Sponge titanium in-situ additive manufacturing method for titanium alloy component

CN118789074APending Publication Date: 2024-10-18BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411154697.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing titanium alloy additive manufacturing methods are high-cost and low-efficiency. In particular, traditional arc additive manufacturing uses wire as raw material, resulting in the cost of preparing large-size titanium alloy components being still high.

Method used

Sponge titanium is used as the raw material, and arc additive manufacturing technology is used for fusion deposition in a gas shield. DC pulse arc and tungsten electrode welding gun are used, combined with reasonable process parameters and protective atmosphere conditions, to form titanium alloy components layer by layer.

Benefits of technology

It achieves the preparation of large-size titanium alloy components at low cost and low equipment requirements, reduces material and equipment costs, improves manufacturing efficiency and the compactness of finished products, and avoids the occurrence of macro defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789074A_ABST
    Figure CN118789074A_ABST
Patent Text Reader

Abstract

The invention discloses a titanium sponge in-situ additive manufacturing method of a titanium alloy component, and relates to the technical field of titanium alloy component preparation, and the method comprises the following steps: S1, placing a titanium alloy substrate on a workbench, arranging a fence around the titanium alloy substrate, and uniformly paving a layer of titanium sponge on the titanium alloy substrate; s2, the titanium alloy substrate and the enclosure cover are covered with a gas protection cover, and a protection atmosphere is built in the gas protection cover; s3, a welding gun is located above the titanium sponge and located in the gas protection cover, the welding gun moves according to the set planned path, and fused deposition is conducted on the titanium sponge located on the planned path to enable the titanium sponge to finally form a deposition layer; s4, after the welding gun completes the deposition layer, a layer of new sponge titanium continues to be laid on the deposition layer on the basis of the deposition layer; s5, the steps S3 to S4 are repeated until a semi-finished product of the titanium alloy component is formed; and post-processing the semi-finished product to form the final titanium alloy component. And the large-size and low-cost titanium alloy component is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloy component preparation, and in particular to a titanium sponge in-situ additive manufacturing method for titanium alloy components. Background Art

[0002] Titanium alloy is a metal material with low density, high specific strength, high corrosion resistance and high heat resistance. Due to its excellent comprehensive performance, it has been widely used in aerospace, military and weapons, marine and shipbuilding, vehicles and biomedical engineering. The traditional manufacturing methods of titanium alloys mainly include machining, investment casting and additive manufacturing. Among them, additive manufacturing of titanium alloys often uses titanium alloy wire or titanium alloy powder as raw materials, and realizes layer-by-layer stacking of materials through melt deposition or selective melting, so as to achieve the purpose of nearly forming the shape of the parts. In recent years, additive manufacturing technology has been widely used due to its advantages such as controllable process, high material utilization rate and controllable cost.

[0003] TC4 titanium alloy is a widely used raw material in the field of additive manufacturing titanium alloys, with the price of wire being 150 yuan per kilogram and the price of powder being 550 yuan per kilogram. Sponge titanium is a raw material for processing a series of titanium products. It has a porous appearance, irregular shape, and light gray color. It has the potential to be used as a raw material for additive manufacturing. Titanium ore is enriched, chlorinated, and then reduced and distilled to obtain sponge-like metallic titanium. Taking the national standard grade 0 sponge titanium with a particle size of 3mm to 12.7mm as an example, its price per kilogram is 60 yuan, which is much lower than the price of finished titanium plates and titanium wires.

[0004] At present, the commonly used methods for additive manufacturing of titanium alloys are: electron beam selective melting (SEBM), laser melt deposition (LDM), selective laser melting (SLM), electric arc additive manufacturing (WAAM), etc. Among them, electron beam selective melting (SEBM) needs to be processed in a vacuum environment, has high requirements for equipment, and has size restrictions on samples; while laser melt deposition (LDM) and selective laser melting (SLM) have specific requirements for the reflectivity of the processed materials, resulting in high manufacturing costs and low processing efficiency; traditional electric arc additive manufacturing (WAAM) uses wire as raw material, and the cost is still relatively high.

