Method for manufacturing electrolyte cell and electrolyte cell
By adjusting the size and number of protrusions of titanium and nickel components in the electrolytic cell unit and using resistance welding technology, the problems of welding quality and structural resistance value are solved, and more efficient electrolytic cell unit manufacturing is achieved.
Patent Information
- Application Number
- CN202380023381.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-01
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing electrolytic cell unit manufacturing method, it is difficult to balance the welding quality of titanium components and nickel components, resulting in insufficient joint strength and excessive structural resistance, which increases the risk of electrolytic cell damage and worsens unit power usage.
By adjusting the size and number of the first and second ribs, protrusions of different sizes and numbers are formed. Resistance welding technology is used to ensure welding quality, control the welding trace area and resistance welding site density, and reduce the structural resistance value.
It improves the welding quality, reduces the cracking and spreading of the molten base material, reduces the structural resistance value, and increases the unit power usage.
Smart Images

Figure CN118786248A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing an electrolytic cell unit and an electrolytic cell unit. Background Art
[0002] Patent Document 1 listed below discloses a method for producing an electrolytic cell unit which is a constituent element of a multipolar electrolytic cell for electrolyzing an aqueous alkali metal chloride solution to produce chlorine and an alkali metal hydroxide.
[0003] In the manufacturing method, first, the following steps are performed: a titanium separator is arranged on the surface of a titanium first partition wall (first plate) having a flange formed on the periphery, and at least a portion of the separator is welded to the flange of the first partition wall to form a gas-liquid separation chamber. Similarly, the following steps are performed: a nickel separator is arranged on the surface of a nickel second partition wall (second plate) having a flange formed on the periphery, and at least a portion of the separator is welded to the flange of the second partition wall to form a gas-liquid separation chamber.
[0004] Next, a plurality of first ribs made of titanium are arranged on the surface of the first partition wall. In addition, a plurality of cladding plates having a double-layer structure of a titanium layer and a nickel layer are arranged at positions corresponding to the first ribs on the back side of the first partition wall. Furthermore, the back side of the second partition wall is overlapped with the back side of the first partition wall, and a plurality of second ribs made of nickel are arranged at positions corresponding to the cladding plates on the surface of the second partition wall.
[0005] Next, the following steps are performed: resistance welding between each first rib and the surface of the first partition wall, resistance welding between the back surface of the first partition wall and the titanium layer of the cladding plate, resistance welding between the nickel layer of the cladding plate and the back surface of the second partition wall, and resistance welding between the surface of the second partition wall and each second rib are simultaneously performed. In addition, a step of filling the frame member in the space formed between the flange portion of the first partition wall and the flange portion of the second partition wall is performed.
[0006] In addition, Patent Document 1 states the following: According to the above-mentioned manufacturing method, by positioning the first rib and the cladding plate relative to each other with the first partition wall in between, and positioning the second rib and the cladding plate relative to each other with the second partition wall in between, resistance welding between the first rib-first partition wall-cladding plate, and resistance welding between the second rib-second partition wall-cladding plate can be simultaneously achieved, thereby reducing welding man-hours.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2002-155388 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] However, in the conventional method of manufacturing an electrolytic cell unit, there is room for improvement in welding quality.
[0012] Since the electrical resistance of nickel is lower than that of titanium, the heat generated during resistance welding of titanium components (the first partition wall, the first rib and the titanium layer of the cladding plate) is greater than the heat generated during resistance welding of nickel components (the second partition wall, the second rib and the nickel layer of the cladding plate).
[0013] Therefore, it is difficult to adjust the welding current that can ensure sufficient bonding strength between titanium components and sufficient bonding strength between nickel components. When the welding current is too small, the components are not fully melted and the bonding strength is insufficient. On the other hand, when the welding current is too large, the possibility of "scattering" in which the molten metal breaks and scatters becomes higher. If "scattering" occurs, it will lead to a decrease in welding strength and damage to the base material. In addition, since the wall thickness of the base material is reduced due to the scattering of the molten base material, the risk of damage to the electrolytic cell during operation increases in an electrolytic cell that generates corrosive gases such as chlorine. In addition, if the welding quality is poor, there is also a problem that the structural resistance value of the electrolytic cell becomes larger during operation, resulting in a deterioration in the unit power usage.
