Method for hydro-thermal synthesis of lithium iron phosphate from pyrite cinder
Through hydrothermal synthesis and load treatment technology, the problem of poor performance and pollution in preparing lithium iron phosphate from pyrite slag was solved, high-performance lithium iron phosphate powder was prepared, and the economic value of pyrite slag was maximized and environmentally friendly production was achieved. .
Patent Information
- Application Number
- CN202410879332.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-18
AI Technical Summary
In the existing technology, the process performance of using pyrite slag to prepare lithium iron phosphate is poor, and the calcination process consumes a lot of energy and produces polluting gases. It is difficult to control the crystal form and particle size, and the economic value of pyrite slag cannot be realized. maximize.
The hydrothermal synthesis method is adopted, heating acid leaching with sulfuric acid, adding H3PO4 and sodium hydroxide to adjust the pH, combining with lithium hydroxide for hydrothermal reaction, and performing low-temperature spray drying, and finally through surface oxidation, silver-carbon loading and ball milling shaping. Steps to prepare high-performance lithium iron phosphate powder.
It achieves the high-performance preparation of lithium iron phosphate, controls the crystal form and particle size, avoids pollution during the calcination process, improves the conductivity and volume energy density of the material, and realizes the high-value utilization of pyrite slag.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new materials, and more specifically, the present invention relates to a method for hydrothermally synthesizing lithium iron phosphate from pyrite slag. Background Art
[0002] Pyrite cinder is also called pyrite baking slag or cinder. At present, sulfuric acid is produced from pyrite in China. In the process of roasting pyrite to prepare raw gas, a large amount of slag and ash are discharged, which is the main solid waste discharged by my country's sulfuric acid industry. my country discharges more than 3 million tons of pyrite cinder every year, and only more than 1 million tons are actually used reasonably.
[0003] In fact, pyrite cinders have been used as raw materials for iron smelting for more than 100 years. At present, there are four main methods for treating pyrite cinders in China. (1) Direct utilization of pyrite cinders, such as using it as a building material or cement mineralizer, is suitable for treating pyrite cinders with an iron content of less than 35%. The process of direct blending for iron smelting generally requires that the iron content of pyrite cinders be greater than 55%. Most of the pyrite cinders in my country have an iron content between 35% and 55%, and need to be treated before they can be directly used in iron smelting production. (2) Chlorination volatilization and chlorination roasting require that the pyrite cinders have a high iron content and contain more non-ferrous metals, which are not suitable for the basic conditions of pyrite cinders in my country and are difficult to apply directly. (3) The method of preparing inorganic pigments, water purifiers and other chemical products from pyrite cinders is generally simple in process, easy to realize industrial production, and has achieved good results. However, this method generally cannot effectively recover non-ferrous metals in pyrite cinders, and the leached slag still needs to be treated; at the same time, the production scale is small, and it cannot completely solve the problem of pyrite cinder treatment. (4) Ore dressing methods generally have poor effects and it is difficult to improve the iron grade. Among the ore dressing methods, only the magnetic roasting-magnetic separation method can effectively improve the iron grade of pyrite slag.
[0004] The pyrite slag from sulfuric acid plants has a high iron content and a low impurity content. Lithium iron phosphate batteries have good rate performance, long service life, and good thermal stability. They occupy a major share in the power battery market. With the popularization of electric vehicles, the price of lithium iron phosphate has skyrocketed. In view of the current situation, preparing lithium iron phosphate with pyrite slag is one of the means to treat pyrite slag and effectively recover the iron element in it. However, in the prior art, the performance of lithium iron phosphate products prepared with pyrite slag is poor.
[0005] Generally speaking, the greater the tap density, the higher the battery capacity can be, so the tap density is also regarded as one of the reference indicators of material energy density. Under certain process conditions, the greater the tap density, the higher the battery capacity. Especially at the peak of the rise of new energy vehicles today, if lithium iron phosphate is to be widely used in new energy electric vehicles and hybrid electric vehicles, the tap density of lithium iron manganese phosphate must be further improved to meet market requirements. At present, the tap density of lithium iron phosphate in the industry is generally 0.8g / cm 3 ~1.2g / cm 3 .