[0005] Therefore, it is necessary to achieve large-scale and low-cost preparation of titanium alloy components by utilizing the low cost of sponge titanium and arc heat source and the small size restrictions of arc additive manufacturing. Summary of the invention

[0006] The purpose of the present invention is to provide a titanium sponge in-situ additive manufacturing method for titanium alloy components, so as to solve the problems existing in the above-mentioned prior art and realize the preparation of large-sized and low-cost titanium alloy components.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] The present invention provides a method for in-situ additive manufacturing of titanium sponge for titanium alloy components, comprising the following steps:

[0009] S1, placing a titanium alloy substrate on a workbench, setting up enclosures around the titanium alloy substrate, and evenly spreading a layer of titanium sponge on the titanium alloy substrate;

[0010] S2, a gas protective cover is provided on the workbench, wherein the gas protective cover covers the titanium alloy substrate and the enclosure inside, and a protective atmosphere is created inside the gas protective cover;

[0011] S3, setting a welding gun of the arc additive manufacturing equipment in the gas shield, the welding gun is located above the titanium sponge, and the welding gun moves according to a set planned path, and finally forms a deposition layer by melting and depositing the titanium sponge located on the planned path;

[0012] S4, after the welding gun completes the deposition layer, a new layer of titanium sponge is continuously laid on the deposition layer as a basis;

[0013] S5, repeating steps S3 to S4 until a semi-finished product of a titanium alloy component is formed; the semi-finished product is post-processed to form a final titanium alloy component.

[0014] Preferably, the particle size of the sponge titanium is 3mm to 7mm; the arc type of the arc additive manufacturing equipment is a DC pulse arc, and the DC pulse frequency is 1.0Hz to 1.4Hz, the peak current is 290A to 340A, the base current is 55A to 75A, and the peak duty cycle is 58% to 65%; a tungsten electrode is provided at the bottom of the welding gun, and the vertical distance between the tungsten electrode and the sponge titanium laid on the corresponding layer is 8mm to 10mm; the moving speed of the welding gun is 150mm / min to 200mm / min.

[0015] Preferably, the height of the deposited layer is 2 mm to 2.5 mm.

[0016] Preferably, in S4, after a certain layer of the deposited layer is completed, the arc of the welding torch is extinguished, and after the deposited layer is cooled to no longer glow red, the next layer of the sponge titanium is laid on top.

[0017] Preferably, after re-laying the next layer of the titanium sponge, the welding gun is raised to a specified height, the protective atmosphere is re-created in the gas protection hood, and the welding gun moves along a corresponding planned path to complete the formation of the deposition layer of this layer.

[0018] Preferably, the welding gun starts to work when the oxygen content in the gas protection cover is less than 1%.

[0019] Preferably, the enclosure is made of stainless steel plate.

[0020] Compared with the prior art, the present invention has achieved the following technical effects:

[0021] The titanium sponge in-situ additive manufacturing method for titanium alloy components provided by the present invention achieves the purpose of preparing large-sized, low-cost titanium alloy components using titanium sponge as raw material by utilizing the low cost of titanium sponge and arc heat source and the small size restriction of arc additive manufacturing; combining the advantages of low price of titanium sponge raw material and low cost and small size restriction of arc additive manufacturing technology, compared with selective laser melting (SLM) and laser melt deposition (LDM), it has no specific requirements for materials and low material cost; compared with electron beam selective melting (SEBM), it only needs to be processed in a protective atmosphere that is easier to create, does not require a vacuum environment, has low requirements for equipment, and has no restrictions on processing size; compared with traditional arc additive manufacturing (WAAM), it uses titanium sponge as raw material, which further reduces the manufacturing cost, which is conducive to the large-scale and low-cost preparation of titanium alloy structural parts.

[0022] Furthermore, by selecting sponge titanium with a particle size of 3mm to 7mm as raw material, and coordinating the relevant process parameter settings of the arc additive manufacturing equipment, as well as the vertical distance setting between the tungsten electrode at the bottom of the welding gun and the sponge titanium, and the moving speed setting of the welding gun, a titanium alloy component with a dense interior and no macroscopic defects such as collapse and cracks on the surface is formed.

[0023] Furthermore, the height of the deposition layer is set to 2 mm to 2.5 mm, which can maintain a faster forming speed and improve the overall manufacturing efficiency; and the shape and size of each deposition layer can be more accurately controlled; by reasonably controlling the height of each deposition layer, the overall internal density effect formed can be guaranteed.