[0014] An object of the present invention is to provide a method for manufacturing an electrolytic cell unit capable of improving welding quality and an electrolytic cell unit capable of improving specific power usage.
[0015] Solutions for solving problems
[0016] According to the present invention, it is possible to provide the following method for manufacturing an electrolytic cell unit that solves the above-mentioned problems. That is, there is provided "a method for manufacturing an electrolytic cell unit, wherein the manufacturing method comprises: an arrangement step, in which the first rib, the first partition wall, the cladding plate, the second partition wall and the second rib are arranged in the order of the first rib, the first partition wall, the cladding plate, the second partition wall and the second rib, the first rib being formed of the first material, the first partition wall being formed of the first material, the cladding plate having a layer of the first material and a layer of a second material having a lower electrical resistance than the first material, the second partition wall being formed of the first material, and the second partition wall being formed of the second material. 2 material, the second rib is formed of the second material; and a joining process, in which the first rib, the first partition wall, the cladding plate, the second partition wall and the second rib are joined by resistance welding, a first protrusion is formed on a joining portion of the first rib joined to the first partition wall, a second protrusion is formed on a joining portion of the second rib joined to the second partition wall, the size of the first protrusion is different from the size of the second protrusion, or the number of the first protrusion is different from the number of the second protrusion. "
[0017] Preferably, the diameter of the first protrusion is larger than the diameter of the second protrusion. Preferably, the protrusion amount of the first protrusion is smaller than the protrusion amount of the second protrusion. Preferably, the number of the first protrusion is greater than the number of the second protrusion.
[0018] Preferably, the thickness of the first rib is greater than the thickness of the second rib. Preferably, the depth of the first rib is greater than the depth of the second rib. The first material is preferably titanium. The second material may be nickel.
[0019] It is desirable that the diameter of the first protrusion is greater than or equal to 1.05 times and less than or equal to 3.7 times the diameter of the second protrusion. It is preferred that the radial distance from the center of the first protrusion to the center of the second protrusion is set to be within 15 mm. It is suitable that in the joining process, resistance welding is performed on 350 or more and less than or equal to 550 locations per square meter of electrode effective area.
[0020] According to the present invention, the following electrolytic cell unit is provided to solve the above-mentioned problems. That is, an electrolytic cell unit is provided, which is an electrolytic cell unit manufactured by the above-mentioned method for manufacturing an electrolytic cell unit, wherein the area of the welding mark of the first protrusion is not less than 1.15 times and not more than 13.7 times the area of the welding mark of the second protrusion.
[0021] In addition, an electrolytic cell unit is provided. The electrolytic cell unit is manufactured by the above-mentioned method for manufacturing an electrolytic cell unit, wherein a radial distance from a center of the welding mark of the first projection to a center of the welding mark of the second projection is within 15 mm.
[0022] Furthermore, an electrolytic cell unit is provided, which is an electrolytic cell unit manufactured by the above-mentioned method for manufacturing an electrolytic cell unit, wherein the number of the resistance-welded locations per square meter of the electrode effective area is 350 or more and 550 or less.
[0023] Effects of the Invention
[0024] In the manufacturing method of the present invention, since the size of the first protrusion formed on the first rib made of the first material is different from the size of the second protrusion formed on the second rib made of the second material, or the number of the first protrusions is different from the number of the second protrusions, the difference between the heat generated during welding of the component made of the first material and the heat generated during welding of the component made of the second material having a lower resistance than the first material becomes smaller. As a result, the adjustment of the welding current becomes easy, and the situation of "scattering" of the molten base material breaking and flying can be reduced while ensuring sufficient bonding strength between the components made of the first material and sufficient bonding strength between the components made of the second material. Therefore, according to the manufacturing method of the present invention, the welding quality is not easy to deviate, and the welding quality can be improved. In addition, according to the electrolytic cell unit of the present invention, the structural resistance value can be suppressed to a low level, so the unit power usage is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a top view of an electrolytic cell unit manufactured according to the method of the present invention.
[0026] Figure 2 yes Figure 1 AA line section view in.