[0006] Chinese patent CN103746115A provides a method for preparing battery-grade lithium iron phosphate using pyrite slag. The method uses reduction roasting to increase the leaching rate of iron elements, and then the leaching solution is decontaminated and hydrothermally synthesized into lithium iron phosphate. This method not only consumes a large amount of energy when calcining the pyrite slag, but also may produce polluting gases.
[0007] The present invention provides a method for preparing battery-grade lithium iron phosphate with excellent performance by using pyrite slag. The method does not involve calcination in the production process and does not generate polluting gases. In addition, the method is easy to control the crystal form and particle size, has a uniform phase, a small powder particle size, and a simple process, and can maximize the economic value of the pyrite slag. Summary of the invention
[0008] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0009] In order to achieve these purposes and other advantages according to the present invention, a method for hydrothermally synthesizing lithium iron phosphate from pyrite slag is provided, comprising:
[0010] Step 1, heating the pyrite slag with sulfuric acid for acid leaching, and performing solid-liquid separation on the leached slurry to obtain a filtrate and a filter residue;
[0011] Step 2: Add H3PO4 solution to the filtrate obtained in step 1, stir, and adjust the pH with sodium hydroxide solution to obtain a mixed solution;
[0012] Step 3, adding lithium hydroxide to the mixed solution in proportion, stirring, and adjusting the pH with sodium hydroxide solution to obtain a mixture;
[0013] Step 4: Transfer the mixture obtained in step 3 to a hydrothermal reaction kettle, perform hydrothermal reaction for a period of time, and then perform low-temperature spray drying to obtain lithium iron phosphate powder.
[0014] Preferably, in step 1, the particle size of the pyrite cinder should be controlled at 0.1 to 500 mm, the concentration of sulfuric acid is 0.1 mol / L to 13 mol / L, and the molar ratio of sulfuric acid to iron in the pyrite cinder is 1.2 to 1.8:1.
[0015] Preferably, in step 1, the acid leaching time is 10 h to 24 h, and the heating temperature is 30° C. to 130° C.
[0016] Preferably, in step 2, the molar ratio of the iron element in the filtrate to the added phosphoric acid is 1:1.2-1.8, and the H3PO4 solution is an H3PO4 solution with a mass fraction of ≥85%.
[0017] Preferably, in step 2, the concentration of the sodium hydroxide solution is 0.5 to 5 mol / L, and the pH is adjusted to 1.6 to 2.0.
[0018] Preferably, in the step three, lithium hydroxide is added in a molar ratio of iron element to lithium hydroxide in the mixed solution of 1:3.2 to 3.8.
[0019] Preferably, in step three, the concentration of the sodium hydroxide solution is 1 to 5 mol / L, and the pH is adjusted to 1.6 to 2.2.
[0020] Preferably, in step 2 and step 3, the stirring time is 10 to 60 minutes.
[0021] Preferably, in step 4, the hydrothermal reaction temperature is 110°C to 140°C, the hydrothermal reaction time is 5 to 8 hours, and the low-temperature spray drying temperature is 40°C to 70°C.
[0022] In order to improve the conductivity and volume energy density of lithium iron phosphate powder, in step 4, the lithium iron phosphate powder is post-processed by:
[0023] S1. Place lithium iron phosphate powder in a heating furnace in an oxygen-rich atmosphere for surface oxidation. The heating furnace temperature is set at 160-200° C. and heated for 2-4 hours.
[0024] S2, putting the surface oxidized lithium iron phosphate powder in S1 into a tube furnace, first introducing a protective gas, then heating to 550-580° C., then introducing a reaction gas, and keeping the temperature for 7-9 hours. After the reaction is completed, introducing a protective gas again and cooling naturally to room temperature to obtain a surface carbon-loaded lithium iron phosphate powder;
[0025] S3. Add the carbon-loaded lithium iron phosphate powder obtained in S2 to the silver-ammonia solution, stir evenly, then add the reducing sugar solution thereto, heat in a water bath with stirring, filter, and obtain the silver-carbon-loaded lithium iron phosphate powder.
