Sintered aeolian sand pottery sand and preparation method thereof
Through the combined utilization of aeolian sand powder, aluminum waste slag and steel slag powder, sintered aeolian sand pottery sand with excellent performance is prepared, which solves the problems of non-renewable resources and environmental pollution in pottery sand production and realizes the sustainability of pottery sand. development and environmental protection.
Patent Information
- Application Number
- CN202410787438.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The non-renewable resources used in the current production of clay sand cause environmental damage, and the wind-blown sand and industrial waste residues cannot be effectively utilized, which affects the sustainable development and environmental protection of clay sand.
Using raw materials such as aeolian sand powder, aluminum waste slag and steel slag powder, sintered aeolian sand ceramic sand is prepared through granulation and sintering processes to realize the recycling of industrial waste residue and resource utilization of aeolian sand.
The sintered aeolian sand pottery sand with excellent performance is prepared, with a bulk density of less than 1200kg/m3, a cylinder pressure strength of more than 22MPa, and a water absorption rate of less than 10% in 1 hour, realizing the recycling and reuse of industrial waste and maximizing the utilization of resources. Reduces environmental pollution.
Smart Images

Figure BDA0004898990040000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to sintered aeolian sand pottery sand and a preparation method thereof. Background Art
[0002] As a lightweight and porous ceramic granular material, ceramic sand is known for its low density, high compressive strength and high porosity. It is mainly used in the construction industry and the fields of thermal insulation and refractory materials. In the production process of ceramic sand, natural resources such as shale and clay are mainly used as raw materials. However, since these raw materials are non-renewable resources, large-scale mining and use may cause environmental damage, thus posing a major threat to the sustainable production and development of ceramic sand. Therefore, finding alternative raw materials to reduce the impact on the environment is crucial for the future development of the ceramic sand industry.
[0003] Aeolian sand is formed by the disintegration of sandstone due to strong desert sunlight, scarce precipitation, and high evaporation. Under long-term wind movement, the edges and corners of the stone fragments are polished and rounded, and the wind blows and accumulates over long distances. Aeolian sand particles are small, with a particle size generally between 0.075 and 0.25 mm. They are prone to form large-scale "sand wasteland" and "sand disasters", which seriously restrict the social and economic development of surrounding areas. In addition, the grading of aeolian sand particles is discontinuous, and the particles are evenly distributed. This grading feature increases the amount of cement when used as fine aggregate, and leads to reduced fluidity and strength of aeolian sand concrete.
[0004] The long-term storage of industrial waste residues will occupy a large amount of land resources, restrict other uses of land, and also lead to a decline in land quality, affecting agricultural production and the ecological environment. Secondly, the harmful components in the waste residues may penetrate into the soil after being leached by rain and snow, causing soil acidification, alkalization and hardening, and even causing heavy metal pollution. At the same time, industrial waste residues will also pollute water bodies. When toxic substances enter water bodies through soil, they will seriously affect water quality, endanger the survival of aquatic organisms, and may enter the human living system through water sources, causing health risks.
[0005] Therefore, it is urgent to consume a large amount of aeolian sand and industrial waste residues that are difficult to utilize to reduce environmental pollution. Therefore, a method for preparing pottery sand by combining aeolian sand and industrial waste residue resources is provided. This is one of the effective ways to realize the large-scale utilization of aeolian sand and industrial waste residues, which is of great significance to the maximum utilization of resources, environmental protection and the sustainable production and development of pottery sand. However, there is currently no solution for preparing pottery sand by combining aeolian sand and industrial waste residues. Summary of the invention
[0006] In view of this, the present invention provides a sintered aeolian sand pottery sand and a preparation method thereof. The main purpose is to use aeolian sand powder, aluminum waste slag, steel slag powder, water, etc. to develop a kind of aeolian sand sintered pottery sand, which can dispose of industrial waste and realize the resource, high value and diversified utilization of aeolian sand.
[0007] In a first aspect, the present invention provides a sintered aeolian sand pottery sand comprising the following components in parts by weight: 50 to 80 parts of aeolian sand powder, 10 to 40 parts of aluminum waste slag, 10 to 20 parts of steel slag powder, and 25 to 30 parts of water.
[0008] Preferably, the particle size of the aeolian sand powder is ≤0.075 mm.
[0009] Preferably, the aluminum waste slag includes at least one of coal gangue powder and fly ash.
[0010] Preferably, the steel slag powder comprises the following components in mass fraction: SiO2 14%-18%, Al2O3 7%-9%, Fe2O3 16%-20%, CaO 36%-40%, MgO 8%-10%, Na2O 1%-2%, K2O1%-2%, MnO 3%-5%, TiO2 1%-2%, and the content of unavoidable impurities is <0.1%.
[0011] Preferably, the particle size of the aluminum waste slag is ≤0.075 mm;
[0012] And / or, the particle size of the steel slag powder is ≤0.075 mm.