[0027] Figure 3 yes Figure 1 A partial enlarged cross-sectional view of line BB in FIG.
[0028] Figure 4 It is a cross-sectional view showing the state after the arrangement step is performed.
[0029] Figure 5 This is a cross-sectional view showing a state after the arrangement step is performed when the number of protrusions on the first rib is greater than the number of protrusions on the second rib.
[0030] Figure 6 It is a cross-sectional view showing the state after the bonding step is performed. DETAILED DESCRIPTION
[0031] Hereinafter, an embodiment of a method for producing an electrolytic cell unit according to the present invention will be described with reference to the drawings.
[0032] (Electrolyzer unit 2)
[0033] Reference Figure 1 and Figure 2 To explain, the electrolytic cell unit 2 that can be manufactured by the method of the present invention includes an anode chamber member 4 formed of a first material, and a cathode chamber member 6 formed of a second material having a lower electrical resistance than the first material (see Figure 2 ), and a cladding plate 8 having a layer 8a of a first material and a layer 8b of a second material (see Figure 2As the first material, for example, titanium (Ti) can be used. The second material may be nickel (Ni).
[0034] (Anode chamber component 4)
[0035] like Figure 2 and Figure 3 As shown, the anode chamber member 4 made of a first material (for example, titanium) includes an anode plate 10 , a first partition wall 12 disposed at a distance from the anode plate 10 , and a plurality of first ribs 14 disposed between the anode plate 10 and the first partition wall 12 .
[0036] (Anode plate 10)
[0037] The rectangular anode plate 10 is provided with a plurality of openings, which are not shown. The shape of the openings is arbitrary, and examples thereof include a rhombus shape, a flat fan shape, a slit shape, etc. The plurality of openings can be arranged in a zigzag shape.
[0038] (No. 1 next door 12)
[0039] No.1 Next Door 12 Figure 2 The anode plate 10 is arranged at a distance from the anode plate 10 in the depth direction (direction D) indicated by the arrow D. Figure 2 As shown in FIG. 1 , the lower end side portion of the first partition wall 12 is bent toward the lower end of the anode plate 10, thereby forming a bottom plate 18 defining the lower end of the anode chamber 16. The width direction ( Figure 1 The two side portions (in the direction indicated by the arrow W) are also bent toward the anode plate 10 to form side walls that define the width end portions of the anode chamber 16, which are not shown in the figure.
[0040] (1st rib 14)
[0041] like Figure 1 As shown in FIG. 1 , a plurality of first ribs 14 are provided at intervals in the width direction. Figure 1 The vertical direction (V direction) indicated by the arrow V is extended. Figure 2 and Figure 3 To explain, the first rib 14 includes a main portion 20 extending from the anode plate 10 toward the first partition wall 12 , and a plurality of joining pieces 22 protruding in the width direction from an end portion of the main portion 20 on the first partition wall 12 side.
[0042] The end of the main part 20 on the anode plate 10 side is joined to the anode plate 10 by welding. On the other hand, each joining piece 22 is joined to the surface 12a of the first partition wall 12 by welding. Figure 2As can be understood, a plurality of notches 24 are provided at intervals in the vertical direction at the end of the first partition wall 12 of the main portion 20. The notches 24 are located between adjacent bonding pieces 22. The plurality of notches 24 ensure the flow of liquid and gas in the anode chamber 16 in the width direction.
[0043] (Cathode Chamber Component 6)
[0044] like Figure 2 and Figure 3 As shown, the cathode chamber member 6 made of the second material (eg, nickel) includes a current collector 26 , a second partition wall 28 disposed at a distance from the current collector 26 , and a plurality of second ribs 30 disposed between the current collector 26 and the second partition wall 28 .
[0045] (Current Collector 26)
[0046] Similar to the anode plate 10, a plurality of openings (not shown) are provided in the rectangular current collector 26. The shape of the openings is arbitrary, and for example, a rhombus shape, a flat fan shape, a slit shape, etc. The plurality of openings may be arranged in a zigzag pattern.
[0047] In addition, when the electrolytic cell is assembled by arranging a plurality of electrolytic cell units 2 in the depth direction and applying pressure from both sides in the depth direction, the outer surface ( Figure 2 A cathode plate is installed on the right side of the image through a metal buffer (not shown).
