Coating agent
By forming a coating of organopolysiloxane compounds with methyl, phenyl, acrylic and/or vinyl groups on the surface of the glass container, the problem of formulation residue and high pH dissolution caused by the highly hydrophilic nature of the container is solved, achieving Tolerance and heat resistance to high pH preparations, reducing the amount of Si dissolution, and improving the stability and transparency of the container.
Patent Information
- Application Number
- CN202380023474.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-29
- Filing Date
- 2023-01-31
- Publication Date
- 2024-10-15
AI Technical Summary
The high hydrophilicity of existing glass containers leads to preparation residues, white turbidity after freeze-drying, dissolution of glass components when the pH becomes high, and the risk of deterioration of preparations, and the coating has insufficient tolerance to high pH preparations.
Form a coating containing an organopolysiloxane compound on the glass surface, with organic substituents of methyl, phenyl, acrylic and/or vinyl, which can maintain good hydrophobicity and inhibit deterioration and peeling, and is suitable for high pH Preparation tolerance.
It achieves good tolerance to high-pH preparations, prevents deterioration of preparations and reduced visibility of containers, reduces the amount of Si elution, and improves heat resistance and transparency of containers.
Smart Images

Figure BDA0005007916070000051 
Figure BDA0005007916070000052
Abstract
Description
Technical Field
[0001] The present invention relates to a coating agent having good hydrophobicity and resistance to high pH agents. Background Art
[0002] Pharmaceutical containers such as vial containers and ampoule containers require high chemical durability in order to stably store the preparations. Therefore, borosilicate glass, which has excellent chemical resistance, is used in pharmaceutical containers.
[0003] In addition, before the pharmaceutical container is filled with the preparation, it is washed with a water jet, washed with a detergent, washed with an ultrasonic wave, etc. Furthermore, it is sterilized by dry heat at about 300°C for pyrogen inactivation. Therefore, it is important that the pharmaceutical container does not deteriorate, deteriorate, or peel even after the washing process and dry heat sterilization. It is particularly important that the pharmaceutical container does not deteriorate, deteriorate, or peel even when the preparations of various pH values are filled into the container.
[0004] Patent Document 1 proposes a method for improving the hydrophobicity, water resistance, and alkali resistance of a glass container by forming a fluororesin-based coating on the inner surface of the container.
[0005] Patent Document 2 proposes a method for improving the hydrophobicity of a glass container by forming a fluorine-containing coating on the inner surface of the container, and a method for reducing the amount of Si elution when the container is filled with water and subjected to an autoclave treatment.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2013 / 179514
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 5-132065 Summary of the invention
[0010] Technical problem that the invention aims to solve
[0011] For injections, it is required to give the patient a certain dosage. However, if the hydrophilicity of the glass surface is high, liquid may remain on the inner surface of the container, and the appropriate dosage may not be given. This is a very serious problem. In order to solve this problem, the current situation is to consider the residual amount in advance and fill the preparation in excess of the appropriate amount. As a result, the preparation is given in excess of the appropriate amount, and the preparation cost increases.
[0012] In addition, it is known that biological preparations that have been developed in recent years are very unstable and thus may deteriorate due to external factors such as temperature fluctuations and vibrations. Therefore, freeze drying of liquid preparations is performed. However, if the hydrophilicity of the glass surface is high, the liquid preparation in the container will flow to the container body during the freeze drying process, and white turbidity will occur after freeze drying, which may sometimes cause problems such as reduced visibility and appearance of the container.
[0013] Furthermore, the pH of the preparation is designed to be around pH 6 to 8 so that there is no pain or numbness during administration. However, depending on the type of preparation, it sometimes exhibits an acidity or alkalinity such as pH 4 or pH 11. Although borosilicate glass has a certain degree of resistance to acidic solutions, it is easily corroded by alkaline solutions. Therefore, when the pH of the preparation becomes high, there is a risk that the glass component of the container will dissolve, causing the preparation to deteriorate.
[0014] However, current coatings suffer from problems of hydrophobicity and insufficient resistance to high pH formulations.
[0015] Therefore, an object of the present invention is to provide a coating agent having excellent hydrophobicity and resistance to high-pH agents.
[0016] Technical solutions to the problem
[0017] The inventors conducted various experiments and found that the above technical problems can be solved by applying a coating layer containing an organopolysiloxane compound on a substrate, and thus proposed the present invention. Hereinafter, various aspects of the coating agent that solve the above problems will be described.
