Method for producing hardened steel component
By using thin steel plate blanks with metal anti-corrosion layers for cold forming and form hardening in the preparation of steel plate parts, and combining the processes of cold final forming and hot final forming, the limitations of the direct and indirect methods are solved, and the economy of complex shapes is achieved. preparation and high mechanical properties.
Patent Information
- Application Number
- CN202380011151.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-10-15
AI Technical Summary
Among the existing steel plate component preparation methods, the direct method can only produce simple geometric shapes and external trimming and hole pattern manufacturing need to be carried out in a hardened state. Although the indirect method can produce complex shapes, it is more expensive and contains liquid or gaseous zinc. Material embrittlement caused by reaction with austenite.
Cold forming using a thin steel plate blank with a metal corrosion protection layer, partial or complete austenitization, and cooling and quench hardening in a form hardening tool above the critical hardening rate, combining surface area distribution of cold final forming and hot final forming , eliminating cold forming tools and corrective grinding, reducing material and tool usage.
The flexibility and economy of preparing steel plate parts with complex shapes are achieved, while the adverse effects of microcracks and mechanical properties are avoided, reducing production complexity and cost.
Smart Images

Figure CN118786228A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a hardened steel sheet component. Background Art
[0002] In the production of sheet steel components, in particular in the automotive industry, there are currently two common methods for producing sheet steel components which are used in particular to fulfill load-bearing functions, such as longitudinal members and struts, and therefore provide high strength and rigidity in the event of a crash, as well as corrosion protection and at the same time low weight.
[0003] The first common method is the press hardening method, also called the direct method. In press hardening, a sheet steel component is produced by heating a flat sheet blank made of hardenable steel to a temperature above the austenitizing temperature so that the steel structure is at least in parts in the high-temperature transformation zone, i.e. austenite. The flat sheet blank is then formed into the desired shape in a forming tool, preferably by a single forming stroke, and heat is rapidly extracted from the semi-steel material by contact with the forming tool, so that martensitic hardening occurs, wherein the austenite is essentially transformed into martensite. For this to happen, the rate of heat dissipation must be higher than the so-called critical hardening rate, which is usually higher than 20 Kelvin / second. This press hardening method is well known and very mature, in particular for the production of components with a design that is not too complex to be produced with a single press stroke.
[0004] A second known method is the form hardening method, also called the indirect method, developed by the applicant and known from EP 1 651 789 B1. Form hardening allows significantly more complex shapes to be produced.
[0005] For this purpose, the sheet metal blank or the steel strip is first cold-formed into a preformed component in a manner known per se. This cold forming is carried out in a conventional manner, for example, in a press line with five forming presses and a so-called progressive die, or in a transfer press with a so-called transfer die, wherein the flat sheet metal blank or the steel strip is formed step by step into a complex preformed component and then shaped.
[0006] The preformed component cold-formed in this way is then usually heated in a furnace, for example a continuous furnace or a multi-chamber furnace, to a temperature above the austenitizing temperature, so that a mostly or completely austenitic state of the steel structure is also achieved.
[0007] The already formed and heated preformed part is then placed in a form-hardening tool, where it is cooled at a rate above the critical hardening rate using the surface of the form-hardening tool and thereby hardened. In this case, the aforementioned cold forming is effected in such a way that the dimensional changes of the preformed part (caused by expansion in the furnace, contraction during the phase change, further expansion in the furnace and contraction during the transfer from the furnace to the forming tool) are taken into account by a correspondingly reduced final shape in all three spatial directions, so that the dimensions of the inserted heated preformed part are matched to the dimensions of the form-hardening tool.
[0008] This method is also known from WO 2006 / 015849. It is also known from this publication that if the dimensional deviations of the pre-cold formed part lie outside the tolerance band, these deviations can still be corrected or re-punched during the actual form hardening after the hot calibration.
[0009] Smartform technology is known from DE 10 20 200 808 A1, which discloses upsetting with compressive stress in order to produce cold-formed components that are as precise as possible.
