Preparation method and application of titanium alloy ring piece for aero-engine

Through the plasma rotating electrode method and hot isostatic pressing treatment, the problems of uneven structure and limited size in the preparation of traditional titanium alloy rings are solved, and the uniform performance of rings of arbitrary thickness and complex shape is achieved and the yield rate is improved. and reduced production costs.

CN118788970APending Publication Date: 2024-10-18SINO EURO MATERIALS TECH OF XIAN CO LTD

Patent Information

Application Number
CN202411031788.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The traditional titanium alloy ring preparation process has problems such as uneven structure, limited size, low material utilization, long forging process, and many cracks. It is especially difficult to produce large-sized and complex-shaped rings, and has low efficiency and low yield rate.

Method used

The plasma rotating electrode method was used to prepare titanium alloy metal spherical powder, and by designing an annular metal jacket for screening and vibration powder loading, combined with hot isostatic pressing densification treatment, a titanium alloy ring with a uniform structure was prepared.

Benefits of technology

It achieves the efficient preparation of titanium alloy rings of arbitrary thickness and complex shape, with excellent performance, uniform structure, and high yield rate, reducing the production process and cost, and avoiding thermal stress during heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788970A_ABST
    Figure CN118788970A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aerospace, and particularly relates to a preparation method and application of a titanium alloy ring piece for an aero-engine. The titanium alloy ring piece prepared through the preparation method is not limited by the product size, and is excellent in performance and high in yield; the same ring piece is uniform in structure and isotropic; the consistency of products in different batches is high, and the product quality is stable; and the titanium alloy subjected to hot isostatic pressing can obtain a compact structure, phase change does not occur in the hot isostatic pressing process, a basket structure obtained through PREP powder preparation is reserved in the powder, a small-size equiaxial alpha structure obtained through mutual extrusion deformation of the powder in the hot isostatic pressing process is obtained on the edge of the powder, and the structure has good toughness and is not prone to deformation. The strength, plasticity and comprehensive performance are good and superior to those of a forged structure; and the obtained ring piece product does not have thermal stress, is excellent in performance and can meet the use requirement, so that thermal treatment is not needed, the preparation process is reduced, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aerospace technology and relates to the preparation of titanium alloy rings for aerospace, and specifically to a preparation method of a titanium alloy ring for an aero-engine and an application thereof. Background Art

[0002] The preparation process of titanium alloy rings is usually to forge the titanium alloy ingot after smelting, upset and draw it multiple times, and form it to obtain a titanium alloy bar blank, which is then sawed and cut into pieces, and then upset, punched, expanded, or expanded and then rolled into a ring to finally obtain the ring.

[0003] The traditional titanium alloy ring preparation process is long, the production cycle has many forging fires, and the punching core material is wasted. There are also problems such as cracks, uneven deformation, deformation dead zone, difficult to control deformation, inconsistent organization, and uneven performance during the hole expansion process. In addition, grinding and damage removal are required between multiple fires. The ring rolling process is only suitable for preparing rings with a wall thickness / ring height greater than 2 and a wall thickness greater than 20mm. The production of rings with a diameter greater than 3000mm requires a larger reamer, and can only be produced in single or double sizes, with low efficiency and low yield. For simple special-shaped rings, mold production is required, and complex special-shaped rings cannot be produced. Therefore, it is urgent to provide a preparation method for titanium alloy rings for aircraft engines to overcome the problems of uneven forging organization, limited ring size, low material utilization, long forging process, and many forging cracks.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art. The present invention provides a method for preparing a titanium alloy ring for an aero-engine.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] On the one hand, the present invention provides a method for preparing a titanium alloy ring for an aero-engine, and the specific steps are as follows:

[0008] S1. Preparing titanium alloy metal spherical powder by a plasma rotating electrode method, and sieving the prepared titanium alloy metal spherical powder to obtain a powder with a particle size of 53-250 μm and an oxygen content of less than 50 ppm;

[0009] S2. Design and prepare an annular metal sheath. The design of the annular metal sheath is based on the size of the part. The inner diameter of the sheath is 0.8-0.85 times the inner diameter of the part, the outer diameter is 1.2-1.25 times the outer diameter of the part, and the height is 1.1-1.15 times the height of the part. The inner circle and outer circle of the annular metal sheath are prepared by steel plate rolling process and then welded. The upper plate and lower plate of the annular sheath are prepared by plate machining method. After that, different sheath parts are welded together. A powder filling hole is welded on the outer circle to place a metal funnel for powder filling. The steel plate is 3-5mm 45 steel plate.