[0018] The coating agent of embodiment 1 is a coating agent for forming a coating on a glass surface or a resin surface, characterized in that it contains an organopolysiloxane compound having the following organic substituents: a methyl group and a phenyl group; and an acrylic group and / or a vinyl group. The coating containing the organopolysiloxane compound having the organic substituent can maintain good hydrophobicity even in a state of long-term contact with a high pH agent, and can suppress degradation, peeling, etc.
[0019] In the coating agent of embodiment 2, in embodiment 1, it is preferred that the organopolysiloxane compound further has one or two or more organic substituents selected from the group consisting of epoxy groups, ether groups, and polyester groups.
[0020] The coating agent of embodiment 3 preferably contains substantially no halogen component in embodiment 1 or embodiment 2. Here, “substantially contains no halogen component” means that the content of the halogen component in the coating layer is less than 0.8 mass %.
[0021] In the coating agent of aspect 4, it is preferred that the content of the organopolysiloxane compound is 0.5 mass % to 40 mass % in any of aspects 1 to 3. This makes it easy to adjust the viscosity of the coating agent and to make the thickness of the coating layer uniform.
[0022] In the coating agent of embodiment 5, it is preferred that in any one of embodiments 1 to 4, the organopolysiloxane compound comprises dimethylpolysiloxane, phenylpolysiloxane, methylpolysiloxane, and acrylic polysiloxane and / or vinyl polysiloxane, and when the molar ratio is dimethylpolysiloxane:phenylpolysiloxane:methylpolysiloxane:acrylic polysiloxane+vinyl polysiloxane=A:B:C:D, A is 0.8 to 5.0, B is 0.8 to 5.0, C is 1.0 to 5.2, and D is 0.1 to 2.5. Here, "acrylic polysiloxane+vinyl polysiloxane" refers to the total amount of acrylic polysiloxane and vinyl polysiloxane.
[0023] The coating agent of aspect 6 preferably has a refractive index (589 nm) of 1.40 to 1.55 after thermal curing in any of aspects 1 to 5. This can reduce the difference in refractive index with the glass surface, thereby preventing light scattering and achieving high transparency.
[0024] The coating agent of aspect 7 is preferably a coating agent for forming a coating layer on the inner surface of a medical container in any of aspects 1 to 6.
[0025] Effects of the Invention
[0026] According to the present invention, a coating agent having excellent hydrophobicity and resistance to high-pH agents can be provided. DETAILED DESCRIPTION
[0027] Hereinafter, embodiments of the coating agent will be described. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments.
[0028] [Coating agent]
[0029] The coating agent of the present invention is a coating agent for forming a coating on a glass surface or a resin surface, and the coating agent comprises an organopolysiloxane compound, and the organopolysiloxane compound has: organic substituents of methyl and phenyl groups; and organic substituents of acrylic and / or vinyl groups. In addition, it may also have one or more organic substituents selected from the group consisting of epoxy groups, ether groups and polyester groups. For the coating comprising the organopolysiloxane compound having the above-mentioned organic substituents, good hydrophobicity can be maintained even in a state of long-term contact with a high pH preparation, and degradation, peeling, etc. can be suppressed. It should be noted that the effect of improving the hydrophobicity of the coating agent is particularly good for polysiloxanes having methyl groups, the effect of improving the heat resistance of the coating agent is particularly good for polysiloxanes having phenyl groups, and the effect of improving the alkali resistance of the coating agent is particularly good for polysiloxanes having acrylic and / or vinyl groups.
[0030] The organopolysiloxane compound generally contains at least one siloxane structure as shown in [Chemical 1] and [Chemical 2] below. The siloxane structure is the structure shown below, and may be a composite structure including a single chain, a chain and a cage structure, and the side chain R represents a hydrogen atom or a hydrocarbon group. The organopolysiloxane compound of the present invention has a structure represented by a polysiloxane (SiOR1R2)n (n≥1) having an organic side chain (R≠H), and R1 and R2 have the following organic substituents: methyl and phenyl; and acrylic and / or vinyl. In addition, it may also have one or more organic substituents selected from the group consisting of epoxy, ether and polyester groups.
[0031] [Chemistry 1]
[0032]
[0033] [Chemistry 2]
[0034]
[0035] Representative examples of polysiloxane are shown below.