[0010] EP 2 848 715 A1 has disclosed an electrolytic coating of sheet metal blanks for a hot forming process, the aim being to deposit it as thinly as possible in order to achieve a high degree of flexibility in processing properties.
[0011] EP2338618B1 discloses a hybrid form of an indirect method and a direct method, wherein a shaping step is provided after cold forming and final forming, and laser trimming or water jet trimming is performed. In this case, the proportion of cold forming is defined as 50-80% of the depth of drawing of the finished component.
[0012] In the form hardening method, as explained above, the advantage is that the usually multi-step cold forming method can achieve significantly more complex component shapes than the direct method.
[0013] At the same time, if a metallic corrosion protection layer, in particular a zinc-based metallic corrosion protection layer, is applied to the sheet metal blank or the steel strip, the sheet steel component is corrosion-resistant even in the hardened state.
[0014] In the so-called form-hardening method, the precooled formed part, which essentially has its final shape and is reduced in all three spatial directions to compensate for subsequent dimensional changes, is heated to the austenitizing temperature required for hardening and then placed in a form-hardening tool, where it is pressed all around, if necessary with minor corrections, in particular corrections to deformations caused by heating, and quench-hardened by contact with the form tool all around. Summary of the invention
[0015] The object of the present invention is to disclose a method for producing hardened sheet steel components, making the production process more flexible and economical.
[0016] This object is achieved by a method having the features of claim 1 .
[0017] Advantageous further embodiments are characterized by the features of the dependent claims.
[0018] The inventors have found that the advantage of using the direct method is that only one hot forming tool is required, but the disadvantage is that only simple geometries can be achieved, and in addition, the external trimming and the production of the hole pattern must be carried out in the hardened state.
[0019] In contrast, in the indirect method, the advantage is that after hardening, no hard or laser trimming is required, because the external trimming and hole patterning have already been done in the cold forming before hardening. In addition, due to the multi-step cold forming, more complex geometries can be produced. However, it has been found that the costs are relatively high, especially for small batches or small quantities, because in addition to the form-hardening tool, a cold forming tool set is required, that is, a plurality of cold forming tools arranged one after another, for example five cold forming tools and the associated press.
[0020] For the purposes of the present invention, a cold forming tool is one of a group of cold forming tools, such as a progressive die or a multi-station die, in which a thin sheet blank or a thin steel strip is sequentially formed into a component in a multi-step forming and trimming process by a combination of main deep drawing, trimming and post-forming.
[0021] It has also been found that in the direct process, there are problems associated with the reaction of liquid or gaseous zinc with austenite during hardening. This contact of austenite grains with liquid and gaseous zinc apparently produces two phenomena, namely liquid metal embrittlement (due to liquid zinc) or vapor metal embrittlement (due to zinc vapor). Both phenomena lead to embrittlement of the material, resulting in the formation of microcracks in the interior of the steel material during the forming process.
[0022] Liquid metal embrittlement (LME) can be counteracted by using a steel grade with delayed transformation, precooling it to below the liquid point of the zinc alloy coating before forming, and then forming it at the end. This is disclosed, for example, in DE102015113056. In order to prevent vapor metal embrittlement (VME), air or other gases, especially oxygen-containing gases, can be blown into the component or the forming tool before forming. This method is known from DE102016102344.
[0023] In the indirect method with zinc coatings, post-forming is not permitted for the same reasons, i.e. the final forming must be carried out during the cold forming process, cold forming scaling must be carried out, and the insert temperature and insert geometry must be adapted to the form-hardening method. Waviness due to cold forming or other shape deviations that are flattened during the form-hardening process are not permitted, or only to a very limited extent, which means that the necessary measures and corrections to avoid them require a high level of tool and / or material expenditure in the cold forming. In addition, there is a risk that microcracks may occur or other adverse effects on the mechanical properties of the component may occur.
[0024] According to the invention, it has been found that in form-hardened tools, local post-forming or final forming of components in a defined manner occurs for various reasons. According to the invention, this is achieved with surprising success despite high zinc deposits and unavoidably high insertion temperatures, so that the requirements of the end product with regard to microcracks and mechanical properties can also be reliably met.