[0048] (No. 28)
[0049] The second partition wall 28 is disposed at a distance from the current collector 26 in the depth direction (direction D). Figure 2 As shown, similarly to the first partition wall 12, the lower end side portion of the second partition wall 28 is bent toward the lower end of the current collector 26 to form a bottom plate 34 that defines the lower end of the cathode chamber 32. The two side portions of the second partition wall 28 in the width direction (W direction) are also bent toward the current collector 26 to form side walls that define the width end portions of the cathode chamber 32, which are not shown.
[0050] (2nd rib 30)
[0051] Similar to the first rib 14, a plurality of second ribs 30 are provided at intervals in the width direction and extend in the up-down direction (V direction). Figure 3 As shown, the plurality of second ribs 30 are arranged at positions corresponding to the positions of the plurality of first ribs 14. The second rib 30 has a main portion 36 extending from the current collector 26 toward the second partition wall 28 and a plurality of engaging pieces 38 protruding in the width direction from the end of the main portion 36 on the second partition wall 28 side.
[0052] The end of the main portion 36 on the collector 26 side is joined to the collector 26 by welding. On the other hand, each joining piece 38 is joined to the surface 28a of the second partition wall 28 by welding. Figure 2 As can be understood, a plurality of notches 40 are provided at intervals in the vertical direction at the end of the second partition wall 28 of the main portion 36. The notches 40 are located between adjacent joining pieces 38. The plurality of notches 40 ensure the flow of liquid and gas in the cathode chamber 32 in the width direction.
[0053] Regarding the relationship between the size of the first rib 14 and the size of the second rib 30, as shown in FIG. Figure 3 As shown, the thickness T1 of the first rib 14 is preferably greater than the thickness T2 of the second rib 30 (T1>T2). In addition, the depth D1 of the main portion 20 of the first rib 14 is preferably greater than the depth D2 of the main portion 36 of the second rib 30 (D1>D2).
[0054] (Cladding plate 8)
[0055] Reference Figure 2 and Figure 3 The cladding plates 8 are provided at intervals in the width direction and extend in the vertical direction. The cladding plates 8 are arranged between the back surface 12b of the first partition wall 12 and the back surface 28b of the second partition wall 28 and at positions corresponding to the joining pieces 22 of the first rib 14 and the joining pieces 38 of the second rib 30.
[0056] The cladding plate 8 of the illustrated embodiment is a double-layered plate in which a layer 8a of a first material (e.g., a titanium layer) and a layer 8b of a second material having a lower electrical resistance than the first material (e.g., a nickel layer) are joined together by explosive welding or the layer 8a of the first material and the layer 8b of the second material are joined together by rolling. The layer 8a of the first material is joined to the back surface 12b of the first partition wall 12 made of the first material by welding. On the other hand, the layer 8b of the second material is joined to the back surface 28b of the second partition wall 28 made of the second material by welding.
[0057] (Supply nozzles 44, 46)
[0058] like Figure 2 As shown, a hollow lower frame 42 with a square cross section is provided at the lower part of the electrolytic cell unit 2. The lower frame 42 can be formed of an appropriate metal material such as stainless steel. The lower frame 42 is provided with two through holes (not shown) that penetrate in the vertical direction. A supply nozzle 44 for supplying raw materials to the anode chamber 16 is installed in one through hole, and a supply nozzle 46 for supplying raw materials to the cathode chamber 32 is installed in the other through hole (see Figure 1 ) In addition, side frames are provided at both side ends in the width direction of the electrolytic cell unit 2, although they are not shown in the figure.
[0059] (Gas-Liquid Separation Chambers 48, 50)
[0060] In the upper part of the electrolytic cell unit 2, as Figure 2 As shown, a gas-liquid separation chamber 48 on the anode side and a gas-liquid separation chamber 50 on the cathode side are provided.
[0061] (Gas-liquid separation chamber 48 on the anode side)
[0062] The gas-liquid separation chamber 48 on the anode side has a separator 52 with an L-shaped cross section made of a first material and a rectangular top plate 54 made of the first material. A plurality of openings (not shown) spaced apart in the width direction are formed in the bottom surface portion 52a of the separator 52. Through the plurality of openings, liquid and gas can flow in the vertical direction between the anode chamber 16 and the gas-liquid separation chamber 48.