[0036] Methyl polysiloxane: (SiO2(CH3)) n (n≥1)
[0037] Phenyl polysiloxane: (SiO2(C6H5)) n (n≥1)
[0038] Dimethylpolysiloxane: (SiO(CH3)2) n (n≥1)
[0039] Acrylic polysiloxane: (SiO2(CH2)3-O-(C=O)-C3H5) n (n≥1)
[0040] Vinyl polysiloxane: (SiO2(CH2=CH)) n (n≥1)
[0041] The content of the organopolysiloxane compound in the coating agent is preferably 0.5% or more, 1% or more, 2% or more, 4% or more, 5% or more, 10% or more, particularly preferably 12% or more, preferably 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, particularly preferably 15% or less. When the content of the organopolysiloxane compound is too low, the hydrophobicity becomes poor, and it is difficult to suppress the deterioration and peeling of the coating. On the other hand, if the content of the organopolysiloxane compound is too high, the viscosity of the coating agent becomes high, and it is difficult to form a coating with uniform wall thickness on the inner surface of the container. As a result, during drying and thermal curing, cracks and peeling are easily generated due to residual stress in the coating.
[0042] The organopolysiloxane compound contained in the coating agent preferably includes: dimethylpolysiloxane; phenylpolysiloxane; methylpolysiloxane; and acrylic polysiloxane and / or vinyl polysiloxane. When these are included, the hydrophobicity can be improved and the stability to temperature can be improved. When the molar ratio is dimethylpolysiloxane:phenylpolysiloxane:methylpolysiloxane:acrylicpolysiloxane+vinylpolysiloxane=A:B:C:D, A is 0.8-5.0, B is 0.8-5.0, C is 1.0-5.2, and D is 0.1-2.5, preferably A is 1.2-4.0, B is 1.2-3.8, C is 1.5-4.2, and D is 0.3-1.7, more preferably A is 1.8-3.5, B is 1.8-3.5, C is 2.0-3.9, and D is 0.5-1.5, and particularly preferably A is 2.0-3.2, B is 2.0-3.0, C is 2.0-3.5, and D is 0.5-1.5. If the molar ratio is outside the above range, it is difficult to fully improve the hydrophobicity and alkali resistance, and the thermal stability to temperature is impaired. Specifically, if A and C are too little (B and D are too much), the thermal stability to temperature is easily impaired. On the other hand, if A and C are too much (B and D are too little), it is difficult to fully improve the hydrophobicity and alkali resistance.
[0043] The coating agent is preferably applied to the content surface of the container in a state uniformly mixed with the organic solvent. The organic solvent is not particularly limited, and examples thereof include butanol, isopropanol, isopropyl acetate, and the like. These organic solvents may be mixed in a plurality of forms, or only one form may be used. In addition, the content of the organic solvent in the coating agent is preferably 1% or more, 5% or more, 10% or more, 15% or more, 20% or more, particularly preferably 25% or more, preferably 90% or less, 80% or less, 70% or less, and particularly preferably 60% or less in mass %.
[0044] The coating agent may contain a surface adjuster for adjusting the surface tension. Based on this, after being applied to the content surface of the container, the smoothness of the coating can be improved. The content of the surface adjuster in the coating agent is preferably 0 to 10% by mass, more preferably 0 to 5%, and particularly preferably 0.5% to 1%.
[0045] The coating agent preferably contains substantially no halogen components, particularly fluorine components and chlorine components, because this can reduce environmental load and improve workability.
[0046] [Method of applying coating agent]
[0047] In order to uniformly apply the coating agent, it is preferable to clean the container in advance. The cleaning method is not particularly limited, and dust and the like may be removed by air blowing, or cleaning may be performed using a solvent such as purified water or acetone.
[0048] The method for applying the coating agent is not particularly limited, and a dipping method, a spraying method, an electrostatic spraying method, or the like can be used.
[0049] [Formation of coating]
[0050] It is preferred that the coating agent is dried and thermally cured after being applied to the inner surface of the container to form a coating. The drying step is a step of volatilizing the organic solvent in the coating agent. The thermal curing step is a step of causing the coating agent to undergo a dehydration condensation reaction and firmly bond to the inner surface of the container.
