High-entropy oxide ceramic capable of improving crack resistance and preparation method of high-entropy oxide ceramic

By using components such as nanosilica sol and binders in high-entropy oxide ceramics, combined with 3D direct writing printing technology, the crack problem during the sintering process is solved, the strength and toughness of the ceramics are improved, and the crack resistance performance is significantly improved.

CN118791285AInactive Publication Date: 2024-10-18GUILIN UNIV OF ELECTRONIC TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410925663.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the sintering process of existing high-entropy oxide ceramics, uneven thermal stress caused by differences in thermal expansion coefficients and sintering rates leads to the formation of cracks within the material, reducing its strength and toughness, and affecting electrical and optical properties.

Method used

High-entropy oxide ceramics are prepared through 3D direct writing printing technology using components such as nano-silica sol, binder and dispersant. The nano-silica sol is tightly distributed in the ceramic matrix as a bridge to connect the components, and the binder and dispersant enhance The cohesion of ceramics reduces the occurrence of cracks.

Benefits of technology

It improves the strength and toughness of ceramics, reduces the occurrence of micro-cracks, significantly improves crack resistance, and enhances the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004938055810000011
    Figure BDA0004938055810000011
  • Figure FDA0004938055780000011
    Figure FDA0004938055780000011
Patent Text Reader

Abstract

The embodiment of the invention discloses high-entropy oxide ceramic with improved crack resistance and a preparation method of the high-entropy oxide ceramic. The high-entropy oxide ceramic comprises the following components: oxide ceramic powder, nano silica sol, a binder, a dispersing agent and a solvent. The nano-silica sol has the advantages of uniform particles, no toxicity, no pollution, large specific surface area, high reaction activity, high adsorption capacity, high bonding performance and the like, and the application finds that the nano-silica sol is applied to the high-entropy oxide ceramic, can be closely distributed in a ceramic matrix and can be well combined with other components, so that the high-entropy oxide ceramic can be prepared. The stability of the overall structure of the high-entropy oxide ceramic is enhanced, the generation of microcracks is reduced, and the crack resistance is improved; in the preparation process of the high-entropy oxide ceramic, slurry is prepared through mixing and stirring, then the slurry is formed by using a 3D direct-writing printing technology, and finally the high-entropy oxide ceramic with excellent crack resistance is obtained through the steps of drying, degreasing, sintering and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of high entropy ceramics, and in particular to a high entropy oxide ceramic with improved crack resistance and a preparation method thereof. Background Art

[0002] With the continuous development of materials science, high entropy ceramics, as an emerging type of material, have received extensive attention. Among them, high entropy oxide ceramics, as a type of high entropy ceramics, show a significant high entropy effect due to its unique single crystal structure formed by more than three metal elements and a non-metallic element, which shows broad application prospects in the fields of mechanics, electricity and optics.

[0003] During the sintering process of existing high-entropy oxide ceramic materials, due to the differences in thermal expansion coefficients and sintering rates of various metal oxides, uneven thermal stress will be generated inside the material as the temperature rises. When this thermal stress exceeds the material's tolerance limit, cracks will form inside the material. The above cracks will not only reduce the material's strength and toughness, but also affect its electrical and optical properties, greatly reducing the performance of the high-entropy oxide ceramic material.

[0004] Application Contents

[0005] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a high entropy oxide ceramic with improved crack resistance.

[0006] The high entropy oxide ceramic comprises the following components calculated by weight:

[0007]

[0008] To be more specific, in the above technical scheme, the preparation method of the nano silica sol includes: dissolving silica ash in a sodium hydroxide solution, stirring and heating to 70-80°C, keeping warm for 20-30 minutes, filtering out unreacted silica ash, neutralizing the obtained sodium silicate solution with sulfuric acid to pH = 8-8.5, removing the sodium sulfate generated by the reaction to obtain silica sol, adding the precipitate formed by the silica sol with a sodium hydroxide solution, and then obtaining the nano silica sol after ultrasonic treatment.

[0009] More specifically, in the above technical solution, the high entropy oxide ceramic further includes 2-4 parts of fluorocarbon surfactant by weight.

[0010] To be more specific, in the above technical scheme, the oxide ceramic powder includes any five or more of TiO2, Ta2O5, Al2O3, Fe2O3, Ga2O3, CuO, MgO, ZnO, NiOCaO, CoO, CeO2, Gd2O3, SnO2, La2O3, Er2O3, Y2O3, Co3O4 and CaCO3.