[0024] Furthermore, after completing a certain layer of deposition, the arc of the welding torch is extinguished first, and then the next layer of sponge titanium is laid on top, which can ensure manufacturing safety and improve safety.

[0025] Furthermore, when preparing the next layer of deposition, the protective atmosphere in the gas protection hood is recreated. The protective atmosphere can effectively isolate harmful gases such as oxygen and nitrogen in the air, reduce the reaction of these gases with the molten pool during welding, thereby avoiding the formation of pores and inclusions and ensuring the forming effect of the deposition layer; it can stabilize the burning of the arc, make the arc more concentrated, and the energy more concentrated, which is beneficial to the transition of the molten droplet and the formation of the molten pool, and improve the stability and consistency of the welding process.

[0026] Furthermore, in an environment where the oxygen content in the gas protective hood is less than 1%, the contact between the molten pool metal and oxygen can be reduced, reducing the occurrence of oxidation reactions; and the generation of pores can be reduced, improving the density of the deposited layer; the low-oxygen environment helps to stabilize the combustion of the arc, reduce arc fluctuations and spattering, and improve deposition efficiency and forming accuracy.

[0027] Furthermore, stainless steel fencing is selected. Due to the high temperature and high energy generated by the electric arc, certain substances in the surrounding environment may undergo chemical reactions to produce corrosive gases or liquids. Stainless steel fencing can effectively prevent these corrosive substances from damaging the titanium alloy substrate and equipment. Stainless steel material has a high melting point and good thermal stability, and can maintain stable physical and chemical properties in a high temperature environment. It will not melt, deform or produce harmful substances due to high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 A schematic diagram of a manufacturing device used in the in-situ additive manufacturing method of titanium sponge for a titanium alloy component provided by the present invention;

[0030] Figure 2 A schematic diagram of the forming mechanism in the titanium sponge in-situ additive manufacturing method of the titanium alloy component provided by the present invention;

[0031] Figure 3 A semi-finished product of a titanium alloy component with a square structure prepared by the titanium sponge in-situ additive manufacturing method of a titanium alloy component provided by the present invention;

[0032] Figure 4 for Figure 3 Schematic diagram of longitudinal section;

[0033] Figure 5 for Figure 3 Internal metallographic structure diagram.

[0034] In the figure: 1- workbench; 2- titanium alloy substrate; 3- enclosure; 4- welding gun; 5- titanium sponge; 6- semi-finished product; 7- gas protection cover; 8- control system; 9- protective gas cylinder; 10- welding machine; 11- titanium sponge on both sides of the arc; 12- titanium sponge directly below the arc; 13- arc. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The purpose of the present invention is to provide a titanium sponge in-situ additive manufacturing method for titanium alloy components, so as to solve the problems existing in the prior art and realize the preparation of large-sized and low-cost titanium alloy components.

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0038] Embodiment 1

[0039] This embodiment provides a titanium sponge in-situ additive manufacturing method for a titanium alloy component, using titanium sponge 5 as a raw material and adopting arc additive manufacturing technology to prepare a titanium alloy component. Figure 1 to Figure 5 As shown, the following steps are included:

[0040] S1, placing a titanium alloy substrate 2 on a workbench 1, setting a fence 3 around the titanium alloy substrate 2, and evenly spreading a layer of titanium sponge 5 on the titanium alloy substrate 2;

[0041] S2, a gas protection cover 7 is installed on the workbench 1, the gas protection cover 7 covers the titanium alloy substrate 2 and the enclosure 3 inside, and a protective atmosphere is created inside the gas protection cover 7;

[0042] S3, placing a welding gun 4 of the arc additive manufacturing equipment in the gas shield 7, the welding gun 4 is located above the titanium sponge 5, and the welding gun 4 moves according to the set planned path, and finally forms a deposition layer by melting and depositing the titanium sponge 5 located on the planned path;

[0043] S4, after the welding gun 4 completes the deposition layer, a new layer of titanium sponge 5 is continuously laid on the deposition layer as a basis;

[0044] S5, repeating steps S3 to S4 until a semi-finished product 6 of a titanium alloy component is formed; the semi-finished product 6 is post-processed to form a final titanium alloy component.

