La(OH)3, La2O3, and La2(CO3)3 can be used. It should be noted that as the lanthanum compound, La(OH)3 is preferred.

[0048] The molybdenum compound is a compound containing molybdenum (Mo) necessary for producing La-Mo composite oxides or La-Mo-W composite oxides, and examples thereof include MoO3, MoO2, MoO, Mo(OH)3, Mo(OH)5, etc. As the molybdenum compound, for example, at least one selected from the group consisting of MoO3, MoO2, MoO, Mo(OH)3, and Mo(OH)5 can be used. It should be noted that as the molybdenum compound, MoO3 is preferred.

[0049] The tungsten compound is a compound containing tungsten (W) necessary for producing La-Mo-W composite oxide or La-W composite oxide, and examples thereof include WO3, WO2, and W2O3. It should be noted that WO3 is preferred as the tungsten compound.

[0050] The mixing ratio of the lanthanum compound and the molybdenum compound when producing the La—Mo-based composite oxide is preferably adjusted to a molar ratio of La:Mo=1:1.

[0051] The mixing ratio of the lanthanum compound, the molybdenum compound and the tungsten compound when preparing the La—Mo—W composite oxide is preferably adjusted to a molar ratio of La:Mo:W=2:1.5-0.5:0.5-1.5.

[0052] The mixing ratio of the lanthanum compound and the tungsten compound when preparing the La—W-based composite oxide is preferably adjusted to La:W=2:1.5 to 0.5:0.5 to 1.5 in terms of molar ratio.

[0053] The raw materials of La-based composite oxides such as lanthanum compounds, molybdenum compounds, and tungsten compounds are all powders, and they can be mixed in a powder state, or a solvent such as a lower alcohol (ethanol) can be added to these powders for wet mixing. The mixing of the raw materials can be carried out, for example, by wet mixing using alumina balls (alumina pebbles) or the like. It should be noted that the wet-mixed mixture (wet mixture) can be appropriately dried by hot water bath drying, spray drying, etc.

[0054] Through such a preparation process, a mixed powder of a lanthanum compound and a molybdenum compound, a mixed powder of a lanthanum compound, a molybdenum compound and a tungsten compound, or a mixed powder of a lanthanum compound and a tungsten compound can be obtained.

[0055] The first calcination step is a step of calcining the mixed powder in order to react the lanthanum compound and the molybdenum compound in the mixed powder obtained in the preparation step. The first calcination step is, for example, to calcine the mixed powder for more than 1 hour at a temperature of 500° C. to 900° C. It should be noted that the first calcination step is performed under a normal atmospheric pressure atmosphere and does not need to be performed under a special synthetic air atmosphere.

[0056] When the mixed powder is a mixed powder of a lanthanum compound and a molybdenum compound, the lanthanum compound and the molybdenum compound in the mixed powder are reacted with each other through the first calcination step to obtain a La-Mo-based composite oxide including La2Mo2O9 and the like.

[0057] When the mixed powder is a mixed powder of a lanthanum compound, a molybdenum compound and a tungsten compound, the lanthanum compound, the molybdenum compound and the tungsten compound in the mixed powder are reacted to obtain a La-Mo-W type composite oxide including La2MoWO9 and the like.

[0058] When the mixed powder is a mixed powder of a lanthanum compound and a tungsten compound, the lanthanum compound and the tungsten compound in the mixed powder are reacted to obtain a La-W based composite oxide including La2W2O9 and the like.

[0059] The pulverization step is a step of pulverizing the La-based composite oxide after the first calcination using a media agitation pulverization device such as a bead mill so that the median particle size thereof is within a predetermined range. The pulverization time and other conditions are appropriately set so that the median particle size of the La-based composite oxide is within a predetermined range.

[0060] As described above, La-based composite oxide particles such as La—Mo-based composite oxide particles having a predetermined median particle size to be used in the slurry composition are obtained.

[0061] It should be noted that the obtained La-based composite oxide particles can be granulated as needed. For example, by adding a solvent such as ethanol to the La-based composite oxide particles, wet mixing and crushing using alumina balls, etc., to prepare a slurry, and passing the dried product of the slurry through a sieve with a predetermined mesh size to obtain La-based composite oxide particles granulated to a predetermined size.