[0025] For the purposes of the present invention, the insertion temperature is the temperature of the preformed part shortly after it has been inserted into the mold and before it reaches the bottom dead center of the mold, ie at the start of the final forming process.
[0026] Compared to press hardening of flat sheet blanks, when preformed parts are form hardened, due to their complex geometry, they cannot be precooled with sufficient uniformity and accuracy by contact or convection after austenitization and before insertion into the forming tool to a lower insertion temperature, i.e. below the liquidus point of the zinc alloy coating.
[0027] It has been found that transferring the forming process from the cold forming tool to the form-hardening tool and thereby reducing the cold forming process can lead to considerable savings even for smaller component ranges by eliminating the need for an entire cold forming tool.
[0028] Furthermore, correction grinding of cold forming, in particular to eliminate cold forming ripples etc., can be omitted and can be effectively integrated into the form hardening tool as hot post-forming during form hardening. According to the invention, hot post-forming can also be referred to as hot final forming.
[0029] Furthermore, it has been found that the outlay required for achieving a cold-formed component without corrugation, in particular with regard to the use of material and with regard to the use of draw beads or other cold-forming tool modifications, etc., can be dispensed with.
[0030] If required for manufacturing reasons, it can also be used to form parts with specific protrusions, such as in the flange area, which is useful, for example, for processing from cold forming into a furnace, and for processing from the furnace to a form-hardening tool and for stable insertion into a form-hardening tool and then post-forming into multiple protrusions in the form-hardening tool.
[0031] Surprisingly, it has been found that, contrary to all expectations, despite the significant zinc coating and despite the high insertion temperatures, in the indirect process, i.e. in the form-hardening method, austenitized cold-formed components can be post-formed in the form-hardening tool or finally locally formed and hardened in a defined manner even without precooling and have good properties with regard to microcracks, mechanical properties, layer thickness, etc.
[0032] Even larger post-forming steps, i.e. defined forming steps such as chamfering, folding up, corrugation etc., can be easily realized in the form-hardening process, i.e. in the form-hardening tool in the form-hardening form, in the form of hot post-forming.
[0033] In particular, microcracks generated by VME and / or LME can be prevented, if necessary, by targeted local injection of air. However, it has been found that even without injection of air, small post-forming, i.e. corrugations up to a few millimeters, can be achieved without microcracks.
[0034] In order to be regarded as a defined reshaping or final shaping during the form-hardening process, the geometric deviation between the component geometry after cold forming and the component geometry after form-hardening must be at least 1 mm, in particular in the case of corrugations.
[0035] According to the invention, a thin steel sheet blank or steel strip is used which has a metallic anticorrosion layer, in particular a zinc-based metallic anticorrosion layer, with a layer thickness of 7 μm to 20 μm per side. This provides a good anticorrosion effect. In particular, this can be a coating Z120 or Z140 or Z180 according to DIN EN 10346.
[0036] The zinc-based anticorrosion layer may have a relatively high zinc content of 85 wt% to 98 wt% and contain, besides unavoidable impurities, 0.2 wt% to 2 wt% of aluminum. Other elements with an affinity for oxygen, such as magnesium, may also be present.
[0037] Particularly preferably, the zinc-based metal anti-corrosion layer can be applied by a hot-dip coating method. This can constitute a simple and cost-effective coating method.
[0038] According to the invention, relative to the total surface area of the finished component, 85-99% of the surface area is cold final formed (and therefore only hardened during form hardening) and 1-15% of the surface area is hot final formed and hardened during form hardening.
[0039] The percentage of the component surface area that has been hot final formed and hardened is calculated in such a way that the component area that has geometric deviations from the state before form hardening (i.e. after cold forming) is added to the state after form hardening and then related to the total surface area of the component after form hardening (i.e. the total surface area of the finished component).