[0045] By utilizing the low cost of titanium sponge 5 and arc heat source and the small size restriction of arc additive manufacturing, the purpose of preparing large-sized and low-cost titanium alloy components using titanium sponge 5 as raw material is achieved; combining the advantages of low price of titanium sponge 5 raw material and low cost and small size restriction of arc additive manufacturing technology, compared with selective laser melting (SLM) and laser melt deposition (LDM), it has no specific requirements for materials and low material cost; compared with electron beam selective melting (SEBM), it only needs to be processed in a protective atmosphere that is easier to create, without the need for a vacuum environment, with low requirements for equipment and no restrictions on processing size; compared with traditional arc additive manufacturing (WAAM), it uses titanium sponge 5 as raw material, which further reduces the manufacturing cost, and is conducive to the large-scale and low-cost preparation of titanium alloy structural parts.

[0046] Among them, for the planned path:

[0047] Firstly, the SolidWorks 3D drawing software is used to establish a 3D model of the titanium alloy component to be manufactured, and the processing path is planned according to the constructed 3D model.

[0048] In S4, when forming the next deposition layer (the next deposition layer refers to the deposition layer formed above the already formed deposition layer):

[0049] In the optional scheme of this embodiment, it is more preferred that in S4, after a certain layer of deposition is completed, the welding gun 4 is extinguished, and after the deposition is cooled to no longer glow red, the next layer of titanium sponge 5 is re-laid on top. After a certain layer of deposition is completed, the welding gun 4 is extinguished first, and then the next layer of titanium sponge 5 is laid on top, which can ensure manufacturing safety and improve safety.

[0050] In the optional scheme of this embodiment, it is more preferred that after re-laying the next layer of titanium sponge 5, the welding gun 4 is raised to a specified height, and a protective atmosphere is re-created in the gas shield 7. The welding gun 4 moves according to the corresponding planned path to complete the formation of the deposition layer of this layer. When preparing the deposition layer of the next layer, the protective atmosphere in the gas shield 7 is re-created. The protective atmosphere can effectively isolate harmful gases such as oxygen and nitrogen in the air, reduce the reaction of these gases with the molten pool during welding, thereby avoiding the formation of pores and inclusions, and ensuring the forming effect of the deposition layer; it can stabilize the burning of the arc, make the arc more concentrated, and the energy more concentrated, which is conducive to the transition of the molten droplet and the formation of the molten pool, and improve the stability and consistency of the welding process.

[0051] Among them, the description of enclosure 3:

[0052] Specifically, the function of the enclosure 3 is to ensure that the titanium sponge 5 will not scatter around the titanium alloy substrate 2 during laying.

[0053] Among the optional solutions of this embodiment, it is more preferred that the enclosure 3 is made of stainless steel plate. The enclosure 3 made of stainless steel may cause certain substances in the surrounding environment to undergo chemical reactions and produce corrosive gases or liquids due to the high temperature and high energy generated by the electric arc. The stainless steel enclosure 3 can effectively prevent these corrosive substances from damaging the titanium alloy substrate 2 and the equipment; the stainless steel material has a high melting point and good thermal stability, and can maintain stable physical and chemical properties in a high temperature environment, and will not melt, deform or produce harmful substances due to high temperature.

[0054] Among them, the setting requirements of relevant process parameters in the deposition layer forming process are as follows:

[0055] Specifically, the titanium sponge 5 is selected from national standard 0A grade titanium sponge 5 with a particle size of 3 mm to 7 mm, wherein the purity of titanium is 99.8 wt %.

[0056] Specifically, the titanium alloy substrate 2 is a TC4 titanium alloy substrate.

[0057] Specifically, the arc type of the in-situ arc additive manufacturing equipment is a DC pulse arc, and the DC pulse frequency is 1.0Hz~1.4Hz, the peak current is 290A~340A, the base current is 55A~75A, and the peak duty cycle is 58%~65%.

[0058] Specifically, a tungsten electrode is provided at the bottom of the welding gun 4, and the vertical distance between the tungsten electrode and the corresponding layer of titanium sponge 5 is 8 mm to 10 mm; the moving speed of the welding gun 4 is 150 mm / min to 200 mm / min.