[0011] More specifically, in the above technical solution, the binder includes at least one of polyvinyl alcohol, polydimethylsiloxane alcohol and methyl cellulose.

[0012] More specifically, in the above technical solution, the dispersant includes at least one of BYK-153, sodium hexametaphosphate, polyethyleneimine and polyaspartic acid.

[0013] More specifically, in the above technical solution, the solvent includes at least one of water, ethanol, propanol, glycerol and acetic acid, and the solvent must contain water.

[0014] More specifically, in the above technical solution, the high entropy oxide ceramic further includes 3-4 parts of lubricant and / or 10-17 parts of reinforcing agent, calculated by weight.

[0015] More specifically, in the above technical solution, the lubricant includes one or more of silicone oil, polyvinyl pyrrolidone and polytetrafluoroethylene;

[0016] The reinforcing agent includes one or more of quartz powder, corundum powder, feldspar powder, biotite powder and kaolinite powder.

[0017] The present application also proposes a method for preparing a high entropy oxide ceramic, comprising mixing and stirring the raw material components of the high entropy oxide ceramic described in any one of the above items in proportion to obtain a high entropy oxide ceramic slurry;

[0018] Printing the high entropy oxide ceramic slurry into a high entropy oxide ceramic slurry green body by 3D direct writing printing technology;

[0019] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic.

[0020] Compared with the prior art, this application has at least the following beneficial effects:

[0021] The present application found that nano-silica sol itself has good bonding properties. When nano-silica sol is applied to high-entropy oxide ceramics, it can be tightly distributed in the ceramic matrix, acting as a bridge, tightly connecting the various components such as oxide ceramic powder, binder and dispersant together, and combining well with other components, thereby enhancing the cohesion of the ceramic matrix, improving the strength and toughness of the ceramic, reducing the generation of microcracks and improving crack resistance. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0024] The phrase "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, but means "one or more but not all embodiments", unless otherwise specifically emphasized. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized.

[0025] The present application proposes a high entropy oxide ceramic with improved crack resistance.

[0026] The high entropy oxide ceramic comprises the following components, calculated by weight: 50-75 parts of oxide ceramic powder, 7-10 parts of nano silica sol, 2-5 parts of binder, 5-6 parts of dispersant, and 6-8 parts of solvent.

[0027] As the main component of ceramics, the selection of oxide ceramic powder not only provides the basic structure and strength of the ceramics, but also forms a more complex and stable crystal structure through the synergistic effect of multiple components such as nano-silica sol, binder and dispersant, thereby reducing the generation and expansion of cracks.

[0028] Nano-silica sol itself has good bonding properties. When applied to high-entropy oxide ceramics, it can be tightly distributed in the ceramic matrix, acting as a bridge, tightly connecting the various components together, and combining well with other components, thereby enhancing the cohesion of the ceramic matrix, improving the strength and toughness of the ceramic, reducing the generation of microcracks and improving crack resistance.

[0029] An appropriate amount of binder can ensure that the ceramic powder maintains good adhesion during the preparation process, helps to form a dense ceramic body, and improves the strength and durability of the material; the addition of dispersant helps to evenly disperse the various components in the solvent and prevent particle agglomeration, thereby ensuring the uniformity and consistency of the ceramic material; the solvent can fully mix the components.

[0030] Specifically, during the slurry preparation process, the binder binds solid particles such as oxide ceramic powder and nano-silica sol together to form a slurry with a certain fluidity. The addition of the dispersant enables the solid particles to be evenly dispersed in the solvent, preventing particle agglomeration and ensuring the stability and uniformity of the slurry.

[0031] During the sintering process, as the solvent evaporates and the temperature rises, the ceramic body gradually densifies and forms the final high-entropy oxide ceramic material. In this process, the reinforcing effect of nano-silica sol, the bonding effect of the binder, and the dispersing effect of the dispersant jointly enhance the cohesion of the ceramic matrix, improve the strength and toughness of the ceramic, reduce the generation of microcracks, and improve the crack resistance.

[0032] In the present application, there is no particular limitation on the specific sources of oxide ceramic powder, nano-silica sol, binder, dispersant, and solvent. The above components can be purchased from the market or extracted or prepared by conventional methods known in the art.