[0010] S3, the powder after screening by S1 is loaded into the annular metal sheath prepared by S2, and a 250 micron screen is used to filter the powder again during loading; during the loading process, the sheath is placed on the powder loading platform, and the powder loading platform is provided with 4 vibration motors, and the vibration motors are installed at 4 positions under the platform corresponding to the ring, and the 4 positions are at an angle of 90°, and the powder, the annular metal sheath and the platform can be vibrated at the same time, the vibration frequency is 30-35HZ, the vibration amplitude is 5-7mm, the powder tap density is 68%-70% of the theoretical density of the material, and the powder loading weight = powder tap density × annular sheath volume;

[0011] S4, heating and vacuuming the annular metal sheath filled with powder to remove the gas between the powder particles, and then sealing and welding; placing the annular metal sheath in a heating furnace, heating temperature is 500-550℃, the furnace temperature uniformity of the heating furnace is ±20℃, and heat preservation and vacuum degassing are carried out, the heat preservation and degassing time = ring wall thickness × first insulation coefficient, wherein the first insulation coefficient is equal to 6-8min / mm, when the temperature reaches 500℃ and the vacuum degree is greater than 1.0×10 -5 When the heating and degassing is completed, the insulation and degassing time is calculated. The insulation and degassing time = ring wall thickness × the first insulation coefficient, wherein the first insulation coefficient is equal to 6-8min / mm. After the heating and degassing is completed, the powder loading port is sealed with hydraulic pliers. The sealing length is 40-70mm. At the same time, in order to prevent the powder from being drawn into the mechanical pump molecular pump group, a steel wool filter device is provided in the powder loading port to prevent the powder from being drawn into the mechanical pump.

[0012] S5. Perform hot isostatic pressing densification treatment on the bag filled with powder, wherein the hot isostatic pressing treatment adopts a synchronous heating and pressure rising process, the holding temperature is 900-920°C, the holding pressure is 130-140Mpa, the holding time = ring wall thickness × second insulation coefficient, wherein the second insulation coefficient is 3-4min / mm, and the cooling rate is 2-3°C / min;

[0013] S6. The annular metal sheath is removed by machining to obtain a titanium alloy ring for an aero-engine.

[0014] Specifically, the mechanical properties of the titanium alloy ring prepared by the preparation method are as follows: tensile strength is >1030MPa, yield strength is >900MPa, elongation is >15%, and cross-sectional shrinkage is >30%.

[0015] On the other hand, the present invention provides an application of a method for preparing a titanium alloy ring for an aero-engine, wherein the method is used to prepare a thin-walled, large-sized titanium alloy ring for an aero-engine.

[0016] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0017] The preparation method of the present invention can be used to prepare titanium alloy rings of any thickness / height, any thickness and complex shape. The prepared titanium alloy rings are not restricted by product size, have excellent performance and a high yield rate. Moreover, the same ring has uniform structure and isotropic properties. The products of different batches have high consistency and stable product quality. Moreover, the titanium alloy after hot isostatic pressing can obtain a dense structure, and no phase change occurs during the hot isostatic pressing process. The basket structure obtained by PREP powder making is retained inside the powder, and the small-sized equiaxed α structure obtained by mutual extrusion and deformation between powders during hot isostatic pressing is obtained at the edge of the powder. This structure has good toughness, good comprehensive strength and plasticity properties, and is better than the forging structure. Moreover, the obtained ring product does not have thermal stress, has excellent performance and can meet the use requirements. Therefore, no heat treatment is required, the preparation process is reduced, and the production cost is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0020] Figure 1 The present invention is a flow chart of the preparation of the titanium alloy ring;

[0021] Figure 2 It is a schematic diagram of the cross-sectional structure of the metal sheath and the powder loading port of the present invention;

[0022] Figure 3 This is a diagram showing the structure of the titanium alloy prepared by the present invention. DETAILED DESCRIPTION

[0023] Here, exemplary embodiments will be described in detail, and examples thereof are shown in the accompanying drawings. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention as detailed in the appended claims.