[0059] By selecting titanium sponge 5 with a particle size of 3 mm to 7 mm as the raw material, and coordinating the relevant process parameter settings of the arc additive manufacturing equipment, as well as the vertical distance setting between the tungsten electrode at the bottom of the welding gun 4 and the titanium sponge 5 and the moving speed setting of the welding gun 4, a titanium alloy component with a dense interior and no macroscopic defects such as collapse and cracks on the surface is formed.

[0060] Specifically, the protective atmosphere is preferably an argon atmosphere, the argon flow rate is 18L / min to 22L / min, and the purity is 99.99vol%. In a specific embodiment of the present invention, the method for forming the protective atmosphere is: using a closed gas protective cover 7 to completely surround the welding gun 4 and its scanning path range, there is a gap between the gas protective cover 7 and the workbench 1 or an outlet is provided on the gas protective cover 7, and then argon gas is introduced, and when the oxygen content in the gas protective cover 7 is less than 1%, the preparation of the parts is started.

[0061] In the optional scheme of this embodiment, it is more preferred that the welding torch 4 starts to work when the oxygen content in the gas shield 7 is less than 1%. In the environment where the oxygen content in the gas shield 7 is less than 1%, the contact between the molten pool metal and oxygen can be reduced, and the occurrence of oxidation reaction can be reduced; and the generation of pores can be reduced, and the density of the deposited layer can be improved; the low oxygen environment is conducive to stabilizing the combustion of the arc, reducing the fluctuation and splashing of the arc, and improving the deposition efficiency and forming accuracy.

[0062] Specifically, the height of the deposition layer formed by a single deposition is related to the particle size of the selected titanium sponge 5 and the heat input size of the welding gun 4. In the optional scheme of this embodiment, it is more preferred that the height of the deposition layer is 2mm to 2.5mm. The height of the deposition layer is set to 2mm to 2.5mm, which can maintain a faster forming speed and improve the overall manufacturing efficiency; and the shape and size of each deposition layer can be more accurately controlled; by reasonably controlling the height of each deposition layer, the overall internal density effect formed can be guaranteed.

[0063] Among them, regarding other related instructions:

[0064] Specifically, regarding the formation mechanism of the deposition process of the deposited layer, such as Figure 2 As shown, a layer of sponge titanium 5 raw material is laid on the titanium alloy substrate 2, the welding gun 4 peak value melts the sponge titanium 5, and the sponge titanium 12 directly below the arc is melted by the arc 13; the sponge titanium 11 on both sides of the arc begins to melt after being immersed in the molten pool, and is gradually attracted into the molten pool under the action of the molten pool tension; the base value maintains the molten state of the molten pool, and further absorbs the sponge titanium 5 below the arc 13 side.

[0065] Specifically, Figure 1 As shown, it is a schematic diagram of the manufacturing equipment used in the sponge titanium in-situ additive manufacturing method of the titanium alloy component of the present embodiment, wherein the welding gun 4 is connected to the welding machine 10, and the corresponding protective gas cylinder 9 is connected to the welding gun 4; the welding machine 10 and the welding gun 4 are both connected to the control system 8; the gas protection cover 7 is connected to the protective gas cylinder 9 for providing a protective atmosphere; a titanium alloy substrate 2 is placed on the workbench 1, and a fence 3 is provided around the titanium alloy substrate 2, and a semi-finished product 6 of the titanium alloy component is provided on the titanium alloy substrate 2.

[0066] Here, the three-dimensional model of a titanium alloy component is taken as an example with a length of 80 mm, a width of 80 mm, and a height of 70 mm:

[0067] The three-dimensional model of the titanium alloy component to be manufactured is established by using SolidWorks three-dimensional drawing software, and the processing path is planned according to the constructed three-dimensional model; the processing path program is compiled according to the three-dimensional model, and the code of the processing path program is imported into the control system 8. The code of the single-layer processing path is:

[0068] M05

[0069] G92 Y0 X0 Z0

[0070] G54

[0071] G91

[0072] M32 P1000

[0073] G04 P1000

[0074] M03

[0075] G01 Y-80F200

[0076] G01 X10

[0077] G01 Y80 F200

[0078] G01 X10

[0079] G01 Y-80F200

[0080] G01 X10

[0081] G01 Y80 F200

[0082] G01 X10

[0083] G01 Y-80F200

[0084] G01 X10

[0085] G01 Y80 F200

[0086] G01 X10

[0087] G01 Y-80F200

[0088] G01 X10

[0089] G01 Y80 F200

[0090] M05

[0091] G04 P1000

[0092] M33

[0093] A sufficient amount of titanium sponge 5 is prepared and evenly spread on the titanium alloy substrate 2. To ensure that the titanium sponge 5 does not scatter during laying, it is necessary to add a fence 3 around the substrate. The control system 8 controls the welding gun 4 to move along the above-planned path, and under the above-mentioned relevant process parameter settings, layer-by-layer molten deposition is achieved under a protective atmosphere to obtain a semi-finished product 6 of a titanium alloy component, and then through relevant post-processing (such as removing the unfused titanium sponge 5 particles attached to the surface of the semi-finished product 6) operations, the final titanium alloy component is obtained.

[0094] A total of 30 layers of molten deposition were completed above, including Figure 3 The semi-finished product 6 of the final square titanium alloy component is 100 mm long, 100 mm wide and 80 mm high. The semi-finished product 6 has a high quality, with unfused titanium sponge particles 5 attached to the surface, and no macroscopic defects such as collapse and cracks. Figure 4 As shown in the figure, it can be observed that its interior is dense and has a silvery white metallic luster; its internal metallographic structure is as follows Figure 5 shown.

[0095] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for in-situ additive manufacturing of titanium sponge for titanium alloy components, characterized in that: The following steps are involved: S1, placing a titanium alloy substrate on a workbench, setting up enclosures around the titanium alloy substrate, and evenly spreading a layer of titanium sponge on the titanium alloy substrate; S2, a gas protective cover is provided on the workbench, wherein the gas protective cover covers the titanium alloy substrate and the enclosure inside, and a protective atmosphere is created inside the gas protective cover; S3, setting a welding gun of the arc additive manufacturing equipment in the gas shield, the welding gun is located above the titanium sponge, and the welding gun moves according to a set planned path, and finally forms a deposition layer by melting and depositing the titanium sponge located on the planned path; S4, after the welding gun completes the deposition layer, a new layer of titanium sponge is continuously laid on the deposition layer as a basis; S5, repeating steps S3 to S4 until a semi-finished product of a titanium alloy component is formed; the semi-finished product is post-processed to form a final titanium alloy component.

2. The method for in-situ additive manufacturing of titanium sponge components of a titanium alloy component according to claim 1, characterized in that: The particle size of the titanium sponge is 3 mm to 7 mm; The arc type of the arc additive manufacturing equipment is a DC pulse arc, and the DC pulse frequency is 1.0 Hz to 1.4 Hz, the peak current is 290A to 340A, the base current is 55A to 75A, and the peak duty cycle is 58% to 65%; A tungsten electrode is provided at the bottom of the welding gun, and the vertical distance between the tungsten electrode and the titanium sponge laid on the corresponding layer is 8 mm to 10 mm; The moving speed of the welding gun is 150 mm / min to 200 mm / min.

3. The method for in-situ additive manufacturing of titanium sponge components of a titanium alloy component according to claim 2, characterized in that: The height of the deposited layer is 2 mm to 2.5 mm.

4. The method for in-situ additive manufacturing of titanium sponge components of a titanium alloy component according to claim 1, characterized in that: In S4, after a certain layer of the deposited layer is completed, the arc of the welding torch is extinguished, and after the deposited layer is cooled to no longer glow red, the next layer of the sponge titanium is laid on top.

5. The method for in-situ additive manufacturing of titanium sponge for titanium alloy components according to claim 4, characterized in that: After re-laying the next layer of the titanium sponge, the welding gun is raised to a specified height, the protective atmosphere is re-created in the gas shield, and the welding gun moves along a corresponding planned path to complete the formation of the deposition layer of this layer.

6. The method for in-situ additive manufacturing of titanium sponge components of a titanium alloy component according to claim 1, characterized in that: When the oxygen content in the gas protective cover is less than 1%, the welding gun starts to work.

7. The method for in-situ additive manufacturing of titanium sponge components of a titanium alloy component according to claim 1, characterized in that: The enclosure is made of stainless steel plate.