[0062] In addition, as long as the present invention is not impaired, after sintering the La-based composite oxide particles, the obtained sintered body may be crushed, and the obtained product (crushed product) may be used as the "La-based composite oxide particles" used in the slurry composition. The sintered body is obtained, for example, by forming the La-based composite oxide particles before sintering into a predetermined shape and sintering the obtained molded body under predetermined temperature conditions (for example, above 900°C). In this specification, the sintering process performed for sintering the La-based composite oxide particles is referred to as the "second sintering process". The second sintering process can be performed under an atmospheric atmosphere. It should be noted that, as needed, the La-based composite oxide obtained after the second sintering process can be adjusted to a particle state having a median particle size in a predetermined range through a pulverizing process.

[0063] As the dispersion medium used in the slurry composition, water, ethanol, isopropyl alcohol (IPA), methyl ethyl ketone (MEK), ethyl acetate, toluene, etc. can be used. These can be used alone or in combination of two or more.

[0064] The content of the La-based composite oxide particles in the slurry composition is 0.1% by mass to 10% by mass.

[0065] The slurry composition may contain other components in addition to the La-based composite oxide particles and the dispersion medium unless the object of the present invention is impaired.

[0066] Examples of other components (compounds) include a binder, a dispersant, an ultraviolet curable resin, a colorant (pigment, dye), etc. Components other than these may also be used as other components.

[0067] The binder is used for the purpose of improving the adhesion between the La-based composite oxide particles contained in the slurry composition and the object. As such a binder, there is no particular limitation as long as it does not impair the purpose of the present invention, and examples thereof include polyvinyl alcohol (PVA), polyvinyl butyral (PVB), etc. These substances can be used alone or in combination of two or more.

[0068] The content of the binder in the slurry composition is not particularly limited unless the object of the present invention is impaired, but is preferably 0.05% by mass to 5% by mass based on the La-based composite oxide particles, for example.

[0069] The dispersant is used for the purpose of improving the dispersibility of the La-based composite oxide particles in the dispersion medium. As such a dispersant, there is no particular limitation as long as it does not impair the purpose of the present invention, and examples thereof include: water-soluble acrylic dispersants, anionic surfactants, cationic surfactants, nonionic surfactants, polyethylene glycol (PEG)-polypropylene glycol (PPG) block polymers, polyacrylic acid ammonium salts, polycarboxylic acid copolymers having alkyl chains or polyalkylene glycol (PAG) chains, etc. These dispersants can be used alone or in combination of two or more.

[0070] The content of the dispersant in the slurry composition is not particularly limited unless the object of the present invention is impaired. For example, it is preferably 5% by mass or less based on the La-based composite oxide particles.

[0071] The slurry composition of the present embodiment can be used as a coating agent by containing a curing agent. As a curing agent, as long as the purpose of the present invention is not impaired, any curing agent such as a curing agent formed by dissolving a synthetic resin in a volatile solvent, a moisture-curing curing agent, a two-liquid mixed curing agent, and an ultraviolet curing curing agent can be selected. The curing agent is used for the purpose of improving the adhesion of the La-based composite oxide particles contained in the slurry composition to the object. As the ultraviolet curing resin used in the ultraviolet curing curing agent, for example, acrylic ultraviolet curing resins can be cited.

[0072] The content of the ultraviolet curable resin in the slurry composition is not particularly limited unless the object of the present invention is impaired. For example, it is preferably 5% by mass or less based on the La-based composite oxide particles.

[0073] In addition, the slurry composition (coating agent) of the present embodiment may also contain a pigment. The pigment is used for the purpose of coloring the coating film containing La-based composite oxide particles formed on the surface of the object. The pigment may be water-based or oily. There are no particular restrictions on the pigment, and examples thereof include carbon black, synthetic resins, metal powders, minerals, etc. These substances may be used alone or in combination of two or more.

[0074] There are no particular restrictions on the object to which the slurry composition is applied. Examples of the material constituting the object include glass, ceramics, synthetic resins such as thermoplastic resins and thermosetting resins, rubber (natural rubber, synthetic rubber), genuine leather (natural leather), synthetic leather, metal materials composed of metals or alloys, wood, paper, fiber, nonwoven fabrics, silicon (silicon wafers, etc.), carbon materials, minerals, and the like.