[0024] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0025] See also Figure 1 As shown, the present invention provides a method for preparing a titanium alloy ring for an aero-engine, and the specific steps are as follows:

[0026] S1. Preparing titanium alloy metal spherical powder by plasma rotating electrode method PREP, and sieving the prepared titanium alloy powder. The particle size after sieving is 53-250 μm, and the oxygen content is less than 50 ppm;

[0027] S2. Design and prepare an annular metal sheath. The design of the annular metal sheath is based on the size of the part. The inner diameter of the sheath is 0.8-0.85 times the inner diameter of the part, the outer diameter is 1.2-1.25 times the outer diameter of the part, and the height is 1.1-1.15 times the height of the part. The inner circle and outer circle of the annular metal sheath are prepared by steel plate rolling process and then welded. The upper plate and lower plate of the annular sheath are prepared by plate machining method. After that, different sheath parts are welded together, and a powder filling hole is welded on the outer circle to place a metal funnel for powder filling. The steel plate is 3-5mm 45 steel plate, see Figure 2 As shown;

[0028] S3, the powder after screening by S1 is loaded into the annular metal sheath prepared by S2, and a 250 micron screen is used to filter the powder again when loading the powder; the powder loading platform is provided with 4 vibration motors, which are installed at 4 positions under the platform corresponding to the ring, and the 4 positions are at an angle of 90°, and the powder, the annular metal sheath and the platform can be vibrated at the same time. The number of motors to be turned on is selected according to the size of the ring, the vibration frequency is 30-35HZ, the vibration amplitude is 5-7mm, the powder tap density is 68%-70% of the theoretical density of the material, and the powder loading weight = powder tap density × annular sheath volume;

[0029] S4, heating and vacuuming the annular metal sheath filled with powder to remove the gas between the powder particles, and then sealing and welding; placing the annular metal sheath in a heating furnace at a heating temperature of 500-550°C, when the vacuum degree is greater than 1.0×10 -5When the temperature reaches 500°C, the insulation and degassing time is calculated. The insulation and degassing time = ring wall thickness × the first insulation coefficient, wherein the first insulation coefficient = 6-8min / mm, the furnace temperature uniformity of the heating furnace is ±20°C, after the heating and degassing is completed, the powder loading port is sealed with hydraulic pliers, and the sealing length is 40-70mm. At the same time, in order to prevent the powder from being drawn into the mechanical pump molecular pump group, a filtering device is set in the powder loading port;

[0030] S5. Perform hot isostatic pressing densification treatment on the annular metal sheath filled with powder, wherein the hot isostatic pressing treatment adopts a synchronous heating and pressure rising process, the holding temperature is 900-920°C, the holding pressure is 130-140Mpa, the holding and holding time are both the ring wall thickness × the second insulation coefficient, wherein the second insulation coefficient is 3-4min / mm, and the cooling rate is 2-3°C / min;

[0031] S6. The annular metal sheath is removed by machining to obtain a titanium alloy ring for an aero-engine.

[0032] Specifically, the mechanical properties of the titanium alloy ring prepared by the preparation method are as follows: tensile strength is >1030MPa, yield strength is >900MPa, elongation is >15%, and cross-sectional shrinkage is >30%.

[0033] Example 1

[0034] This embodiment provides a method for preparing a titanium alloy ring for an aero-engine, preparing a small-sized titanium alloy ring of Φ300×Φ200×50, preparing 4 titanium alloy rings at a time, leaving a 5mm machining margin between each ring, so the blank to be prepared is Φ300×Φ200×215, wherein the wall thickness of the ring is (300-200) / 2;

[0035] The specific steps are as follows:

[0036] Step 1: Prepare titanium alloy powder by plasma rotating electrode (PREP) method, and sieve to obtain titanium alloy powder with a particle size of 53-250 microns and an oxygen content of less than 50 ppm;

[0037] Step 2: Prepare an annular metal sheath with a size of Φ360×Φ180×236. The raw material is 3mm thick 45 steel plate. The inner circle and outer circle of the annular metal sheath are prepared by steel plate rolling process and then welded. The upper plate and lower plate of the annular sheath are prepared by plate machining method. Then, different sheath parts are welded together. A powder filling hole is welded on the outer circle to place a metal funnel for powder filling.