[0040] For the above-mentioned percentage of the component surface that undergoes hot final forming, extremely small deviations (i.e. deviations from the component geometry after form hardening of less than 1 mm) and known material springback effects (e.g. side wall jump and flange jump during cold forming) are not taken into account for the purpose of hot calibration. This means that only deviations greater than 1 mm are used for the percentage of the surface area that undergoes hot final forming, whether due to deliberately prescribed geometric adjustments, such as repositioning of the formed component from the cold forming tool to the form hardening tool, or flattening of the corrugations. This facilitates the correction of any corrugations in the cold forming, which are usually difficult to avoid in cold forming or require greater expenditure to avoid. In the past, for example, it was then necessary to modify the cold forming tool, and additional drawbeads had to be introduced, which meant an increase in material costs because the sheet metal blank had to be enlarged as a result.
[0041] Therefore, the present invention particularly relates to a method for producing a hardened steel component, in which a thin steel sheet blank made of hardenable steel and having a metallic corrosion protection layer, in particular a zinc-based metallic corrosion protection layer, is first cold-formed, the resulting cold preformed component is then fully or partially austenitized by heating, and then inserted into a forming hardening tool, the insertion temperature being at least 500° C., in particular greater than 600° C., and cooled in the forming hardening tool by contact with the forming tool at a rate above the critical hardening rate, thereby quench-hardening and forming a finished component, wherein the layer thickness of the metallic corrosion protection layer is 7 μm to 20 μm on each side, and relative to the total surface area of the finished component, 85-99% of the surface area consists of cold final formed areas and 1-15% of the surface area consists of hot final formed areas during the form hardening process.
[0042] This preferred surface area distribution of surfaces with cold and hot final forming optimally combines the advantages of eliminating the entire cold forming tool and eliminating the material expenditure required for correction grinding and eliminating cold forming corrugations with a reliable hot forming percentage during the form hardening process.
[0043] According to one embodiment, relative to the total surface area of the finished component, 90-98% of the surface area consists of cold-finished areas and 2-10% of the surface area consists of areas that are hot-finished during form hardening.
[0044] According to one embodiment, cold forming is performed in 3-10 cold forming tools, and form hardening in a hot state and final forming are performed in one tool, namely, a form hardening tool.
[0045] According to one embodiment, for calculating the surface that has undergone hot final forming during the form hardening process, the deviation from the geometry of the hardened, ie finished component after cold forming (to be reshaped), in particular in the case of corrugations, is at least 1 mm.
[0046] According to one embodiment, before the form hardening, and during or after the heated preformed part is inserted into the form hardening tool, an oxygen-containing gas, in particular air, is blown toward, into or flushed into the form hardening tool and / or the preformed part. This can further reduce the possible risk of microcracks formed by LME and / or VME under unfavorable geometric conditions.
[0047] According to one embodiment, oxygen-containing gas, in particular air, is blown into the preform prior to form hardening and during or after the heated preform is inserted into the form hardening tool only in those areas where deformations exceeding 5 mm occur in the form hardening tool.
[0048] According to one embodiment, the metal, in particular alloy galvanized, anticorrosion layer has a layer thickness of 10 μm to 15 μm per side. This can further increase the corrosion protection, in particular the cathodic corrosion protection.
[0049] According to one embodiment, the metal, in particular alloy galvanized, anti-corrosion layer is applied by hot-dip method, in particular hot-dip galvanizing. This can constitute a particularly simple and cost-effective coating method.
[0050] According to one embodiment, the steel strip is made of hardenable alloy steel, in particular boron manganese steel, for example, 22MnB5 or 34MnB5 alloy steel.
[0051] According to one embodiment, the steel material used is a material that undergoes delayed transformation relative to austenite-martensite transformation during cooling, and the steel strip is hot rolled or cold rolled.