[0075] As a method for applying the slurry composition to an object, for example, a brush, a roller, a scraper casting, or dipping can be used. As a method for drying the slurry composition after applying it to an object, known methods such as natural drying and heating in a drying furnace can be used. At this time, it is preferred to select a method for suppressing the aggregation of La-based composite oxide particles.

[0076] The present invention will be further described below based on examples. It should be noted that the present invention is not limited to these examples.

[0077] [Example 1]

[0078] La(OH)3 was prepared as a lanthanum compound, and MoO3 was prepared as a molybdenum compound. Then, the raw material powder of the lanthanum compound and the raw material powder of the molybdenum compound were weighed respectively so that the molar ratio was 1:1 (La:Mo=1:1). The weighed raw material powders were mixed with a predetermined amount of ethanol, and the obtained wet mixture was dried to obtain a mixed powder.

[0079] Next, the mixed powder was calcined under an air atmosphere at a temperature of 700° C. for 10 hours to obtain a calcined powder consisting of a reaction product of a lanthanum compound and a molybdenum compound.

[0080] Then, the obtained calcined powder was pulverized by a bead mill for 4.5 hours to obtain La-Mo composite oxide particles. It should be noted that the median particle size of the La-Mo composite oxide particles of Example 1 is 100 nm or less. The method for measuring the median particle size is described below.

[0081] The La—Mo-based composite oxide particles were blended in water (dispersion medium) so that the solid content concentration in the finally obtained slurry composition became 1 mass %, and the mixture was stirred to obtain a slurry composition of Example 1.

[0082] [Example 2]

[0083] A slurry composition of Example 2 was obtained by the same method as in Example 1 except that a dispersant was blended (1% by mass relative to the La-Mo-based composite oxide particles).

[0084] [Example 3]

[0085] A slurry composition of Example 3 was obtained by the same method as in Example 1 except that a binder and a dispersant were added (0.1 mass % (binder) and 1 mass % (dispersant) relative to the La—Mo-based composite oxide particles).

[0086] [Example 4]

[0087] A slurry composition of Example 4 was obtained by the same method as Example 1 except that an ultraviolet curable resin and a dispersant (0.1 mass % (ultraviolet curable resin) and 1 mass % (dispersant) relative to the La—Mo composite oxide particles) were added.

[0088] [Example 5]

[0089] The La-Mo type composite oxide particles are mixed in water (dispersion medium) so that the solid content concentration in the final slurry composition becomes 8 mass %, and a dispersant (1 mass % relative to the La-Mo type composite oxide particles) is mixed. Except for this, the slurry composition of Example 5 is obtained by the same method as Example 1.

[0090] [Example 6]

[0091] A calcined powder was prepared by the same method as in Example 1, and the calcined powder was pulverized by a pot mill for 90 hours to obtain La-Mo composite oxide particles of Example 6. It should be noted that the median particle size of the La-Mo composite oxide particles of Example 6 was 600 nm. The method for measuring the median particle size is described below.

[0092] The La-Mo type composite oxide particles of Example 6 are mixed in water (dispersion medium) so that the solid content concentration in the final slurry composition becomes 1 mass %, and a dispersant (1 mass % relative to the La-Mo type composite oxide particles) is further mixed, and the mixture is stirred to obtain the slurry composition of Example 6.

[0093] [Example 7]

[0094] A calcined powder was prepared in the same manner as in Example 1, and the calcined powder was pulverized by a bead mill for 4.5 hours to obtain La—Mo based composite oxide particles of Example 7. The median particle size of the La—Mo based composite oxide particles of Example 6 was 150 nm.

[0095] The La-Mo type composite oxide particles are mixed in ethanol (dispersion medium) so that the solid content concentration in the final slurry composition becomes 1 mass %, and a dispersant (1 mass % relative to the La-Mo type composite oxide particles) is further mixed, and the mixture is stirred to obtain the slurry composition of Example 7.

[0096] [Example 8]

[0097] A calcined powder was prepared in the same manner as in Example 1, and the calcined powder was pulverized in a pot mill for 75 hours to obtain La—Mo based composite oxide particles of Example 8. The median particle size of the La—Mo based composite oxide particles of Example 8 was 800 nm.