[0038] Step 3: Put the sieved powder into the metal sleeve through a metal funnel, wherein a 250-micron screen is provided in the metal funnel to filter the powder again; place the metal sleeve on the powder loading platform, and turn on four motors to vibrate and load the powder, with a vibration frequency of 32 Hz and a vibration amplitude of 5 mm;

[0039] Step 4: Heat the bag filled with powder to 500°C and the vacuum degree reaches 1.0×10 -5 When the temperature and vacuum degree are reached at pa, the insulation time starts to be calculated, and the insulation time is 300 minutes. The mechanical pump molecular pump group is connected to the bag full of powder through a pipeline. In order to prevent the powder from being drawn into the mechanical pump molecular pump group, a steel wool filter device is arranged in the pipeline to prevent the powder from being drawn into the mechanical pump. After the degassing is completed, the mechanical pump molecular pump group and the pipeline of the bag full of powder are sealed and welded with hydraulic pliers, and the sealing length is 40mm;

[0040] Step 5: The package filled with powder is subjected to hot isostatic pressing densification treatment. The hot isostatic pressing temperature is 920℃, the pressure is 135Mpa, and the heat and pressure are maintained for 150min. After hot isostatic pressing, the titanium alloy can obtain a dense structure. No phase change occurs during the hot isostatic pressing process. The basket structure obtained by PREP powder making is retained inside the powder. The small-sized equiaxed α structure obtained by mutual extrusion and deformation between powders during hot isostatic pressing is obtained at the edge of the powder. This structure has good toughness, good comprehensive strength and plasticity, and uniform structure, which is better than the forging structure; see Figure 3 As shown;

[0041] Step 6: First, the sheath is removed by machining, and the size after machining is Φ300×Φ200×215. Then, wire cutting is used to divide it into 1:4 to obtain four titanium alloy rings with a size of Φ300×Φ200×50. The surface of the titanium alloy rings is further machined to a bright state.

[0042] The mechanical properties of the prepared titanium alloy ring are as follows: tensile strength is >1030MPa, yield strength is >900MPa, elongation is >15%, and cross-sectional shrinkage is >30%.

[0043] Since the obtained titanium alloy ring is subjected to a tensile performance test and has no thermal stress, and has a uniform structure and excellent performance, it can meet the use requirements and therefore does not require heat treatment.

[0044] Example 2

[0045] This embodiment provides a method for preparing a titanium alloy ring for an aero-engine, and prepares a large thin-walled titanium alloy ring of Φ3000×Φ2960×100, wherein the ring wall thickness = (3000-2960) / 2;

[0046] The specific steps are as follows:

[0047] Step 1: Prepare titanium alloy powder by plasma rotating electrode (PREP) method, and sieve to obtain titanium alloy powder with a particle size of 53-250 microns and an oxygen content of less than 50 ppm;

[0048] Step 2: Prepare an annular metal sheath with a size of Φ3660×Φ2660×115. The raw material is 3mm thick 45 steel plate. The inner circle and outer circle of the annular metal sheath are prepared by steel plate rolling process and then welded. The upper plate and lower plate of the annular sheath are prepared by plate machining method. Then, different sheath parts are welded together. A powder filling hole is welded on the outer circle to place a metal funnel for powder filling.

[0049] Step 3: Put the sieved powder into the metal sleeve through a metal funnel, wherein the metal funnel is provided with a 250-micron screen to filter the powder again; place the metal sleeve on the powder loading platform, turn on two motors to vibrate and load the powder, the vibration frequency is 35HZ, and the vibration amplitude is 7mm;

[0050] Step 4: Heat the bag filled with powder to 530℃ and the vacuum degree reaches 1.0×10 -5 pa, when both the temperature and vacuum degree are reached, the insulation time is calculated, and the insulation time is 160 minutes. The mechanical pump molecular pump group is connected to the bag full of powder through a pipeline. In order to prevent the powder from being drawn into the mechanical pump molecular pump group, a steel wool filter device is arranged in the pipeline to prevent the powder from being drawn into the mechanical pump. After the degassing is completed, the mechanical pump molecular pump group and the pipeline of the bag full of powder are sealed and welded with hydraulic pliers, and the sealing length is 40mm;

[0051] Step 5: The package filled with powder is subjected to hot isostatic pressing densification treatment. The hot isostatic pressing temperature is 920℃, the pressure is 135Mpa, and the temperature and pressure are kept for 80min. After hot isostatic pressing, the titanium alloy can obtain a dense structure. No phase change occurs during the hot isostatic pressing process. The basket structure obtained by PREP powder making is retained inside the powder. The small-sized equiaxed α structure obtained by mutual extrusion and deformation between powders during hot isostatic pressing is obtained at the edge of the powder. This structure has good toughness, good comprehensive strength and plasticity, and uniform structure, which is better than the forging structure; see Figure 3 As shown;

[0052] Step 6: First, remove the sheath by machining. The size after machining is Φ3000×Φ2960×100. Further remove the sheath and machine the surface of the titanium alloy ring to a bright state.