[0013] In a second aspect, the present invention further provides a method for preparing the sintered aeolian sand pottery sand, comprising the following steps:
[0014] Mixing aluminum waste slag, steel slag powder and aeolian sand powder to obtain a mixture;
[0015] The mixed material is added to a granulator, and water is added to granulate the mixture to obtain ceramic sand raw material balls;
[0016] Place the raw clay balls in an indoor environment for natural curing;
[0017] The naturally cured pottery sand raw material balls are sintered to obtain sintered aeolian sand pottery sand.
[0018] Preferably, sintering the naturally cured pottery sand raw material balls specifically includes:
[0019] The ceramic sand raw material balls are added into a high temperature furnace and preheated at 300-500° C. for 10-60 minutes, and then heated to a sintering temperature of 1050-1200° C. at a heating rate of 5-20° C. / min, and sintered for 1-60 minutes.
[0020] Preferably, placing the ceramic sand raw material balls in an indoor environment for natural curing specifically includes:
[0021] Place the raw ceramic sand balls in an indoor environment and cure them at a temperature of 20±3°C and a relative humidity of 60±5%RH for 1 to 3 days.
[0022] Preferably, the mixture is added to a granulator for granulation, and water is added in multiple times for stirring and granulation to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60-120r / min, the rotation angle is 30-60°, and the rotation time is 5-25min; the particle size of the ceramic sand raw material balls is 1.18-4.75mm.
[0023] Preferably, aluminum waste slag, steel slag powder and aeolian sand powder are mixed and placed in a disperser to be dispersed for 3 to 5 minutes to obtain a mixture.
[0024] The sintered aeolian sand pottery sand of the present invention has the following beneficial effects compared with the prior art:
[0025] The sintered aeolian sand pottery sand of the present invention uses aluminum waste slag as aluminum material and steel slag powder as a melting aid component to prepare sintered pottery sand, turning industrial waste slag that pollutes the environment into treasure; the present invention uses aeolian sand powder as siliceous material and prepares aeolian sand sintered pottery sand with a large amount of aeolian sand powder, which plays a positive role in the sustainable development of mineral resources and the resource utilization of aeolian sand; the aeolian sand sintered pottery sand prepared by the combination of various raw materials of the present invention has a bulk density of less than 1200kg / m 3 The cylinder pressure strength can reach more than 22MPa, and the 1h water absorption rate is less than 10%. It is a high-strength lightweight aggregate. By reasonably controlling the formula ratio, the product performance is excellent. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The following are described in detail. It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered ranges, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.
[0028] The invention provides sintered aeolian sand pottery sand, which comprises the following components in parts by weight: 50-80 parts of aeolian sand powder, 10-40 parts of aluminum waste slag, 10-20 parts of steel slag powder and 25-30 parts of water.
[0029] In the aeolian sand sintered pottery sand of the present invention, the aeolian sand powder belongs to the siliceous material, the aluminum waste slag provides the aluminum material, and the steel slag powder is the melting-aiding component. At 573℃, α-quartz in aeolian sand powder transforms into β-quartz, at 870℃, it transforms into β-phosphotarzite, at 1100℃~1200℃, amorphous SiO2 transforms into β-cristobalite; at 0~400℃, water vapor and CO2 in the pellets escape, at 400~500℃, MgCO3 decomposes into MgO and CO2, at 400~800℃, CaCO3 decomposes into CaO and CO2, at 900℃, sulfide decomposes into S and SO2, at 1000~1300℃, iron oxide decomposes into CO2 and CO; at the same time, aeolian sand powder appears liquid phase components under the action of high temperature and steel slag powder, the liquid phase components play a role in bonding solid phase components while encapsulating gases such as CO2 and CO, the gas pressure increases to cause the pellets to expand, and Al2O3 forms a large amount of mullite phase after firing, giving the ceramic sand excellent mechanical properties.
[0030] In some embodiments, the aeolian sand powder is ground aeolian sand, and the particle size of the aeolian sand powder is ≤0.075 mm.
[0031] In some embodiments, the aluminum waste slag includes at least one of coal gangue powder and fly ash.
[0032] In some embodiments, the steel slag powder includes the following components by mass fraction: SiO2 14%-18%, Al2O3 7%-9%, Fe2O3 16%-20%, CaO 36%-40%, MgO 8%-10%, Na2O 1%-2%, K2O1%-2%, MnO 3%-5%, TiO21%-2%, and the content of unavoidable impurities is <0.1%.
[0033] In some embodiments, the particle size of the aluminum waste slag is ≤ 0.075 mm;
[0034] In some embodiments, the particle size of the steel slag powder is ≤ 0.075 mm.
[0035] Based on the same inventive concept, the present invention also provides a method for preparing sintered aeolian sand pottery sand, comprising the following steps:
[0036] S1, mixing aluminum waste slag, steel slag powder and aeolian sand powder to obtain a mixture;
[0037] S2, adding the mixture to a granulator, adding water, and granulating to obtain ceramic sand raw material balls;
[0038] S3, placing the raw ceramic sand balls in an indoor environment for natural curing;
[0039] S4, sintering the natural curing pottery sand raw material balls to obtain sintered aeolian sand pottery sand.