[0051] The drying temperature in the drying step is preferably 40° C. or higher, 45° C. or higher, particularly preferably 50° C. or higher, preferably 180° C. or lower, 170° C. or lower, particularly preferably 150° C. or lower. If the drying temperature is too low, the organic solvent cannot be fully removed from the coating agent, and the coating is prone to white turbidity, peeling, etc. On the other hand, if the drying temperature is too high, the thermal curing reaction proceeds rapidly, and the coating is prone to white turbidity, peeling, etc.
[0052] The drying time is preferably 1 minute or more, 5 minutes or more, 10 minutes or more, 15 minutes or more, particularly preferably 20 minutes or more, preferably 60 minutes or less, 40 minutes or less, particularly preferably 30 minutes or less. If the drying time is too short, the organic solvent cannot be fully removed from the coating agent, and the coating is prone to white turbidity, peeling, etc. If the drying time is too long, the productivity of the pharmaceutical container is reduced.
[0053] The heat curing temperature in the heat curing step is preferably 185°C or higher, 190°C or higher, particularly preferably 200°C or higher, preferably 450°C or lower, 400°C or lower, particularly preferably 350°C or lower. If the heat curing temperature is too low, the heat curing reaction cannot be fully generated, and it is difficult to improve the hydrophobicity of the pharmaceutical container. On the other hand, if the heat curing temperature is too high, the coating agent is thermally decomposed, and defects may occur in the coating. In the worst case, the coating may disappear.
[0054] The heat curing time is preferably 5 minutes or more, 10 minutes or more, particularly preferably 15 minutes or more, preferably 100 minutes or less, 60 minutes or less, particularly preferably 40 minutes or less. If the heat curing time is too short, the heat curing reaction is insufficient and it is difficult to improve the hydrophobicity of the pharmaceutical container. On the other hand, if the heat curing time is too long, the productivity of the pharmaceutical container decreases.
[0055] The coating agent preferably has a refractive index close to that of the container. Based on this, it is possible to prevent light scattering and obtain high transparency. Specifically, the refractive index of the coating layer for light of a wavelength of 589 nm is 1.40 to 1.55, preferably 1.42 to 1.52, more preferably 1.43 to 1.52, further preferably 1.44 to 1.50, and particularly preferably 1.45 to 1.49.
[0056] The thickness of the coating is preferably 10 nm or more, 20 nm or more, 50 nm or more, 100 nm or more, preferably 2500 nm or less, 2000 nm or less, and particularly preferably 1500 nm or less. Based on this, defects such as pores are not easily generated, and the stress generated after thermal curing is reduced, so it is possible to suppress the deterioration and peeling of the coating.
[0057] [container]
[0058] From the viewpoint of chemical resistance, the container is preferably made of glass, particularly silicate glass. As silicate glass, it is preferred that the following be contained by mass %: SiO2 65% to 85%, Al2O3 0 to 15%, B2O3 0 to 13% (preferably 1% to 13%), Li2O 0 to 5%, Na2O 3% to 15%, K2O 0 to 5%, BaO 0 to 5%, CaO 0 to 15%, and MgO 0 to 5%. In addition, it is preferred that the following be contained by mass %: SiO2 65% to 85%, Al2O3 1% to 15%, B2O3 0 to 13% (preferably 1% to 13%), Na2O 3% to 15%, K2O 0 to 5%, BaO 0 to 5%, CaO 0 to 5%, and MgO 0 to 5%. In addition, the container may be brown in order to shield ultraviolet rays. That is, it may also contain, by mass%, Fe2O3 0.001% to 5%, TiO2 0.001% to 5%. In addition, in the case of a glass container, as a clarifier, SnO2, Sb2O3, As2O3, CeO2, F, Cl, and sodium sulfate may be contained. There is no particular restriction on their content, but from the viewpoint of manufacturing cost and environmental load, the individual content or the total amount is preferably 0% or more, 0.001% or more, 0.002% or more, 0.005% or more, 0.007% or more, preferably 2% or less, 1.8% or less, 1.5% or less, 1% or less, 0.8% or less, 0.5% or less, and 0.3% or less. From the viewpoint of processability in processing into a container shape, the container preferably contains a resin, particularly a resin such as polypropylene, polyethylene, polyethylene terephthalate, polyvinyl chloride, cycloolefin polymer, cycloolefin copolymer, polymethylpentene, and polycarbonate.