[0033] In the present application, the amount of each component in the high entropy oxide ceramic can be adjusted according to the above definition, for example:

[0034] The ceramic powder can be 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, etc.;

[0035] Nano silica sol can be 7 parts, 8 parts, 9 parts, 10 parts, etc.;

[0036] The binder can be 2 parts, 3 parts, 4 parts, 5 parts, etc.;

[0037] The dispersant can be 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6 parts, etc.;

[0038] The solvent can be 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, etc.

[0039] In one embodiment, the preparation method of the nano silica sol includes: dissolving silica ash in a sodium hydroxide solution, stirring and heating to 70-80°C, keeping warm for 20-30 minutes, filtering out unreacted silica ash, neutralizing the obtained sodium silicate solution with sulfuric acid to pH=8-8.5, removing the sodium sulfate generated by the reaction to obtain silica sol, adding the precipitate formed by the silica sol with a sodium hydroxide solution, and then ultrasonically treating to obtain nano silica sol.

[0040] The preparation method of the nano-silica sol has the advantages of easy availability of raw materials, fast reaction efficiency, high purity, good nano-effect and strong process controllability. It is a preparation method with broad application prospects. The prepared nano-silica sol is suitable for high-entropy oxide ceramics.

[0041] Specifically, firstly, silica ash is dissolved in a 2.5 mol / L sodium hydroxide solution, and the solution is continuously stirred and heated to 80°C for 30 minutes; unreacted silica ash is filtered out, and the obtained sodium silicate solution is neutralized with 2.5 mol / L sulfuric acid to pH=8-8.5, and washed with distilled water for 5-6 times to remove the sodium sulfate generated by the reaction to obtain a clean silica sol; finally, sodium hydroxide is added dropwise to the precipitate formed by the silica sol, and then the nano silica sol is obtained after ultrasonic treatment.

[0042] The silica ash used in the preparation process of the nano-silica sol in this application was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0043] In one embodiment, the high entropy oxide ceramic further comprises 2-4 parts of a fluorocarbon surfactant by weight.

[0044] Preferably, the fluorocarbon surfactant used in the present application is tridecafluorooctanol, which is purchased from Condis Chemical (Hubei) Co., Ltd.; tridecafluorooctanol is slightly soluble in water and soluble in most organic solvents. It has many excellent properties that general hydrocarbon surfactants do not have, such as high surface activity, high heat resistance and chemical stability. It can be used in many special occasions where hydrocarbon surfactants cannot be used. Even at lower concentrations, it has excellent performance and can effectively reduce the surface tension of water to below 20dyn / cm.

[0045] The high surface activity of tridecafluorooctanol enables it to effectively reduce the surface tension of liquids. In the slurry preparation process of solid particles such as ceramic powders and nano-silica sols, it can improve the wetting ability of the solvent on the solid particles, promote the uniform dispersion of the particles, and reduce agglomeration, thereby preparing a slurry with better fluidity and more uniformity, further reducing the generation of microcracks.

[0046] In one embodiment, the oxide ceramic powder includes any five or more of TiO2, Ta2O5, Al2O3, Fe2O3, Ga2O3, CuO, MgO, ZnO, NiOCaO, CoO, CeO2, Gd2O3, SnO2, La2O3, Er2O3, Y2O3, Co3O4 and CaCO3.

[0047] These elements can produce complex interactions in ceramics, forming a synergistic effect, significantly improving the overall performance of ceramic materials, such as mechanical properties, thermal stability, oxidation resistance, and corrosion resistance.

[0048] The oxides in the above-mentioned oxide ceramic powders can be purchased from Zibo Ruisu New Materials Co., Ltd., Shanghai Chuangsai Technology Co., Ltd. and Shanghai Aladdin Biochemical Technology Co., Ltd.

[0049] In one embodiment, the binder includes at least one of polyvinyl alcohol, polydimethylsiloxane alcohol and methyl cellulose.

[0050] Polyvinyl alcohol (PVA) has excellent water solubility and film-forming properties. It can form a viscous solution in water and effectively bond ceramic particles together. It also forms a strong film during the drying process, thereby enhancing the strength of the ceramic body. In polydimethylsiloxane alcohol, the special structure of the siloxane bond gives it good wettability and adhesion, which can promote the bonding between ceramic particles to a certain extent. Methyl cellulose can increase the viscosity and cohesion of the slurry, which helps to evenly distribute and stably suspend the ceramic particles.