[0026] S4, putting the silver-carbon-loaded lithium iron phosphate powder obtained in S3 into a ball mill for ball milling and shaping, the grinding medium is zirconia grinding beads with a diameter of 20 to 30 mm, the ball-to-material mass ratio is 1:5 to 7, grinding for 4 to 12 hours, and the grinding speed is 300 to 400 rpm;
[0027] S5. Ultrasonic dispersion of the ground silver-carbon-loaded lithium iron phosphate powder in water at a frequency of 40 to 60 kHz for 2 to 4 hours. After the ultrasonic dispersion, the solution is subjected to secondary low-temperature spray granulation at a temperature of 40° C. to 70° C. to finally obtain silver-carbon-loaded lithium iron phosphate nanopowder.
[0028] Preferably, in S2, the protective gas is at least one of helium and argon, and the reaction gas is at least one of carbon monoxide, ethylene, propylene and butene.
[0029] Preferably, in S2, the molar ratio of lithium iron phosphate powder to reaction gas is 1:1-4;
[0030] Preferably, in S3, the concentration of the silver ammonia solution is 0.2-0.5 mol / L, the reducing sugar solution is a glucose solution with a concentration of 0.2-0.5 mol / L, the volume ratio of the silver ammonia solution to the reducing sugar solution is 1:2-4, and the water bath heating temperature is 40-70°C.
[0031] The present invention has at least the following beneficial effects:
[0032] (1) The preparation method of the present invention can easily control the crystal form and particle size of lithium iron phosphate, and the phase is uniform and the powder particle size is small.
[0033] (2) The lithium iron phosphate preparation method provided by the present invention ingeniously uses phosphate to precipitate trivalent iron under the condition of 1.6-2.0 pH, while avoiding the precipitation of copper, aluminum, magnesium and zinc, thereby achieving the purpose of impurity removal.
[0034] (3) The present invention effectively improves the conductivity of lithium iron phosphate by loading lithium iron phosphate with carbon-silver on its surface, and simultaneously performs ball milling and spray granulation on the lithium iron phosphate to obtain carbon-silver loaded lithium iron phosphate nanopowder with strong conductivity and high tap density, thereby improving the volume energy density of the lithium iron phosphate material.
[0035] (4) The preparation method provided by the present invention converts pyrite slag into high-value and high-performance lithium iron phosphate, thereby realizing its economic value. The preparation method is simple and easy to industrialize.
[0036] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION
[0037] The present invention is described in further detail below so that those skilled in the art can implement it according to the description.
[0038] It should be understood that terms such as “having”, “including” and “comprising” used herein do not specify the existence or addition of one or more other elements or combinations thereof.
[0039] Example 1
[0040] A method for hydrothermally synthesizing lithium iron phosphate from pyrite slag comprises the following steps:
[0041] Step 1, soak the pyrite slag with a particle size of less than 1 mm (main components are Fe2O3: 83.39%, MgO: 3.36%, SiO2: 2.68%, S: 1.6%, Al2O3: 1.4%, Zn: 0.91%, Cu: 0.27%, other impurities content is 6.39%, and the single impurity component is less than 0.05%) in 7 mol / L sulfuric acid and heat to 70 ° C, stir for 1 hour, the molar ratio of iron element to sulfuric acid is 1:1.4, and the leached slurry is solid-liquid separated to obtain filtrate and filter residue;
[0042] Step 2: Add 85 wt% H3PO4 solution to the filtrate obtained in step 1 at a molar ratio of trivalent iron to H3PO4 of 1:1.4, stir for 10 min, and adjust the pH to 1.9 with 1 mol / L sodium hydroxide solution to obtain a mixed solution;
[0043] Step 3, adding lithium hydroxide to the mixed solution obtained in step 2 at a molar ratio of trivalent iron to lithium hydroxide of 1:3.5, stirring for 10 minutes, and adjusting the pH to 2.0 with 1 mol / L sodium hydroxide solution to obtain a mixture;
[0044] Step 4: Transfer the mixture obtained in step 3 to a hydrothermal reactor, perform hydrothermal reaction at 120° C. for 7 hours, and perform low-temperature spray drying after the reaction. The low-temperature spray drying temperature is 60° C. to obtain lithium iron phosphate powder.