[0059] The linear thermal expansion coefficient of silicate glass at 30°C to 380°C is preferably 100×10 -7 / ℃ below, 90×10 -7 / ℃ below, 80×10 -7 / ℃ below, 70×10 -7 / ℃ below, 60×10 -7 / ℃ below, 50×10 -7 / ℃ below, 35×10 -7 / ℃ and above 45×10 -7 / °C or less. If the linear thermal expansion coefficient at 30°C to 380°C is limited to the above range, the amount of Si elution is reduced. It should be noted that the linear thermal expansion coefficient at 30°C to 380°C can be measured using a dilatometer or the like.
[0060] On the other hand, when the linear thermal expansion coefficient of silicate glass at 30°C to 380°C is high, the manufacturing efficiency of the medical container becomes high, but on the other hand, the amount of Si elution becomes large, making it difficult to use as a medical container. However, if the coating of the present invention is formed, it can be used as a medical container even in such a case. That is, when the linear thermal expansion coefficient of silicate glass at 30°C to 380°C is high, the effect of the present invention can be reliably enjoyed. In this case, the linear thermal expansion coefficient of silicate glass at 30°C to 380°C is preferably 25×10 -7 / ℃ or above, 30×10 -7 / ℃ or above, 40×10 -7 / ℃ or above, 50×10 -7 / ℃ or above, 60×10 -7 / ℃ or above, 70×10 -7 / ℃ or above, 80×10 -7 / ℃ or above, 100×10 -7 / ℃ below.
[0061] [Medical container]
[0062] The container for forming the coating layer may be in various forms, for example, preferably a vial container, an ampoule container, a syringe, a syringe, or the like.
[0063] In a pharmaceutical container (20 mmφ, 1 mm thick, 10 mL in volume) after the coating is formed on the surface using the coating agent of the present invention, a sodium hydroxide aqueous solution adjusted to pH 11 is filled to 90 volume, and then heat-treated at 121°C for 60 minutes. The amount of Si eluted at this time is preferably 2 μg / mL or less and 1.8 μg / mL or less. If the amount of Si eluted is too much, insoluble foreign matter is easily generated in the pharmaceutical.
[0064] Example
[0065] The present invention will be described in detail based on the examples. The following examples are for illustration only and the present invention is not limited to the following examples at all.
[0066] [Sample No. 1]
[0067] A coating agent was prepared by mixing and dissolving 30% by mass of an organopolysiloxane compound containing methyl, phenyl and acrylic groups, 15% by mass of butanol, 10% by mass of isopropyl acetate and 45% by mass of isopropyl alcohol. The molar ratio of dimethylpolysiloxane, phenylpolysiloxane, methylpolysiloxane and acrylic polysiloxane contained in the organopolysiloxane compound was adjusted to 2.9:2.7:2.7:1.
[0068] A borosilicate glass tube with an outer diameter of 20 mmφ and a wall thickness of 1 mm was processed to prepare a vial container with a volume of 10 mL. The vial container was filled with the above-mentioned coating agent, and after the vial was inverted to discharge the coating agent, it was tilted horizontally with the mouth of the vial facing the outside and rotated using a centrifuge to remove the coating agent remaining in the vial container. The vial coated with the coating agent was dried in a dryer heated to 60°C for 60 minutes. Then, a heat curing treatment was performed in a dryer heated to 260°C to 290°C for 30 minutes to form a coating with an average thickness of 250 nm.
[0069] It should be noted that the coating thickness was measured according to the following steps. A scar was formed on the outer surface of the container body using a grinding wheel glass cutter (Normal Wheel Type, manufactured by Samsung Diamond Co., Ltd.). The scar was formed along the length direction in a manner that the container circumference is divided into 6 or 8 equal parts from the bottom of the container to the shoulder. The outer surface of the bottom of the container was also radially scarred in a manner that the bottom surface is divided into 6 or 8 equal parts. Next, a thermal expansion coefficient of about 100×10 -7 / ℃, one end of a soda-lime glass rod is baked with an oxygen burner to soften it. While keeping the mouth of the container in an inverted state, press the softened glass rod against the scarred part of the side of the container and hold it for a few seconds. Repeat the heating and pressing of the glass rod until the crack extends from the shoulder of the container to the bottom. The cracks in other adjacent scarred parts are also extended in the same way. Finally, press the heated glass rod against the bottom of the container to extend the crack radially. After the crack has basically extended, knock on the side and bottom of the container, and take out the side and bottom parts. Place the removed glass piece on the sample holder in a way that the cross-section part becomes the upper surface, and use a high spatial resolution SEM SU 8220 (manufactured by Hitachi High-Technologies Co., Ltd.) to observe the cross section and measure the thickness of the coating film.