[0051] In one embodiment, the dispersant includes at least one of BYK-153, sodium hexametaphosphate, polyethyleneimine and polyaspartic acid.

[0052] By adjusting the type and amount of dispersant, the dispersion performance of ceramic slurry can be accurately controlled, the ceramic preparation process parameters can be optimized, and the quality of ceramic products can be improved.

[0053] In one embodiment, the solvent includes at least one of water, ethanol, propanol, glycerol and acetic acid, and the solvent must contain water.

[0054] Water is a good solvent for many inorganic salts and organic matter, and can dissolve a variety of ceramic powders and dispersants; at the same time, the water-based solvent system is also more friendly to subsequent processing (such as drying, sintering, etc.).

[0055] In one embodiment, the high entropy oxide ceramic further includes 3-4 parts of lubricant and / or 10-17 parts of reinforcing agent, calculated by weight.

[0056] Lubricants can improve the smoothness of mixed oxide ceramic slurry extrusion and improve printing quality.

[0057] During the sintering process, the reinforcing agent can promote the bonding and densification between ceramic particles, form a denser material structure, reduce the pores and defects in the ceramic material, and improve its density and mechanical properties.

[0058] In one embodiment, the lubricant includes one or more of silicone oil, polyvinyl pyrrolidone and polytetrafluoroethylene;

[0059] The reinforcing agent includes one or more of quartz powder, corundum powder, feldspar powder, biotite powder and kaolinite powder.

[0060] The present application also proposes a method for preparing a high entropy oxide ceramic, comprising mixing the raw material components of the high entropy oxide ceramic described in any one of the above items in proportion, stirring, and obtaining a high entropy oxide ceramic slurry, wherein no specific temperature or pressure is required during stirring, but uniform mixing should be ensured, which can be achieved by mechanical stirring or ball milling.

[0061] The high entropy oxide ceramic slurry is printed into a high entropy oxide ceramic slurry body by 3D direct writing printing technology; illustratively, when using 3D direct writing printing technology, the high entropy oxide ceramic slurry is printed layer by layer through a 0.1 mm to 0.6 mm nozzle to form a high entropy oxide ceramic slurry body, the printing speed is 6 mm / s to 10 mm / s; the printing layer thickness is 0.4-0.6 mm;

[0062] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic; illustratively, the degreasing conditions are: heating to 500-570°C at a rate of 1-2°C / min and keeping warm for 2-3 hours, and the degreased body is cooled to room temperature with the furnace; the sintering conditions are: heating to 1500-1700°C at a rate of 7-10°C / min, keeping warm for 2-3 hours, while introducing protective gas, and cooling naturally.

[0063] The raw materials and equipment used in this application, unless otherwise specified, are all commonly used raw materials and equipment in this field; the methods used in this invention, unless otherwise specified, are all conventional methods in this field.

[0064] Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art. However, if there is any conflict, the definitions in this specification shall prevail.

[0065] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0066] The nano-silica sol in the embodiments was prepared by the following method: first, silica ash was dissolved in a 2.5 mol / L sodium hydroxide solution, and the solution was heated to 80°C and kept for 30 min with continuous stirring; unreacted silica ash was filtered out, and the obtained sodium silicate solution was neutralized with 2.5 mol / L sulfuric acid to pH = 8.5, and washed with distilled water for 5 times to remove the sodium sulfate generated by the reaction to obtain a clean silica sol; finally, sodium hydroxide was added dropwise to the precipitate formed by the silica sol, and then the nano-silica sol was obtained after ultrasonic treatment.

[0067] Example 1

[0068] High entropy oxide ceramics include the following components calculated by weight:

[0069] 60 parts of oxide ceramic powder,

[0070] 8 parts of nano silica sol,

[0071] 3 parts of polyvinyl alcohol,

[0072] BYK-153 5 parts,

[0073] 3 parts silicone oil and

[0074] 7 parts water.

[0075] Among them, the oxide ceramic powder is weighed according to the following molar ratio: TiO2:Al2O3:CuO:ZnO:Er2O3=2:1:2:2:1.