[0063] like Figure 1 As shown, a discharge nozzle 56 for discharging the gas and liquid in the gas-liquid separation chamber 48 is provided at an end portion in the width direction of the gas-liquid separation chamber 48. The discharge nozzle 56 is formed of a first material.
[0064] (Gas-Liquid Separation Chamber 50 on Cathode Side)
[0065] The gas-liquid separation chamber 50 on the cathode side has a separator 58 made of a second material and having an L-shaped cross section, and a rectangular top plate 60 made of the second material. A plurality of openings (not shown) are formed at intervals in the width direction on the bottom surface portion 58a of the separator 58. Through the plurality of openings, liquid and gas can flow in the vertical direction between the cathode chamber 32 and the gas-liquid separation chamber 50.
[0066] A discharge nozzle 62 for discharging gas and liquid in the gas-liquid separation chamber 50 is provided at the end in the width direction of the gas-liquid separation chamber 50 (the end opposite to the end provided with the discharge nozzle 56 on the anode side). The discharge nozzle 62 is made of the second material.
[0067] (Method for Manufacturing Electrolytic Cell Unit 2)
[0068] Next, a method for manufacturing the electrolytic cell unit 2 as described above will be described.
[0069] First, the separator 52, the top plate 54 and the discharge nozzle 56 are joined by welding on the upper part of the first partition wall 12 to form the gas-liquid separation chamber 48 on the anode side. Similarly, the separator 58, the top plate 60 and the discharge nozzle 62 are joined by welding on the upper part of the second partition wall 28 to form the gas-liquid separation chamber 50 on the cathode side. Either the gas-liquid separation chamber 48 or 50 may be formed first.
[0070] (Arrangement process)
[0071] After the gas-liquid separation chambers 48 and 50 are formed, an arrangement process is implemented. In the arrangement process, the first rib 14, the first partition wall 12, the cladding plate 8, the second partition wall 28 and the second rib 30 are arranged in the order of the first rib 14, the first partition wall 12, the cladding plate 8, the second partition wall 28 and the second rib 30.
[0072] In this process, for example Figure 4 As shown, the arrangement can be performed in a positional relationship in which the first one from the top is the first rib 14, the second one from the top is the first partition wall 12, the third one from the top is the cladding plate 8, the fourth one from the top is the second partition wall 28, and the fifth one from the top is the second rib 30.
[0073] Or, with Figure 4 Conversely to the positional relationship shown, the first one from the bottom is the first rib 14, the second one from the bottom is the first partition wall 12, the third one from the bottom is the cladding plate 8, the fourth one from the bottom is the second partition wall 28, and the fifth one from the bottom is the second rib 30.
[0074] When the arrangement step is performed, the layer 8a of the first material of the cladding plate 8 faces the back surface 12b of the first partition wall 12 made of the first material, and the layer 8b of the second material of the cladding plate 8 faces the back surface 28b of the second partition wall 28 made of the second material. In addition, the positions of the joining pieces 22 of the first rib 14 and the joining pieces 38 of the cladding plate 8 and the second rib 30 in the width direction are aligned, and the adjacent members are in contact with each other.
[0075] The time sequence of arranging the first rib 14 and the second rib 30, the first partition wall 12 and the second partition wall 28, and the cladding plate 8 is arbitrary. The number of the first rib 14, the second rib 30, and the cladding plate 8 to be arranged may be one or more. However, when arranging the first rib 14, the second rib 30, and the cladding plate 8 in plurality, the number of the first rib 14, the number of the second rib 30, and the number of the cladding plate 8 are made equal.
[0076] (First protrusion 64 and second protrusion 66)
[0077] As reference Figure 4 As can be understood, the first protrusion 64 is formed on the engaging piece 22 (engaging portion engaged with the surface 12a of the first partition wall 12) of the first rib 14. In addition, the second protrusion 66 is formed on the engaging piece 38 (engaging portion engaged with the surface 28a of the second partition wall 28) of the second rib 30. The shapes of the first protrusion 64 and the second protrusion 66 can be any shape such as a circular shape and a rectangular shape.