[0053] The mechanical properties of the prepared titanium alloy ring are as follows: tensile strength is >1030MPa, yield strength is >900MPa, elongation is >15%, and cross-sectional shrinkage is >30%.

[0054] Since the obtained titanium alloy ring is subjected to a tensile performance test and has no thermal stress, and has a uniform structure and excellent performance, it can meet the use requirements and therefore does not require heat treatment.

[0055] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0056] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a titanium alloy ring for an aero-engine, characterized in that: The specific steps are as follows: S1. Preparing titanium alloy metal spherical powder by plasma rotating electrode method, and screening the powder as required; S2. Design and prepare annular metal sheath; S3, putting the powder screened in S1 into an annular metal sleeve and vibrating it at the same time; S4, heating the annular metal sheath filled with powder, evacuating and degassing it for a certain period of time, and then sealing and welding it; S5, performing hot isostatic pressing densification treatment on the annular metal sheath after sealing and welding; S6. The annular metal sheath is removed by machining to obtain a titanium alloy ring for an aero-engine.

2. The preparation method according to claim 1, characterized in that: In S1, the titanium alloy metal spherical powder is sieved to obtain a powder with a particle size of 53-250 μm and an oxygen content of less than 50 ppm.

3. The preparation method according to claim 1, characterized in that: In S2, the design of the annular metal sheath is based on the size of the part, wherein the inner diameter of the annular metal sheath is 0.8-0.85 times the inner diameter of the part, the outer diameter is 1.2-1.25 times the outer diameter of the part, and the height is 1.1-1.15 times the height of the part.

4. The preparation method according to claim 1, characterized in that: In S3, the powder is filtered again using a 250-micron screen before filling.

5. The preparation method according to claim 1, characterized in that: In S3, the bag is vibrated during the powder filling process, with a vibration frequency of 30-35 Hz and a vibration amplitude of 5-7 mm. The powder tap density is 68%-72% of the theoretical density of the material.

6. The preparation method according to claim 1, characterized in that: In S4, the heating temperature is required to be 500-550°C and the degassing vacuum degree is >1.0×10 -5 pa, when the vacuum degree and temperature are reached, continue heating and degassing for a certain period of time. When the heating and degassing are completed, the powder loading port is sealed and welded, and the sealing length is 40-70mm.

7. The preparation method according to claim 6, characterized in that: In S4, heating and degassing time = ring wall thickness × first insulation coefficient, wherein the first insulation coefficient is 6-8 min / mm, and insulation time starts to be calculated when both temperature and vacuum degree meet the requirements.

8. The preparation method according to claim 1, characterized in that: In S5, the hot isostatic pressing treatment adopts a synchronous heating and pressure process, the temperature and pressure are reached at the same time, the insulation temperature is 900-920°C, the pressure is 130-140Mpa, the insulation and pressure are maintained for a certain time, and the cooling rate is 2-3°C / min.

9. The preparation method according to claim 8, characterized in that: In S5, the heat preservation and pressure holding time is the ring wall thickness×the second heat preservation coefficient, wherein the second heat preservation coefficient is 3-4 min / mm.

10. The use of the preparation method according to any one of claims 1 to 9, characterized in that: The preparation method is used for preparing titanium alloy ring parts for aviation engines.

Citation Information

Patent Citations

  • Powder hot isostatic pressing molding method of titanium alloy automobile connecting shaft rod

    CN104174848A

  • High-density Ti2AlNb powder alloy near-net forming technology

    CN105665729A

  • Method for preparing intermediate case through hot isostatic pressure powder metallurgy

    CN108927517A

  • Hot isostatic pressing process of Ti2AlNb alloy powder

    CN110607464A

  • Titanium-based workpiece and hot isostatic pressing preparation method thereof

    CN115026285A

Cited By

  • Preparation method and application of large-size titanium steel bimetallic ring piece