[0052] According to one embodiment, the steel strip used is a steel strip having the following composition (all figures are expressed in wt %): Carbon is at most 0.4, preferably 0.15-0.3 Silicon is at most 1.9, preferably 0.11-1.5 Manganese up to 3.0, preferably 0.8-2.5 Chromium up to 1.5, preferably 0.1-0.9 Molybdenum up to 0.9, preferably 0.1-0.5 Nickel up to 0.9, Titanium up to 0.2, preferably 0.02-0.1 Vanadium up to 0.2, Tungsten up to 0.2, Aluminum up to 0.2, preferably 0.02-0.07 Boron up to 0.01, preferably 0.0005-0.005 Sulfur up to 0.01, preferably up to 0.008 Phosphorus up to 0.025, preferably up to 0.01 Residual iron and impurities. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] The present invention will be explained by way of examples and drawings. In the drawings:
[0054] Figure 1 The results of cold forming according to the prior art are shown in highly schematic form in comparison with the results of cold forming according to the invention and form hardening according to the invention;
[0055] Figure 2 A sample showing the allowable waviness in a cold-formed part according to the present invention;
[0056] Figure 3 shows a perspective view of a sample component before and after form hardening;
[0057] Figure 4 Shows Figure 3 The shape change of the component shown during the form hardening process;
[0058] Figure 5 It is shown that the method according to the prior art and the present invention is prepared Figure 3 Example of the operating sequence of the cold forming tool set (multi-station die) and the form hardening tool in the component;
[0059] Figure 6 An example of the sequence of operations of a cold forming tool set (progressive die) and a form hardening tool in preparing a component according to the prior art and the method of the present invention is shown;
[0060] Figure 7 The form hardening process from sheet metal blank to finished component is schematically described. DETAILED DESCRIPTION
[0061] Figure 1 A comparison of cold forming as a preliminary step to form hardening according to the prior art and cold forming and form hardening according to the invention is shown highly schematically.
[0062] according to Figure 1In the upper line of the left column, the basic requirement of the conventional cold forming method before the form hardening is that there is no corrugation and no possible post-forming is necessary because all the shapes are already significant. This is called CF PA, i.e. cold forming according to the prior art.
[0063] According to the cold forming method of the present invention ( Figure 1 , left column, middle row of CF Inv.), a certain amount of ripple (greater than 1 mm) is allowed, such as Figure 2 In the subsequent forming hardening step ( Figure 1 , left column, bottom row FH Inv.), the corrugations are made uniform by forming the surface of the hardened tool, resulting in a finished part with smooth corrugations.
[0064] The right column shows that a post-forming process was performed in the flange area, in this case an upward folding process in the form-hardening tool, i.e. hot forming with an upward folding tool in the form-hardening tool ( Figure 1 , right column, FH Inv. in the lower line). This means that it is possible to save a cold forming step and thus a whole cold forming tool. In the prior art, the whole part must be finally formed in the cold forming step ( Figure 1 , right column, CF PA of the upper line).
[0065] Figure 2 The photograph shows existing ripples which, according to the invention, can still be present and are produced by the cold forming process. During the form hardening process, such ripples can be eliminated in a simple and very good manner in the hot state, in particular in a better and more efficient manner than a further cold forming correction step.
[0066] Figure 3 and Figure 4 It shows that the corresponding component has been post-stamped or post-formed at the indicated points without any negative impact on the mechanical properties of the component and without any microcracks etc., even with the relatively thick zinc layer. In this sample component, the total component surface area of the finished component is 1236 cm 2 , while the part surface area that deviates (greater than 1 mm) from the finished part geometry after cold forming and before form hardening is 38 cm 2 After cold forming, the percentage of the component surface area that deviates from the geometry of the finished component corresponds to 3.1%. The surface area distribution measured on the finished component is therefore 96.9% of the final cold formed area and 3.1% of the hot formed area.