[0098] The La-Mo type composite oxide particles are mixed in water (dispersion medium) so that the solid content concentration in the final slurry composition becomes 1 mass %, and a dispersant (1 mass % relative to the La-Mo type composite oxide particles) is further mixed, and the mixture is stirred to obtain the slurry composition of Example 8.

[0099] [Example 9]

[0100] A calcined powder was prepared in the same manner as in Example 1, and the calcined powder was pulverized in a pot mill for 70 hours to obtain La—Mo based composite oxide particles of Example 9. The median particle size of the La—Mo based composite oxide particles of Example 9 was 800 nm.

[0101] The La-Mo type composite oxide particles are mixed in water (dispersion medium) so that the solid content concentration in the final slurry composition becomes 10 mass %, and a dispersant (1 mass % relative to the La-Mo type composite oxide particles) is further mixed, and the mixture is stirred to obtain the slurry composition of Example 9.

[0102] [Example 10]

[0103] As a lanthanum compound, La(OH)3 was prepared, as a molybdenum compound, MoO3 was prepared, and as a tungsten compound, WO3 was prepared. Then, the raw material powder of the lanthanum compound, the raw material powder of the molybdenum compound, and the raw material powder of the tungsten compound were weighed respectively so that the molar ratio was 2:1:1 (La:Mo:W=2:1:1). The weighed raw material powders were mixed with a predetermined amount of ethanol, and the obtained wet mixture was dried to obtain a mixed powder.

[0104] Next, the mixed powder was fired at 650° C. for 10 hours in an air atmosphere to obtain a fired powder consisting of a reaction product of a lanthanum compound, a molybdenum compound, and a tungsten compound.

[0105] Then, the obtained calcined powder was pulverized for 6 hours using a bead mill to obtain particles of La-Mo-W composite oxide. It should be noted that the median particle size of the particles of Example 10 was 100 nm or less.

[0106] The particles of the La—Mo—W composite oxide were mixed with water (dispersion medium) so that the solid content concentration in the finally obtained slurry composition became 1 mass %, and the mixture was stirred to obtain a slurry composition of Example 10.

[0107] [Example 11]

[0108] The raw powders of the lanthanum compound, the molybdenum compound and the tungsten compound were weighed respectively so that the molar ratio was 2:1.5:0.5 (La:Mo:W=2:1.5:0.5) to prepare the wet mixture. Except for this, the slurry composition of Example 11 was obtained by the same method as Example 10.

[0109] [Example 12]

[0110] The raw powders of the lanthanum compound, the molybdenum compound and the tungsten compound were weighed respectively so that the molar ratio was 2:0.5:1.5 (La:Mo:W=2:0.5:1.5) to prepare the wet mixture. Except for this, the slurry composition of Example 12 was obtained by the same method as Example 10.

[0111] [Example 13]

[0112] A calcined powder was prepared in the same manner as in Example 10, and the calcined powder was pulverized in a pot mill for 75 hours to obtain particles of La-Mo-W composite oxide of Example 13. The median particle size of the particles of Example 13 was 800 nm.

[0113] The particles of the La—Mo—W composite oxide were blended in water (dispersion medium) so that the solid content concentration in the finally obtained slurry composition became 10 mass %, and the mixture was stirred to obtain a slurry composition of Example 13.

[0114] [Example 14]

[0115] La(OH)3 was prepared as a lanthanum compound, and WO3 was prepared as a tungsten compound. Then, the raw material powder of the lanthanum compound and the raw material powder of the tungsten compound were weighed respectively so that the molar ratio was 1:1 (La:W=1:1). The weighed raw material powders were mixed with a predetermined amount of ethanol, and the obtained wet mixture was dried to obtain a mixed powder.

[0116] Next, the mixed powder was fired at 700° C. for 10 hours in an air atmosphere to obtain a fired powder consisting of a reaction product of a lanthanum compound and a tungsten compound.

[0117] Then, the obtained calcined powder was pulverized for 4.5 hours using a bead mill to obtain particles of La-W-based composite oxide. It should be noted that the median particle size of the particles of Example 14 was 100 nm or less.