[0076] The preparation method comprises: mixing the raw material components of the high entropy oxide ceramic according to a certain proportion, and obtaining a high entropy oxide ceramic slurry by mechanical stirring;

[0077] The high entropy oxide ceramic slurry is printed into a high entropy oxide ceramic slurry body by 3D direct writing printing technology; when using the 3D direct writing printing technology, the high entropy oxide ceramic slurry is printed layer by layer through a 0.5 mm nozzle into a high entropy oxide ceramic slurry body, the printing speed is 8 mm / s, and the printing layer thickness is 0.5 mm;

[0078] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic; the degreasing conditions are: heating to 550°C at a rate of 1.5°C / min and keeping warm for 3 hours, and the degreased body is cooled to room temperature with the furnace; the sintering conditions are: heating to 160°C at a rate of 8°C / min, keeping warm for 3 hours, while introducing protective gas, and cooling naturally.

[0079] The hardness was measured on a small load Vickers hardness tester and the bending strength was measured on an electronic universal material testing machine. The hardness was 92.3HRA and the bending strength was 1750MPa. The fracture toughness K IC16.6MPa·m 1 / 2 .

[0080] Example 2

[0081] High entropy oxide ceramics include the following components calculated by weight:

[0082] 65 parts of oxide ceramic powder,

[0083] 9 parts of nano silica sol,

[0084] 1 part of dimethicone,

[0085] 2 parts of methylcellulose,

[0086] 6 parts of sodium hexametaphosphate, and

[0087] 7 parts water.

[0088] Among them, the oxide ceramic powder is weighed according to the following molar ratio: Ta2O5:Fe2O3:MgO:ZnO:Gd2O3=1:1:2:2:1.

[0089] The preparation method comprises: mixing the raw material components of the high entropy oxide ceramic according to a certain proportion, and obtaining a high entropy oxide ceramic slurry by mechanical stirring;

[0090] The high entropy oxide ceramic slurry is printed into a high entropy oxide ceramic slurry body by 3D direct writing printing technology; when using the 3D direct writing printing technology, the high entropy oxide ceramic slurry is printed layer by layer through a 0.5 mm nozzle into a high entropy oxide ceramic slurry body, the printing speed is 8 mm / s, and the printing layer thickness is 0.5 mm;

[0091] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic; the degreasing conditions are: heating to 550°C at a rate of 1.5°C / min and keeping warm for 3 hours, and the degreased body is cooled to room temperature with the furnace; the sintering conditions are: heating to 160°C at a rate of 8°C / min, keeping warm for 3 hours, while introducing protective gas, and cooling naturally.

[0092] The hardness was measured on a small load Vickers hardness tester and the flexural strength was measured on an electronic universal material testing machine. The hardness was 95.1HRA and the flexural strength was 1810MPa. The fracture toughness K IC 17.3MPa·m 1 / 2 .

[0093] Example 3

[0094] High entropy oxide ceramics include the following components calculated by weight:

[0095] 55 parts of oxide ceramic powder,

[0096] 7 parts of nano silica sol,

[0097] 3 parts of polyvinyl alcohol,

[0098] 3 parts of polyethyleneimine,

[0099] 3 parts of sodium hexametaphosphate,

[0100] 3 parts of polytetrafluoroethylene, and

[0101] 7 parts water.

[0102] Among them, the oxide ceramic powder is weighed according to the following molar ratio: CuO: TiO2: MgO: ZnO: Co3O4: 3: 3: 3: 3: 1.

[0103] The preparation method comprises: mixing the raw material components of the high entropy oxide ceramic according to a certain proportion, and obtaining a high entropy oxide ceramic slurry by mechanical stirring;

[0104] The high entropy oxide ceramic slurry is printed into a high entropy oxide ceramic slurry body by 3D direct writing printing technology; when using the 3D direct writing printing technology, the high entropy oxide ceramic slurry is printed layer by layer through a 0.5 mm nozzle into a high entropy oxide ceramic slurry body, the printing speed is 8 mm / s, and the printing layer thickness is 0.5 mm;

[0105] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic; the degreasing conditions are: heating to 550°C at a rate of 1.5°C / min and keeping warm for 3 hours, and the degreased body is cooled to room temperature with the furnace; the sintering conditions are: heating to 160°C at a rate of 8°C / min, keeping warm for 3 hours, while introducing protective gas, and cooling naturally.