[0045] The primary particle size of the lithium iron phosphate powder was 200 nm and the tap density was 1.01 g / cm 3 .
[0046] Example 2
[0047] A method for hydrothermally synthesizing lithium iron phosphate from pyrite slag comprises the following steps:
[0048] Step 1, soak the pyrite slag with a particle size of less than 1 mm (main components are Fe2O3: 83.39%, MgO: 3.36%, SiO2: 2.68%, S: 1.6%, Al2O3: 1.4%, Zn: 0.91%, Cu: 0.27%, other impurities content is 6.39%, and the single impurity component is less than 0.05%) in 7 mol / L sulfuric acid and heat to 70 ° C, stir for 1 hour, the molar ratio of iron element to sulfuric acid is 1:1.2, and the leached slurry is solid-liquid separated to obtain filtrate and filter residue;
[0049] Step 2: Add 85 wt% H3PO4 solution to the filtrate obtained in step 1 at a molar ratio of trivalent iron to H3PO4 of 1:1.2, stir for 10 min, and adjust the pH to 1.8 with 1 mol / L sodium hydroxide solution to obtain a mixed solution;
[0050] Step 3, adding lithium hydroxide to the mixed solution obtained in step 2 at a molar ratio of trivalent iron to lithium hydroxide of 1:3.2, stirring for 10 minutes, and adjusting the pH to 2.0 with a 1 mol / L sodium hydroxide solution to obtain a mixture;
[0051] Step 4: Transfer the mixture obtained in step 3 to a hydrothermal reactor, perform hydrothermal reaction at 120° C. for 5 hours, and perform low-temperature spray drying after the reaction. The low-temperature spray drying temperature is 50° C. to obtain lithium iron phosphate powder.
[0052] The primary particle size of lithium iron phosphate powder was 150nm and the tap density was 1.05g / cm 3 .
[0053] Example 3
[0054] A method for hydrothermally synthesizing lithium iron phosphate from pyrite slag comprises the following steps:
[0055] Step 1, heat the pyrite slag with a particle size of less than 1 mm (main components are Fe2O3: 83.39%, MgO: 3.36%, SiO2: 2.68%, S: 1.6%, Al2O3: 1.4%, Zn: 0.91%, Cu: 0.27%, other impurities content is 6.39%, and the single impurity component is less than 0.05%) in 7 mol / L sulfuric acid to 70 ° C, stir for 1 hour, the molar ratio of iron element to sulfuric acid is 1:1.3, and the leached slurry is solid-liquid separated to obtain a filtrate and a filter residue;
[0056] Step 2: Add 85 wt% H3PO4 solution to the filtrate obtained in step 1 at a molar ratio of trivalent iron to H3PO4 of 1:1.3, stir for 10 min, and adjust the pH to 1.8 with 1 mol / L sodium hydroxide solution to obtain a mixed solution;
[0057] Step 3, adding lithium hydroxide to the mixed solution obtained in step 2 at a molar ratio of trivalent iron to lithium hydroxide of 1:3.3, stirring for 10 minutes, and adjusting the pH to 2.0 with 1 mol / L sodium hydroxide solution to obtain a mixture;
[0058] Step 4: Transfer the mixture obtained in step 3 to a hydrothermal reactor, perform hydrothermal reaction at 130° C. for 5 hours, and perform low-temperature spray drying after the reaction. The low-temperature spray drying temperature is 50° C. to obtain lithium iron phosphate powder.
[0059] The primary particle size of lithium iron phosphate powder was 100 nm and the tap density was 1.09 g / cm 3 .