[0118] The particles of the La—W-based composite oxide were blended in water (dispersion medium) so that the solid content concentration in the finally obtained slurry composition became 1 mass %, and the mixture was stirred to obtain a slurry composition of Example 14.

[0119] [Example 15]

[0120] A calcined powder was prepared in the same manner as in Example 14, and the calcined powder was pulverized in a pot mill for 75 hours to obtain particles of La—W composite oxide of Example 15. The median particle size of the particles of Example 15 was 800 nm.

[0121] The La—W composite oxide particles were blended in water (dispersion medium) so that the solid content concentration in the finally obtained slurry composition became 1 mass %, and the mixture was stirred to obtain a slurry composition of Example 15.

[0122] [Comparative Example 1]

[0123] A calcined powder was prepared in the same manner as in Example 1, and the calcined powder was pulverized in a pot mill for 15 hours to obtain La—Mo based composite oxide particles of Comparative Example 1. The median particle size of the La—Mo based composite oxide particles of Comparative Example 1 was 2300 nm.

[0124] The La—Mo-based composite oxide particles were blended in water (dispersion medium) so that the solid content concentration in the finally obtained slurry composition became 1 mass %, and the mixture was stirred to obtain a slurry composition of Comparative Example 1.

[0125] [Comparative Example 2]

[0126] A calcined powder was prepared in the same manner as in Example 1, and the calcined powder was pulverized in a pot mill for 90 hours to obtain La—Mo based composite oxide particles of Comparative Example 2. The median particle size of the La—Mo based composite oxide particles of Comparative Example 2 was 600 nm.

[0127] The La-Mo type composite oxide particles are mixed in water (dispersion medium) so that the solid content concentration in the final slurry composition becomes 20 mass %, and a dispersant (1 mass % relative to the La-Mo type composite oxide particles) is further mixed, and the mixture is stirred to obtain the slurry composition of Comparative Example 2.

[0128] [Measurement of median particle size (D50) by laser diffraction method]

[0129] The median particle size (D50) of the particles of the La-based composite oxides (La-Mo-based composite oxides, La-Mo-W-based composite oxides, and La-W-based composite oxides) of Examples 1 to 15 and Comparative Examples 1 to 2 was measured using a laser diffraction particle size distribution device (model "LA-950", manufactured by Horiba, Ltd.). The measurement conditions are as follows.

[0130] <Measurement Conditions>

[0131] An aqueous solution of sodium hexametaphosphate having a concentration of 2% by mass is referred to as solution A. In addition, La-based composite oxide particles (to be measured) are added to an aqueous solution of sodium hexametaphosphate having a concentration of 2% by mass, and the mixture is stirred with a homogenizer to uniformly disperse the La-based composite oxide particles, and the resultant is referred to as solution B. 0.5 mL of solution B is added dropwise to solution A to prepare a solution C in which the concentration of La-based composite oxide particles is 1% by mass or less and the La-based composite oxide particles are monodispersed. Then, using this solution C, a particle size (D50) is obtained as the median particle size when the cumulative frequency becomes 50% by a laser diffraction particle size distribution device. The measurement results of the median particle size (D50) in each embodiment are shown in Table 1.

[0132] It should be noted that the measurement results (median particle size) of the La-Mo-based composite oxide particles in Examples 1 to 5, the measurement results (median particle size) of the La-Mo-W-based composite oxide particles in Examples 10 to 12, and the measurement results (median particle size) of the La-W-based composite oxide particles in Example 14 were 100 nm or less. Therefore, for Examples 1 to 5, 10 to 12, and 14, the particle sizes were measured using FE-SEM as follows.