[0078] In the illustrated embodiment, what is important is that the size of the first protrusions 64 and the size of the second protrusions 66 are different or the number of the first protrusions 64 and the number of the second protrusions 66 are different.
[0079] One example of the difference between the sizes of the first protrusion 64 and the second protrusion 66 is that the diameter d1 of the first protrusion 64 is larger than the diameter d2 of the second protrusion 66 (d1>d2). Another example is that the protrusion amount S1 of the first protrusion 64 is smaller than the protrusion amount S2 of the second protrusion 66 (S1<S2).
[0080] When the diameter d1 of the first protrusion 64 is larger than the diameter d2 of the second protrusion 66, the diameter of the first protrusion 64 is preferably 1.05 times or more and 3.7 times or less, more preferably 1.05 times or more and 3.0 times or less, and particularly preferably 1.15 times or more and 2.5 times or less. Thus, in the electrolytic cell unit obtained through the joining step described later, the area A1 (refer to Figure 6 ) corresponds to the area A2 of the welding mark of the second protrusion 66 (refer to Figure 6 ) is greater than 1.15 times and less than 13.7 times, preferably equal to greater than 1.15 times and less than 6.8 times, and particularly preferably equal to greater than 1.15 times and less than 2.5 times, so that the structural resistance value of the weld can be suppressed to a lower level.
[0081] Generally, the structural resistance value when the components are not welded to each other but are only in contact is larger than the structural resistance value of the continuous structure in which the components are welded to each other. Therefore, if the area A1 of the welding mark of the first protrusion 64 is less than 1.15 times the area A2 of the welding mark of the second protrusion 66, the welding area is small, and therefore the structural resistance value of the mutual welding part of the first rib 14, the first partition wall 12, the cladding plate 8, the second partition wall 28 and the second rib 30 tends to increase, and as a result, there is a tendency for the structural resistance value of the entire electrolytic cell unit to increase.
[0082] On the other hand, when the area A1 of the welding mark of the first protrusion 64 exceeds 13.7 times the area A2 of the welding mark of the second protrusion 66, the heat energy required for welding increases, and therefore, under the influence of thermal deformation caused by welding, the required electrode flatness accuracy deteriorates, resulting in an increase in the structural resistance value. In addition, the increase in the energy required for welding leads to a deterioration in welding quality.
[0083] The difference between the number of the first protrusions 64 and the number of the second protrusions 66 means that, for example, Figure 5 The number of the first protrusions 64 is greater than the number of the second protrusions 66. The number of the first protrusions 64 referred to here refers to the number of protrusions formed on one engaging piece 22 of the first rib 14, and the number of the second protrusions 66 refers to the number of protrusions formed on one engaging piece 38 of the second rib 30.
[0084] exist Figure 5In the example shown, two first protrusions 64 are provided on one engaging piece 22 of the first rib 14, and one second protrusion 66 is provided on one engaging piece 38 of the second rib 30, but the number of each protrusion is not limited to Figure 5 The number shown can be set arbitrarily.
[0085] The relationship between the size and number of the first protrusions 64 and the second protrusions 66 can be summarized as satisfying at least one of the following conditions 1 to 3.
[0086] The diameter d1 of the first protrusion 64 is larger than the diameter d2 of the second protrusion 66 (d1>d2).
[0087] The protrusion amount S1 of the first protrusion 64 is smaller than the protrusion amount S2 of the second protrusion 66 (S1<S2).
[0088] The number of the first protrusions 64 is greater than the number of the second protrusions 66.
[0089] In addition, two of the above conditions 1 to 3 may be satisfied, or all of the above conditions 1 to 3 may be satisfied. Figure 4 In the example satisfying the above conditions 1 and 2, Figure 5 , an example that satisfies all of the above conditions 1 to 3 is shown.