[0070] [Sample No. 2]
[0071] An organic polysiloxane compound containing methyl, phenyl and vinyl groups was mixed and dissolved at a ratio of 24 mass %, butanol 15 mass %, isopropyl acetate 10 mass % and isopropyl alcohol 51 mass % to prepare a coating agent. The molar ratio of dimethyl polysiloxane, phenyl polysiloxane, methyl polysiloxane and vinyl polysiloxane contained in the organic polysiloxane compound was adjusted to 2.9:2.6:2.7:1.
[0072] A borosilicate glass tube with an outer diameter of 20 mmφ and a wall thickness of 1 mm was processed to prepare a vial container with a volume of 10 mL. The vial container was filled with the above-mentioned coating agent, and after the vial was inverted to discharge the coating agent, it was tilted horizontally with the mouth of the vial facing the outside and rotated using a centrifuge to remove the coating agent remaining in the vial container. The vial coated with the coating agent was dried in a dryer heated to 60°C for 10 minutes. Then, a heat curing treatment was performed in a dryer heated to 260°C to 290°C for 30 minutes to form a coating with an average thickness of 300 nm.
[0073] [Sample No. 3]
[0074] A coating agent was prepared by mixing and dissolving 30% by mass of an organopolysiloxane compound containing methyl and phenyl groups, 15% by mass of butanol, 10% by mass of isopropyl acetate, and 45% by mass of isopropyl alcohol. The molar ratio of dimethylpolysiloxane, phenylpolysiloxane, and methylpolysiloxane contained in the organopolysiloxane compound was adjusted to 2.9:2.7:2.7.
[0075] A borosilicate glass tube with an outer diameter of 20 mmφ and a wall thickness of 1 mm was processed to prepare a vial container with a volume of 10 mL. The vial container was filled with the above-mentioned coating agent, and after the vial was inverted to discharge the coating agent, it was tilted horizontally with the mouth of the vial facing the outside and rotated using a centrifuge to remove the coating agent remaining in the vial container. The vial coated with the coating agent was dried in a dryer heated to 60°C for 60 minutes. Then, a heat curing treatment was performed in a dryer heated to 260°C to 290°C for 30 minutes to form a coating with an average thickness of 250 nm.
[0076] [Sample No. 4]
[0077] A coating agent was prepared by mixing and dissolving 30% by mass of a methyl-containing organopolysiloxane compound, 15% by mass of butanol, 10% by mass of isopropyl acetate, and 45% by mass of isopropyl alcohol. The molar ratio of dimethylpolysiloxane to methylpolysiloxane contained in the organopolysiloxane compound was adjusted to 2.9:2.7.
[0078] A borosilicate glass tube with an outer diameter of 20 mmφ and a wall thickness of 1 mm was processed to prepare a vial container with a volume of 10 mL. The vial container was filled with the above-mentioned coating agent, and after the vial was inverted to discharge the coating agent, it was tilted horizontally with the mouth of the vial facing the outside and rotated using a centrifuge to remove the coating agent remaining in the vial container. The vial coated with the coating agent was dried in a dryer heated to 60°C for 60 minutes. Then, a heat curing treatment was performed in a dryer heated to 260°C to 290°C for 30 minutes to form a coating with an average thickness of 250 nm.
[0079] Next, the inside and outside of the prepared vial containers (samples No. 1 to 4) were washed three times with purified water, and then filled with a sodium hydroxide aqueous solution adjusted to pH 11 to 90 volume. Then, a rubber stopper and an aluminum cap were set at the mouth of the vial container and rolled tightly, and then heat-treated at 121° C. for 60 minutes in an autoclave without leaking the internal liquid. These containers were analyzed for Si dissolution.
[0080] For Si elution analysis, the rubber stopper and aluminum cap were removed from the vial container after the heating test, and the elution liquid in the vial container was collected into a centrifuge tube. Then, the Si concentration in the elution liquid was analyzed by ICP-OES.
[0081] The Si elution amount of sample No. 1 was 1.31 μg / mL. The Si elution amount of sample No. 2 was 1.45 μg / mL. The Si elution amount of sample No. 3 was 2.86 μg / mL. The Si elution amount of sample No. 4 was 3.11 μg / mL.