[0133] [Particle size measurement using FE-SEM]

[0134] The particle size of the La-based composite oxide particles of Examples 1 to 5, 10 to 12, and 14 was determined by FE-SEM according to the following operating procedures. Here, the slurry composition of Example 2 was dripped onto a carbon tape and dried for use as a measurement object. It should be noted that in order to suppress the aggregation of particles during drying, a dispersion medium (water, etc.) was appropriately added to dilute the dripped slurry composition so that single particles in the slurry composition could be observed. Figure 1 This is a diagram showing an SEM image of the La-Mo type composite oxide particles (La type composite oxide particles) of Example 2. An SEM image (magnification: 100,000) of the La-Mo type composite oxide particles of Example 2 is obtained, and a plurality of single particles of the La-Mo type composite oxide particles are extracted from the SEM image as a sample using predetermined image analysis software. Then, using the analysis software WinROOF2018, the equivalent circle diameter (μm) is calculated from the image of each extracted single particle. From the results of the plurality of equivalent circle diameters (μm) thus obtained, the particle size (average particle size) of the La-Mo type composite oxide particles is calculated. As a result, the particle size (average particle size) of the La-Mo type composite oxide powder of Examples 1 to 5 is 0.05 μm (50 nm, reference value)).

[0135] [Appearance and Redispersion of Slurry Composition]

[0136] like Figure 2 As shown, 30 ml of each slurry composition was added to a vial with a capacity of 50 ml, and ultrasonic vibration was applied for 10 minutes using a desktop ultrasonic cleaning machine (product name "US-KS", manufactured by SND). Then, the appearance of the slurry composition was visually observed to confirm the color and the presence of precipitation. In addition, whether the La-based composite oxide particles after dispersion were precipitated was judged to determine whether they could be redispersed. The results are shown in Table 1.

[0137] in addition, Figure 2 The appearance photos of the slurry compositions of Examples 1 and 2 are shown in FIG. Figure 3 The appearance photograph of the slurry composition of Comparative Example 1 is shown in FIG. Figure 4 A photograph of the appearance of the slurry composition of Example 15 is shown in FIG.

[0138] [precipitation]

[0139] After applying ultrasonic vibration to each slurry composition as described above, each slurry composition was allowed to stand. The appearance of each slurry composition after standing for 10 minutes was observed to determine whether precipitation occurred.

[0140] [Transmittance of slurry composition]

[0141] The transmittance τ of the slurry composition of Example 2 was determined by the following method. The transmittance τ of the composition of Example 2 was calculated from τ=10 -a Where a is the absorbance of the solid content in the slurry composition. The absorbance a is calculated by a=a n -a0 is calculated. Here, a n represents the absorbance of the slurry composition of Example 2, and a0 represents the absorbance of water alone (blank). n The absorbance a0 was measured using an ultraviolet-visible spectrophotometer under the following measurement conditions.

[0142] <Measurement Conditions>

[0143] Measurement device: UV-visible spectrophotometer manufactured by LMS (model: Evolution 201)

[0144] Measurement range: 360nm~800nm ​​(visible light region)

[0145] Scanning speed: 1200.00nm / min

[0146] Data interval: 1nm

[0147] Integration time: 0.050sec

[0148] Bandwidth: 1nm

[0149] Baseline correction: 100% T

[0150] Figure 5 The results of the transmittance (%) of the slurry composition of Example 2 are shown in FIG. Figure 5 The horizontal axis represents wavelength (nm), and the vertical axis represents transmittance (%). It should be noted that the maximum value of the transmittance (%) is 100%, and the minimum value is 97.6%.

[0151] [Fixedness]

[0152] Use a pipette to drip 2 ml of each slurry composition of Example 1, etc. onto the surface of the glass substrate, and evaporate the dispersion medium. It should be noted that in the case of Example 4, after the slurry composition is attached to the surface of the substrate, ultraviolet rays are irradiated for 30 seconds. The adhesive surface of the adhesive tape is pasted on the slurry composition attached to the surface of the substrate, and then the adhesive tape is peeled off, thereby confirming whether the slurry composition is peeled off from the surface of the substrate using SEM. Such a tape stripping test is performed up to 20 times for each slurry composition. When the number of tape stripping tests is less than 3 times, the slurry composition is peeled off, and the result is expressed as "1". In addition, when the number of tape stripping tests is more than 4 times and less than 10 times, the slurry composition is peeled off, and the result is expressed as "2". In addition, when the number of tape stripping tests is more than 11 times and the slurry composition is not peeled off, the result is expressed as "3". The results are shown in Table 1.