[0090] In the arrangement process, the radial distance (not the vertical direction V, but the distance related to the width direction W and the depth direction D) from the center C1 of the first protrusion 64 to the center C2 of the second protrusion is preferably set to within 15 mm. Thus, in the electrolytic cell unit obtained through the joining process described later, the radial distance from the center of the welding mark of the first protrusion 64 to the center of the welding mark of the second protrusion 66 is within 15 mm, and in the current path from the anode plate 10 to the cathode plate (not shown), the ineffective current flowing along the first partition wall 12 and the second partition wall 28 (ineffective current flowing in a direction orthogonal to the thickness direction of the first partition wall 12 and the second partition wall 28) can be suppressed. Therefore, the electrolytic cell unit with a low resistance value between the anode plate 10 and the cathode plate is obtained.
[0091] (Joining process)
[0092] After the arrangement step is performed, a joining step is performed to join the first rib 14, the first partition wall 12, the cladding plate 8, the second partition wall 28, and the second rib 30 by resistance welding. The resistance welding in the joining step may be spot welding.
[0093] In the joining process, one electrode of a resistance welding machine (not shown) is brought into contact with the joining piece 22 of the first rib 14, and the other electrode of the resistance welding machine is brought into contact with the joining piece 38 of the second rib 30. Thus, the first rib 14, the second rib 30, the first partition wall 12, the second partition wall 28, and the cladding plate 8 are clamped by a pair of electrodes of the resistance welding machine, and a predetermined pressure is applied to the above-mentioned components.
[0094] When current flows from the electrode, Joule heat is generated due to resistance, and the first protrusion 64 melts and collapses. Figure 6 As shown, the engaging piece 22 of the first rib 14 is joined to the surface 12 a of the first partition wall 12 , the second protrusion 66 is melted and collapsed, and the engaging piece 38 of the second rib 30 is joined to the surface 28 a of the second partition wall 28 .
[0095] In addition, due to the Joule heat caused by the resistance when current is applied, the back surface 12b of the first partition wall 12 is bonded to the first material layer 8a of the cladding plate 8, and the back surface 28b of the second partition wall 28 is bonded to the second material layer 8b of the cladding plate 8.
[0096] In such a joining process, it is appropriate to implement resistance welding on more than 350 and less than 550 positions in the effective area of the electrode per square meter. When the number of resistance welding positions is less than 350, it will lead to an increase in the structural resistance value. On the other hand, when the number of resistance welding positions exceeds 550, the effect of suppressing the increase in the structural resistance value accompanying the increase in the resistance welding positions is low, which will lead to a decrease in productivity. In addition, the electrode effective area refers to the area of the portion of the overall area of the electrode plate that is substantially conducive to electrolysis.
[0097] As described above, in the illustrated embodiment, the size of the first protrusion 64 formed on the engaging piece 22 made of the first material is different from the size of the second protrusion 66 formed on the engaging piece 38 made of the second material, or the number of the first protrusion 64 is different from the number of the second protrusion 66. Therefore, the difference between the heat generation of the member made of the first material (the first partition wall 12, the first rib 14, and the layer 8a of the first material of the cladding plate 8) and the heat generation of the member made of the second material having a lower electrical resistance than the first material (the second partition wall 28, the second rib 30, and the layer 8b of the second material of the cladding plate 8) becomes smaller.
[0098] Thus, the welding current can be easily adjusted, and sufficient bonding strength between the components made of the first material and the components made of the second material can be ensured while reducing the "scattering" of the molten base material breaking and scattering. Therefore, according to the embodiment shown in the figure, the welding quality is less likely to vary, and the welding quality can be improved.
[0099] After the joining process is performed in this way, the lower frame 42 is positioned at the lower portion of the first partition wall 12 and the lower portion of the second partition wall 28, and the lower portion of the first partition wall 12 and the lower portion of the second partition wall 28 are respectively joined to the lower frame 42 by welding. Next, the supply nozzle 44 on the anode side and the supply nozzle 46 on the cathode side are joined to the lower frame 42 by welding.
[0100] Then, the side frames are positioned at both side ends of the first partition wall 12 and the second partition wall 28 in the width direction, and the side ends of the first partition wall 12 and the second partition wall 28 in the width direction are respectively joined to the side frames by welding. Then, the anode plate 10 is joined to the end of the main portion 20 of the first rib 14 by welding, and the current collector 26 is joined to the end of the main portion 36 of the second rib 30 by welding.