[0060] Example 4
[0061] The difference between this embodiment and embodiment 1 is that in step 4, the lithium iron phosphate powder is post-treated by:
[0062] S1. Place 500 g of lithium iron phosphate powder in a heating furnace in an oxygen-rich atmosphere for surface oxidation. The heating furnace temperature is set at 160° C. and heated for 2 h.
[0063] S2, putting the surface oxidized lithium iron phosphate powder in S1 into a tube furnace, first introducing helium, then heating to 550° C., then introducing propylene and carbon monoxide, and keeping the temperature for reaction for 9 hours. After the reaction is completed, introducing protective gas and naturally cooling to room temperature to obtain surface carbon-loaded lithium iron phosphate powder, wherein the volume ratio of propylene to carbon monoxide is 1:1, and the molar ratio of lithium iron phosphate powder to propylene and carbon monoxide is 1:2:2;
[0064] S3. Add the carbon-loaded lithium iron phosphate powder obtained in S2 to 1L of 0.5mol / L silver ammonia solution, stir evenly, then add 0.5L of 0.5mol / L glucose solution, heat to 45°C in a water bath, stir, and filter to obtain silver-carbon-loaded lithium iron phosphate powder.
[0065] S4, the silver-carbon-loaded lithium iron phosphate powder obtained in S3 is placed in a ball mill for ball milling and shaping, the grinding medium is zirconia grinding beads with a diameter of 25 mm, the ball-to-material mass ratio is 1:5, and the grinding is performed for 6 hours;
[0066] S5. Ultrasonic dispersion of the ground lithium iron phosphate powder in water at a frequency of 45 kHz for 2 hours. After the ultrasonic dispersion, the solution is subjected to secondary low-temperature spray granulation at a temperature of 50° C. to finally obtain silver-carbon-loaded lithium iron phosphate nanopowder.
[0067] The primary particle size of the silver-carbon-loaded lithium iron phosphate nanopowder was 64 nm and the tap density was 1.30 g / cm3 The electrical properties of silver-carbon-loaded lithium iron phosphate nanopowder were tested using a solid conductivity tester, and its resistivity was measured to be 2.65×10 7 Ω·cm.
[0068] Example 5
[0069] The difference between this embodiment and embodiment 2 is that in step 4, the lithium iron phosphate powder is post-treated by:
[0070] S1. Place 500 g of lithium iron phosphate powder in a heating furnace in an oxygen-rich atmosphere for surface oxidation. The heating furnace temperature is set at 160° C. and heated for 2 h.
[0071] S2, putting the surface oxidized lithium iron phosphate powder in S1 into a tube furnace, first introducing helium, then heating to 550° C., then introducing propylene and carbon monoxide, and keeping the temperature for reaction for 9 hours. After the reaction is completed, introducing protective gas and naturally cooling to room temperature to obtain surface carbon-loaded lithium iron phosphate powder, wherein the volume ratio of propylene to carbon monoxide is 1:1, and the molar ratio of lithium iron phosphate powder to propylene and carbon monoxide is 1:2:2;
[0072] S3. Add the carbon-loaded lithium iron phosphate powder obtained in S2 to 1L of 0.5mol / L silver ammonia solution, stir evenly, then add 0.5L of 0.5mol / L glucose solution, heat to 45°C in a water bath, stir, and filter to obtain silver-carbon-loaded lithium iron phosphate powder.
[0073] S4, the silver-carbon loaded lithium iron phosphate powder obtained in S3 is placed in a ball mill for ball milling and shaping, the grinding medium is zirconia grinding beads with a diameter of 20 mm, the ball-to-material mass ratio is 1:5, and the grinding is performed for 8 hours;
[0074] S5. Ultrasonic dispersion of the ground silver-carbon-loaded lithium iron phosphate powder in water at a frequency of 50 kHz for 2 hours. After the ultrasonic dispersion, the solution is subjected to secondary low-temperature spray granulation at a temperature of 50° C. to finally obtain silver-carbon-loaded lithium iron phosphate nanopowder.