[0106] The hardness was measured on a small load Vickers hardness tester and the bending strength was measured on an electronic universal material testing machine. The hardness was 89.9HRA and the bending strength was 1720MPa. The fracture toughness K IC 16.3MPa·m 1 / 2 .

[0107] Example 4

[0108] High entropy oxide ceramics include the following components calculated by weight:

[0109] 55 parts of oxide ceramic powder,

[0110] 7 parts of nano silica sol,

[0111] 3 parts of polyvinyl alcohol,

[0112] 2 parts of polyethyleneimine,

[0113] 3 parts of tridecafluorooctanol,

[0114] 3 parts of polytetrafluoroethylene, and

[0115] 7 parts water.

[0116] Among them, the oxide ceramic powder is weighed according to the following molar ratio: CuO: TiO2: MgO: ZnO: Co3O4: 3: 3: 3: 3: 1.

[0117] The preparation method comprises: mixing the raw material components of the high entropy oxide ceramic according to a certain proportion, and obtaining a high entropy oxide ceramic slurry by mechanical stirring;

[0118] The high entropy oxide ceramic slurry is printed into a high entropy oxide ceramic slurry body by 3D direct writing printing technology; when using the 3D direct writing printing technology, the high entropy oxide ceramic slurry is printed layer by layer through a 0.5 mm nozzle into a high entropy oxide ceramic slurry body, the printing speed is 8 mm / s, and the printing layer thickness is 0.5 mm;

[0119] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic; the degreasing conditions are: heating to 550°C at a rate of 1.5°C / min and keeping warm for 3 hours, and the degreased body is cooled to room temperature with the furnace; the sintering conditions are: heating to 160°C at a rate of 8°C / min, keeping warm for 3 hours, while introducing protective gas, and cooling naturally.

[0120] The hardness was measured on a small load Vickers hardness tester and the bending strength was measured on an electronic universal material testing machine. The hardness was 98.6HRA and the bending strength was 1830MPa. The fracture toughness K IC 18.3MPa·m 1 / 2 .

[0121] Comparative Example 1

[0122] High entropy oxide ceramics include the following components calculated by weight:

[0123] 60 parts of oxide ceramic powder,

[0124] 3 parts of polyvinyl alcohol,

[0125] BYK-153 5 parts,

[0126] 3 parts silicone oil and

[0127] 7 parts water.

[0128] Among them, the oxide ceramic powder is weighed according to the following molar ratio: TiO2:Al2O3:CuO:ZnO:Er2O3=2:1:2:2:1.

[0129] The preparation method comprises: mixing the raw material components of the high entropy oxide ceramic according to a certain proportion, and obtaining a high entropy oxide ceramic slurry by mechanical stirring;

[0130] The high entropy oxide ceramic slurry is printed into a high entropy oxide ceramic slurry body by 3D direct writing printing technology; when using the 3D direct writing printing technology, the high entropy oxide ceramic slurry is printed layer by layer through a 0.5 mm nozzle into a high entropy oxide ceramic slurry body, the printing speed is 8 mm / s, and the printing layer thickness is 0.5 mm;

[0131] The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic; the degreasing conditions are: heating to 550°C at a rate of 1.5°C / min and keeping warm for 3 hours, and the degreased body is cooled to room temperature with the furnace; the sintering conditions are: heating to 160°C at a rate of 8°C / min, keeping warm for 3 hours, while introducing protective gas, and cooling naturally.

[0132] The hardness was measured on a small load Vickers hardness tester and the bending strength was measured on an electronic universal material testing machine. The hardness was 82.8HRA and the bending strength was 1520MPa. The fracture toughness K IC 13.1MPa·m 1 / 2 .

[0133] According to the above embodiments and comparative examples, after adding nano-silica sol in embodiments 1-4, the high-entropy oxide ceramics obtained after 3D direct writing printing have excellent strength and toughness, reduce the generation of microcracks and improve crack resistance. It is observed that the high-entropy oxide ceramic surface prepared in comparative example 1 has a small amount of cracks, while the high-entropy oxide ceramic surface prepared in embodiments 1-4 does not have cracks. The reason is that during the sintering process, with the volatilization of the solvent and the increase in temperature, the ceramic body gradually densifies and forms the final high-entropy oxide ceramic material. The reinforcing effect of nano-silica sol in this process, the bonding effect of the binder and the dispersing effect of the dispersant jointly enhance the cohesion of the ceramic matrix, improve the strength and toughness of the ceramic, reduce the generation of microcracks and improve crack resistance.