[0067] Figure 5 and Figure 6A corresponding comparison of a sample operating sequence in the production of such a sample component according to the prior art and according to the invention is shown. It is clear that in each case one operating step can be omitted in the cold forming process, namely a cold forming tool. In the case of a multi-station die set ( Figure 5 ), which corresponds to one of the seven steps required in the prior art method. In this case, the local post-forming, i.e. the upward folding of the flange, can be completely transferred to the form hardening process (i.e. hot forming). In the case of a progressive die set ( Figure 6 ), it is possible to save one of the five operating steps. In this case, the final trimming (FTE), i.e. the final shaping, can be integrated into operating step 4, and the post-forming and folding can be integrated into the forming hardening process (i.e. hot forming). Depending on the complexity of the component, the method according to the invention may require 3 to 10 cold forming steps, but compared with the method according to the prior art, one step can be saved. This means that in the prior art, depending on the complexity, 4 to 11 cold forming steps are required.
[0068] The present invention thus facilitates reducing overall production complexity, and thereby costs, as the process is considerably more tolerant of inaccuracies that occur during the process, while also ensuring that other thoughtful measures can be taken to achieve simplified component processing while still achieving components with desired and necessary characteristics.
Claims
1. A method for producing a hardened steel component, wherein a thin steel sheet blank made of hardenable steel and having a metallic corrosion protection layer, in particular a zinc-based metallic corrosion protection layer, is first cold-formed, the resulting cold preformed component is fully or partially austenitized by heating, and then inserted into a form-hardening tool, wherein the insertion temperature is at least 500° C., in particular greater than 600° C., and cooled in the form-hardening tool by contact with the forming tool at a rate above the critical hardening rate, thereby quench-hardening and forming the finished component, wherein the layer thickness of the metallic corrosion protection layer is 7 μm to 20 μm per side, characterized in that Relative to the total surface area of the finished component, 85-99% of the surface area consists of the cold final formed area and 1-15% of the surface area consists of the hot final formed area which is in the process of form hardening.
2. The method according to claim 1, characterized in that: Relative to the total surface area of the finished component, 90-98% of the surface area consists of cold-finished areas and 2-10% of the surface area consists of areas that are hot-finished during the form-hardening process.
3. The method according to claim 1 or 2, characterized in that: Cold forming is carried out in 3-10 cold forming tools, and form hardening and final forming in the hot state are carried out in one tool, the form hardening tool.
4. The method according to any one of the preceding claims, characterized in that To account for the surface which has been hot-finished during the form-hardening process, the deviations to be reshaped from the geometry of the finished component hardened after cold forming, in particular in the case of wavy shapes, should be at least 1 mm.
5. The method according to any one of the preceding claims, characterized in that Prior to form hardening and during or after the heated preform component is inserted into the form hardening tool, an oxygen-containing gas, in particular air, is blown toward, into or flushed into the form hardening tool and / or the preform component.
6. A method according to any one of the preceding claims, characterised in that Prior to form hardening and during or after the heated preform is inserted into the form hardening tool, an oxygen-containing gas, in particular air, is blown into the preform only in those regions in the form hardening tool where deformations exceeding 5 mm occur.
7. A method according to any one of the preceding claims, characterised in that The layer thickness of the metal, in particular alloy galvanized, anticorrosion layer is 10 μm to 15 μm per side.
8. The method according to any one of the preceding claims, characterized in that The anti-corrosion layer of metal, especially alloy zinc, is applied by hot-dip method, especially hot-dip galvanizing method.
9. The method according to any one of the preceding claims, characterized in that The steel strip is made of hardenable alloy steel, in particular boron manganese steel.
10. The method according to claim 9, characterized in that The steel strip used was a steel strip having the following composition (all figures are expressed in wt %): Carbon is at most 0.4, preferably 0.15-0.3 Silicon is at most 1.9, preferably 0.11-1.5 Manganese up to 3.0, preferably 0.8-2.5 Chromium up to 1.5, preferably 0.1-0.9 Molybdenum up to 0.9, preferably 0.1-0.5 Nickel up to 0.9, Titanium up to 0.2, preferably 0.02-0.1 Vanadium up to 0.2, Tungsten up to 0.2, Aluminum up to 0.2, preferably 0.02-0.07 Boron up to 0.01, preferably 0.0005-0.005 Sulfur up to 0.01, preferably up to 0.008 Phosphorus up to 0.025, preferably up to 0.01 Residual iron and impurities.