[0075] The primary particle size of the silver-carbon-loaded lithium iron phosphate nanopowder was 57 nm and the tap density was 1.32 g / cm 3 The electrical properties of silver-carbon-loaded lithium iron phosphate nanopowder were tested using a solid conductivity tester, and its resistivity was measured to be 2.48×10 7 Ω·cm.
[0076] Example 6
[0077] The difference between this embodiment and embodiment 3 is that in step 4, the lithium iron phosphate powder is post-treated by:
[0078] S1. Place 500 g of lithium iron phosphate powder in a heating furnace in an oxygen-rich atmosphere for surface oxidation. The heating furnace temperature is set at 160° C. and heated for 2 h.
[0079] S2, putting the surface oxidized lithium iron phosphate powder in S1 into a tube furnace, first introducing helium, then heating to 550° C., then introducing propylene and carbon monoxide, and keeping the temperature for reaction for 9 hours. After the reaction is completed, introducing protective gas and naturally cooling to room temperature to obtain surface carbon-loaded lithium iron phosphate powder, wherein the volume ratio of propylene to carbon monoxide is 1:1, and the molar ratio of lithium iron phosphate powder to propylene and carbon monoxide is 1:2:2;
[0080] S3. Add the carbon-loaded lithium iron phosphate powder obtained in S2 to 1L of 0.5mol / L silver ammonia solution, stir evenly, then add 0.5L of 0.5mol / L glucose solution, heat to 45°C in a water bath, stir, and filter to obtain silver-carbon-loaded lithium iron phosphate powder.
[0081] S4, the silver-carbon-loaded lithium iron phosphate powder obtained in S3 is placed in a ball mill for ball milling and shaping, the grinding medium is zirconia grinding beads with a diameter of 20 mm, the ball-to-material mass ratio is 1:6, and the grinding is carried out for 12 hours;
[0082] S5. Ultrasonic dispersion of the ground silver-carbon-loaded lithium iron phosphate powder in water at a frequency of 60 kHz for 2 hours. After the ultrasonic dispersion, the solution is subjected to secondary low-temperature spray granulation at a temperature of 50° C. to finally obtain carbon-loaded lithium iron phosphate nanopowder.
[0083] The primary particle size of the silver-carbon-loaded lithium iron phosphate nanopowder was 52 nm and the tap density was 1.33 g / cm 3 The electrical properties of silver-carbon-loaded lithium iron phosphate nanopowder were tested using a solid conductivity tester, and its resistivity was measured to be 2.33×10 7 Ω·cm.
[0084] Comparative Example 1
[0085] The difference between this comparative example and Example 4 is that after the lithium iron phosphate powder is loaded with silver-carbon, the lithium iron phosphate powder is not ground, but is directly ultrasonically dispersed and then subjected to secondary spray granulation.
[0086] The primary particle size of the silver-carbon loaded lithium iron phosphate powder was 108 nm and the tap density was 1.03 g / cm 3 The electrical properties of the silver-carbon-loaded lithium iron phosphate powder were tested using a solid conductivity tester, and its resistivity was measured to be 2.79×10 7 Ω·cm.
[0087] Comparative Example 2
[0088] The difference between this comparative example and Example 4 is that after the lithium iron phosphate powder is loaded with silver-carbon and ground, the lithium iron phosphate powder is not subjected to ultrasonic dispersion and secondary spray granulation.
[0089] The primary particle size of the silver-carbon-loaded lithium iron phosphate powder was 94 nm and the tap density was 1.10 g / cm 3 The electrical properties of the silver-carbon-loaded lithium iron phosphate powder were tested using a solid conductivity tester, and its resistivity was measured to be 2.68×10 7 Ω·cm.
[0090] Comparative Example 3
[0091] The difference between this comparative example and Example 4 is that the lithium iron phosphate powder is not loaded with silver-carbon, but is directly ground and then ultrasonically dispersed and spray granulated twice.
[0092] The primary particle size of lithium iron phosphate powder was 60nm and the tap density was 1.33g / cm 3 The electrical properties of lithium iron phosphate powder were tested using a solid conductivity tester, and its resistivity was measured to be 6.64×10 7 Ω·cm.