[0101] As described above, according to the illustrated embodiment, the difference between the heat generation of the first material member and the second material member during welding is small, and internal dispersion can be reduced. Therefore, the welding quality is less likely to vary, and the welding quality can be improved.
[0102] In addition, since the electrical resistance of the first material is greater than that of the second material, when the thickness T1 of the first rib 14 is greater than the thickness T2 of the second rib 30 (T1>T2) as in the illustrated embodiment, the difference between the heating value of the member made of the first material and the heating value of the member made of the second material can be further reduced. In this regard, the same is true when the depth D1 of the first rib 14 is greater than the depth D2 of the second rib 30 (D1>D2).
[0103] Furthermore, when the first material is titanium and the second material is nickel, if the thickness T1 of the first rib 14 is greater than the thickness T2 of the second rib 30 made of the second material or the depth D1 of the first rib 14 is greater than the depth D2 of the second rib 30 made of the second material, the amount of nickel components can be reduced while suppressing the increase in the structural resistance value of the electrolytic cell unit 2, thereby reducing the cost of the electrolytic cell unit 2.
[0104] Description of Reference Numerals
[0105] 2. electrolytic cell unit; 8. cladding plate; 8a. layer of the first material; 8b. layer of the second material; 12. first partition wall; 14. first rib; 28. second partition wall; 30. second rib; 64. first protrusion; 66. second protrusion.
Claims
1. A method for manufacturing an electrolytic cell unit, wherein: The manufacturing method comprises: an arranging step, in which the first rib, the first partition wall, the cladding plate, the second partition wall, and the second rib are arranged in a positional relationship of a first rib, a first partition wall, a cladding plate, a second partition wall, and a second rib in the order of the first rib, the first rib being formed of a first material, the first partition wall being formed of the first material, the cladding plate having a layer of the first material and a layer of a second material having a lower electrical resistance than the first material, the second partition wall being formed of the second material, and the second rib being formed of the second material; as well as a joining step of joining the first rib, the first partition wall, the cladding plate, the second partition wall, and the second rib by resistance welding, A first protrusion is formed on a portion of the first rib that is joined to the first partition wall, and a second protrusion is formed on a portion of the second rib that is joined to the second partition wall. The size of the first protrusions is different from the size of the second protrusions, or the number of the first protrusions is different from the number of the second protrusions.
2. The method for manufacturing an electrolytic cell unit according to claim 1, wherein: The diameter of the first protrusion is larger than the diameter of the second protrusion.
3. The method for manufacturing an electrolytic cell unit according to claim 1 or 2, wherein: The protrusion amount of the first protrusion is smaller than the protrusion amount of the second protrusion.
4. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 3, wherein: The number of the first protrusions is greater than the number of the second protrusions.
5. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 4, wherein: The thickness of the first rib is greater than the thickness of the second rib.
6. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 5, wherein: The depth of the first rib is greater than the depth of the second rib.
7. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 6, wherein: The first material is titanium.
8. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 7, wherein: The second material is nickel.
9. The method for manufacturing an electrolytic cell unit according to claim 2, wherein: The diameter of the first projections is not less than 1.05 times and not more than 3.7 times the diameter of the second projections.
10. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 9, wherein: The radial distance from the center of the first protrusion to the center of the second protrusion is set within 15 mm.
11. The method for manufacturing an electrolytic cell unit according to any one of claims 1 to 10, wherein: In the joining step, resistance welding is performed on 350 or more and 550 or less locations per square meter of the electrode effective area.
12. An electrolytic cell unit manufactured by the method for manufacturing an electrolytic cell unit according to claim 2 or 9, wherein: The area of the welding mark of the first projection is 1.15 times or more and 13.7 times or less of the area of the welding mark of the second projection.
13. An electrolytic cell unit manufactured by the method for manufacturing an electrolytic cell unit according to any one of claims 1 to 11, wherein: A radial distance from a center of the welding mark of the first protrusion to a center of the welding mark of the second protrusion is within 15 mm.
14. An electrolytic cell unit manufactured by the method for manufacturing an electrolytic cell unit according to any one of claims 1 to 11, wherein: The number of resistance welded locations is 350 or more and 550 or less per square meter of electrode effective area.