[0082] As can be seen from the above, Sample No. 1 and Sample No. 2 have less Si elution than Sample No. 3 and Sample No. 4, and have good chemical durability to high pH solutions.
[0083] [Sample No. 5]
[0084] The same coating agent as that of sample No. 1 was applied to a glass substrate of alkali-free aluminosilicate glass (OA-10G manufactured by Nippon Electric Glass) by spin coating. The glass substrate coated with the coating agent was dried in a dryer heated to 60°C for 60 minutes. Then, a heat curing treatment was performed in a dryer heated to 260°C to 290°C for 60 minutes to form a coating with an average thickness of 250 nm on the glass surface. The contact angle, refractive index and transmittance (wavelength region 400 to 700 nm) of the glass substrate after the heat curing treatment were measured.
[0085] [Sample No.6]
[0086] The same coating agent as that of sample No. 2 was applied to a glass substrate of alkali-free aluminosilicate glass (OA-10G manufactured by Nippon Electric Glass) by spin coating. The glass substrate coated with the coating agent was dried in a dryer heated to 60°C for 10 minutes. Then, a heat curing treatment was performed in a dryer heated to 260°C to 290°C for 60 minutes to form a coating with an average thickness of 300 nm on the glass surface. The contact angle, refractive index and transmittance (wavelength region 400 to 700 nm) of the glass substrate after the heat curing treatment were measured.
[0087] [Sample No.7]
[0088] The same glass substrate as that of Sample No. 5 and Sample No. 6 (OA-10G manufactured by Nippon Electric Glass Co., Ltd.) was used to measure the contact angle, refractive index, and transmittance (wavelength range 400 nm to 700 nm) without forming a coating layer.
[0089] The contact angle was measured using a contact angle meter (Asumi Technology Development B100) and purified water. The refractive index (589 nm) was measured using a spectroscopic ellipsometer. The measurement wavelength was 350 nm to 1700 nm. The transmittance was measured using a spectrophotometer (Japan Spectrophotometer V-670). The measurement wavelength was 200 nm to 800 nm, the sampling interval was 1 nm, the slit width was 5 nm, and the scanning speed was 200 nm / min.
[0090] The contact angle of sample No. 5 is 97°, the contact angle of sample No. 6 is 96°, and the contact angle of sample No. 7 is 30°, which shows that the hydrophobicity of samples No. 5 and No. 6 is better than that of sample No. 7. In addition, the refractive index of samples No. 5 and No. 6 is the same as that of sample No. 7 (1.47), and the transmittance is the same (91%).
Claims
1. A coating agent, characterized in that: The coating agent is a coating agent used to form a coating on a glass surface or a resin surface. The coating agent includes an organopolysiloxane compound having the following organic substituents: a methyl group and a phenyl group; and an acrylic group and / or a vinyl group.
2. The coating agent according to claim 1, wherein The organopolysiloxane compound further has one or two or more organic substituents selected from the group consisting of an epoxy group, an ether group, and a polyester group.
3. The coating agent according to claim 1 or 2, wherein The coating agent contains substantially no halogen component.
4. The coating agent according to claim 1 or 2, wherein The content of the organopolysiloxane compound is 0.5% by mass to 40% by mass.
5. The coating agent according to claim 1 or 2, wherein The organopolysiloxane compound includes dimethylpolysiloxane, phenylpolysiloxane, methylpolysiloxane, acrylic polysiloxane and / or vinylpolysiloxane. When the molar ratio is dimethylpolysiloxane:phenylpolysiloxane:methylpolysiloxane:acrylic polysiloxane+vinylpolysiloxane=A:B:C:D, A is 0.8 to 5.0, B is 0.8 to 5.0, C is 1.0 to 5.2, and D is 0.1 to 2.
5.
6. The coating agent according to claim 1 or 2, wherein The refractive index of the coating for light with a wavelength of 589 nm is 1.40 to 1.
55.
7. The coating agent according to claim 1 or 2, wherein The coating agent is a coating agent for forming a coating on the inner surface of a medical container.
Citation Information
Patent Citations
Surface-treated glass bottle
JP1993132065A
Glass container and method for manufacturing same
WO2013179514A1
Film forming composition, glass substrate coated with said film forming composition, and touch panel obtained using said glass substrate
CN112955514A
Pharmaceutical container, method for producing pharmaceutical container, and coating material
WO2021182379A1