[0134] In Example 4, relative to Example 3, 3 parts of dispersant polyethyleneimine and 3 parts of dispersant sodium hexametaphosphate are replaced with 3 parts of fluorocarbon surfactant tridecafluorooctanol and 2 parts of dispersant polyethyleneimine. The hardness, toughness and flexural strength of Example 4 are all improved. The reason is that although the existing dispersants can effectively improve the dispersibility of ceramic powders, they may not be sufficient to completely prevent the agglomeration of particles. The high surface activity of tridecafluorooctanol enables it to effectively reduce the surface tension of the liquid. In the process of preparing slurry of solid particles such as ceramic powders and nano-silica sols, it can improve the wetting ability of the solvent on the solid particles, promote the uniform dispersion of the particles, reduce agglomeration, thereby preparing a slurry with better fluidity and more uniformity, and further reducing the generation of microcracks.

[0135] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0136] The above-described embodiments only express several embodiments of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A high entropy oxide ceramic with improved crack resistance, characterized in that: The high entropy oxide ceramic comprises the following components calculated by weight:

2. The high entropy oxide ceramic with improved crack resistance according to claim 1, characterized in that: The preparation method of the nano silica sol comprises: Dissolve silica ash in sodium hydroxide solution, stir and heat to 70-80°C, keep warm for 20-30 minutes, filter out unreacted silica ash, neutralize the obtained sodium silicate solution with sulfuric acid to pH=8-8.5, remove the sodium sulfate generated by the reaction to obtain silica sol, add the precipitate formed by silica sol with sodium hydroxide solution, and then obtain nano silica sol after ultrasonic treatment.

3. The high entropy oxide ceramic with improved crack resistance according to claim 2, characterized in that: The high entropy oxide ceramic further comprises 2-4 parts of fluorocarbon surfactant by weight.

4. The high entropy oxide ceramic with improved crack resistance according to claim 1, characterized in that: The oxide ceramic powder includes any five or more of TiO2, Ta2O5, Al2O3, Fe2O3, Ga2O3, CuO, MgO, ZnO, NiOCaO, CoO, CeO2, Gd2O3, SnO2, La2O3, Er2O3, Y2O3, Co3O4 and CaCO3.

5. The high entropy oxide ceramic with improved crack resistance according to claim 1, characterized in that: The binder includes at least one of polyvinyl alcohol, dimethicone alcohol and methyl cellulose.

6. The high entropy oxide ceramic with improved crack resistance according to claim 1, characterized in that: The dispersant includes at least one of BYK-153, sodium hexametaphosphate, polyethyleneimine and polyaspartic acid.

7. The high entropy oxide ceramic with improved crack resistance according to claim 1, characterized in that: The solvent includes at least one of water, ethanol, propanol, glycerol and acetic acid, and the solvent must contain water.

8. The high entropy oxide ceramic with improved crack resistance according to any one of claims 1 to 7, characterized in that: The high entropy oxide ceramic further comprises 3-4 parts of lubricant and / or 10-17 parts of reinforcing agent, calculated by weight.

9. The high entropy oxide ceramic with improved crack resistance according to claim 8, characterized in that: The lubricant includes one or more of silicone oil, polyvinyl pyrrolidone and polytetrafluoroethylene; The reinforcing agent includes one or more of quartz powder, corundum powder, feldspar powder, biotite powder and kaolinite powder.

10. A method for preparing a high entropy oxide ceramic, characterized in that: The method comprises mixing and stirring the raw material components of the high entropy oxide ceramic according to any one of claims 1 to 9 in proportion to obtain a high entropy oxide ceramic slurry; Printing the high entropy oxide ceramic slurry into a high entropy oxide ceramic slurry green body by 3D direct writing printing technology; The high entropy oxide ceramic body is dried, degreased and sintered in sequence to obtain a 3D printed high entropy oxide ceramic.

Citation Information

Cited By

  • Ultrahigh-temperature carbon-based high-entropy ceramic coating and preparation method thereof

    CN119899996A