[0093] Comparative Example 4
[0094] The difference between this comparative example and Example 4 is that only carbon loading but no silver loading is performed on the lithium iron phosphate powder, and the other aspects are consistent with Example 4.
[0095] The primary particle size of the carbon-supported lithium iron phosphate powder was 62 nm and the tap density was 1.32 g / cm 3 The electrical properties of carbon-supported lithium iron phosphate powder were tested using a solid conductivity tester, and its resistivity was measured to be 5.21×10 7 Ω·cm.
[0096] Comparative Example 5
[0097] The difference between this comparative example and Example 4 is that only silver loading but no carbon loading is performed on the lithium iron phosphate powder, and the other aspects are consistent with Example 4.
[0098] The primary particle size of the silver-loaded lithium iron phosphate powder was 61 nm and the tap density was 1.31 g / cm 3 The electrical properties of the silver-loaded lithium iron phosphate powder were tested using a solid conductivity tester, and its resistivity was measured to be 3.14×10 7 Ω·cm.
[0099] It can be seen from the test results of Examples 1 to 6 and Comparative Examples 1 to 5 that the lithium iron phosphate powder prepared by the present invention has uniform phase, small powder particle size, and high tap density, which helps to improve the volume energy density of the lithium iron phosphate material. The silver-carbon loaded lithium iron phosphate nanopowder prepared by silver-carbon loading and grinding and secondary spray granulation has a smaller particle size, a higher tap density and a low resistivity, indicating that it has higher conductivity.
[0100] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for hydrothermally synthesizing lithium iron phosphate from pyrite slag, characterized in that: The following steps are involved: Step 1, heating the pyrite slag with sulfuric acid for acid leaching, and performing solid-liquid separation on the leached slurry to obtain a filtrate and a filter residue; Step 2: Add H3PO4 solution to the filtrate obtained in step 1, stir, and adjust the pH with sodium hydroxide solution to obtain a mixed solution; Step 3, adding lithium hydroxide to the mixed solution in proportion, stirring, and adjusting the pH with sodium hydroxide solution to obtain a mixture; Step 4: Transfer the mixture obtained in step 3 to a hydrothermal reactor, perform hydrothermal reaction for a period of time, and then perform low-temperature spray drying to obtain lithium iron phosphate powder.
2. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 1, the particle size of the pyrite cinder should be controlled at 0.1 to 500 mm, the concentration of sulfuric acid is 0.1 mol / L to 13 mol / L, and the molar ratio of sulfuric acid to the iron element in the pyrite cinder is 1.2 to 1.8:
1.
3. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 1, the acid leaching time is 10 hours to 24 hours, and the heating temperature is 30° C. to 130° C.
4. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 2, the molar ratio of the iron element in the filtrate to the added phosphoric acid is 1:1.2-1.8, and the H3PO4 solution is an H3PO4 solution with a mass fraction of ≥85%.
5. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 2, the concentration of the sodium hydroxide solution is 0.5-5 mol / L, and the pH is adjusted to 1.6-2.
0.
6. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 3, lithium hydroxide is added according to the molar ratio of iron element to lithium hydroxide in the mixed solution of 1:3.2-3.
8.
7. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 3, the concentration of the sodium hydroxide solution is 1-5 mol / L, and the pH is adjusted to 1.6-2.
2.
8. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 2 and the step 3, the stirring time is 10 to 60 minutes.
9. The method for hydrothermal synthesis of lithium iron phosphate from pyrite slag according to claim 1, characterized in that: In the step 4, the hydrothermal reaction temperature is 110°C to 140°C, the hydrothermal reaction time is 5 to 8 hours, and the low-temperature spray drying temperature is 40°C to 70°C.
Citation Information
Patent Citations
Integrated high-rate lithium iron phosphate positive electrode material and preparation method and application thereof
CN112038629A
Method for preparing iron phosphate from sulfuric-acid residues
CN116161635A
Method for preparing battery-grade lithium iron phosphate from pyrite cinder
CN116177515A
Preparation method for iron phosphate and preparation method for lithium iron phosphate
WO2023185056A1