[0153] [Agglomeration after coating and drying]

[0154] 2 ml of each slurry composition of Example 1 etc. was dripped onto the surface of the glass substrate using a pipette, and then the dispersion medium was evaporated. The image was obtained using a scanning electron microscope with an accelerating voltage of 5 kV. The magnification was appropriately adjusted according to the size of the condensed particles. In the image obtained by the scanning electron microscope, the situation where the particles were continuous for more than 50 μm was defined as "condensation". The results are shown in Table 1. Figure 6 This is a SEM image (magnification: 500) showing a state in which La—Mo-based composite oxide particles (La-based composite oxide particles) of Comparative Example 2 are attached to the surface of a substrate.

[0155]

[0156] As shown in Table 1, each slurry composition of Examples 1 to 9 can be redispersed in a state after applying ultrasonic vibration for 10 minutes. The slurry compositions of Examples 2, 3, and 4 are transparent, the slurry compositions of Examples 1, 5, and 7 are translucent, and the slurry compositions of Examples 6, 8, and 9 are turbid. Each slurry composition of Examples 1 to 9 can be applied to an object. In addition, even after standing for 10 minutes, no precipitation of La-Mo-based composite oxide particles was observed in each slurry composition of Examples 1 to 9. In addition, for each slurry composition of Examples 1 to 9, in a state where the dispersion medium was evaporated after being applied to the object, no continuous state of particles exceeding 50 μm was observed, and thus no aggregation of La-Mo-based composite oxide particles was confirmed.

[0157] On the other hand, in the slurry composition of Comparative Example 1, the La-Mo composite oxide particles and the dispersion medium separated into two layers and could not be dispersed again when ultrasonic vibration was applied for 10 minutes. Therefore, the slurry composition of Comparative Example 1 could not be applied to the object. This is believed to be because the median particle size of the La-Mo composite oxide particles involved in Comparative Example 1 was 2300 nm.

[0158] In addition, the slurry composition of Comparative Example 2 was turbid in the state after applying ultrasonic vibration for 10 minutes, and the La-Mo composite oxide particles were able to be redispersed. However, after the application of ultrasonic vibration was completed, the La-Mo composite oxide particles were precipitated after being left to stand for 10 minutes. Figure 5 As shown in FIG. 1 , after the application to the object was dried, aggregation of the La-Mo composite oxide particles was observed. This is believed to be because the concentration of the La-Mo composite oxide particles in the slurry composition according to Comparative Example 2 was 20 mass %.

[0159] In addition, it was confirmed that the slurry composition of Example 4 containing an ultraviolet curable resin had the best fixation (adhesion) to the object. In addition, it was confirmed that the slurry composition of Example 3 containing a binder in the composition also had excellent fixation (adhesion) to a certain extent.

[0160] In addition, as shown in Table 1, each slurry composition of Examples 10 to 15 can be redispersed in the state after applying ultrasonic vibration for 10 minutes, similarly to the above-mentioned Example 1, etc. The slurry compositions of Examples 10, 11, 12, and 14 are translucent in the same manner as Example 1, etc., and the slurry compositions of Examples 13 and 15 are turbid in the same manner as Example 9, etc. Each slurry composition of Examples 10 to 15 can be applied to an object in the same manner as Example 1, etc. In addition, even after each slurry composition of Examples 10 to 15 was left to stand for 10 minutes, precipitation of La-based composite oxide particles (La-Mo-W-based composite oxide particles, La-W-based composite oxide particles) was not observed. In addition, for each slurry composition of Examples 10 to 15, in the state where the dispersion medium was evaporated after being applied to the object, no continuous state of particles of more than 50 μm was observed, and thus no aggregation of La-based composite oxide particles was confirmed.

Claims

1. A slurry composition comprising particles of a composite oxide and a dispersion medium, wherein the composite oxide comprises La and at least one element selected from the group consisting of Mo and W, wherein: The median particle size of the particles is less than 800 nm. The content of the particles is 0.1% by mass to 10% by mass.

2. The slurry composition according to claim 1, wherein The composite oxide is La2Mo x W (2-X) O9(0≦x≦2). 3 . The slurry composition according to claim 1 , which contains a binder. 4 . The slurry composition according to claim 1 , comprising a dispersant. 5 . The slurry composition according to claim 1 , comprising an ultraviolet curable resin. 6 . A coating agent comprising the slurry composition according to claim 1 .