[0040] In some embodiments, sintering the naturally cured ceramic sand raw material balls specifically includes:
[0041] The ceramic sand raw material balls are added into a high temperature furnace and preheated at 300-500° C. for 10-60 minutes, and then heated to a sintering temperature of 1050-1200° C. at a heating rate of 5-20° C. / min, and sintered for 1-60 minutes.
[0042] In some embodiments, placing the ceramic sand raw material balls in an indoor environment for natural curing specifically includes:
[0043] Place the raw ceramic sand balls in an indoor environment and cure them at a temperature of 20±3°C and a relative humidity of 60±5%RH for 1 to 3 days.
[0044] In some embodiments, the mixture is added to a granulator for granulation, and water is added multiple times (specifically 3 to 5 times) for stirring and granulation to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60 to 120 r / min, the rotation angle is 30 to 60°, and the rotation time is 5 to 25 min; the particle size of the ceramic sand raw material balls is 1.18 to 4.75 mm.
[0045] In some embodiments, aluminum waste slag, steel slag powder, and aeolian sand powder are mixed and placed in a disperser for 3 to 5 minutes to obtain a mixture.
[0046] In some embodiments, the method for preparing aeolian sand powder is: placing the accumulated sand in an oven to dry, crushing the dried aeolian sand into powder, and passing it through a 200-mesh square hole sieve to obtain aeolian sand powder.
[0047] The aeolian sand sintered pottery sand and the preparation method thereof of the present invention have at least the following advantages: the present invention uses aluminum waste slag as aluminum material and steel slag powder as a melting aid component to prepare sintered pottery sand, thereby turning industrial waste slag that pollutes the environment into treasure; the present invention uses aeolian sand powder as siliceous material and prepares aeolian sand sintered pottery sand with a large amount of aeolian sand powder, thereby playing a positive role in the sustainable development of mineral resources and the resource utilization of aeolian sand; the aeolian sand sintered pottery sand prepared by the combination of various raw materials of the present invention has a bulk density of less than 1200kg / m 3 The cylinder pressure strength can reach more than 22MPa, and the 1h water absorption rate is less than 10%. It is a high-strength lightweight aggregate. By reasonably controlling the formula ratio, the product performance is excellent.
[0048] The sintered aeolian sand pottery sand prepared by the invention has excellent properties in all aspects and realizes the recycling and reuse of industrial waste. Meanwhile, a large amount of aeolian sand powder added is of great significance to the maximum utilization of resources, environmental protection and sustainable production and development of pottery sand.
[0049] The sintered aeolian sand pottery sand and its preparation method of the present application are further described below with specific examples. This section further illustrates the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0050] Example 1
[0051] This embodiment provides a sintered aeolian sand pottery sand, comprising the following components by weight: 70 parts of aeolian sand powder, 20 parts of aluminum waste slag, 10 parts of steel slag powder, and 30 parts of water;
[0052] Among them, the average particle size of aeolian sand powder is 0.035mm;
[0053] Aluminum waste residue is fly ash;
[0054] The steel slag powder includes the following components by mass fraction: SiO2 17%, Al2O3 8.55%, Fe2O3 18%, CaO38.5%, MgO 9.5%, Na2O 1.7%, K2O 1.5%, MnO 3.55%, TiO2 1.65%, and unavoidable impurities content 0.05%;
[0055] The average particle size of aluminum waste slag is 0.045mm;
[0056] The average particle size of the steel slag powder is 0.05 mm.
[0057] This embodiment also provides a method for preparing the sintered aeolian sand pottery sand, comprising the following steps:
[0058] S1. Mix aluminum waste slag, steel slag powder and aeolian sand powder and place them in a disperser for 5 minutes to obtain a mixture;
[0059] S2, adding the mixture to a granulator, and adding water three times (each time with the same amount of water), stirring and granulating to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60r / min, the rotation angle is 45°, and the rotation time is 10min; the average particle size of the ceramic sand raw material balls is 2.32mm;
[0060] S3, placing the raw ceramic sand balls in an indoor environment, and curing them at a temperature of 20°C and a relative humidity of 60%RH for 1 day;
[0061] S4. Add the cured pottery sand raw material balls into a high-temperature furnace, preheat at 450°C for 30 minutes, heat to a sintering temperature of 1150°C at a heating rate of 5-20°C / min, sinter for 30 minutes, and cool to room temperature to obtain sintered aeolian sand pottery sand.
[0062] Example 2
[0063] This embodiment provides a sintered aeolian sand pottery sand, comprising the following components by weight: 60 parts of aeolian sand powder, 30 parts of aluminum waste slag, 10 parts of steel slag powder, and 30 parts of water;
[0064] Among them, the average particle size of aeolian sand powder is 0.035mm;
[0065] Aluminum waste residue is fly ash;
[0066] The steel slag powder includes the following components by mass fraction: SiO2 17%, Al2O3 8.55%, Fe2O3 18%, CaO38.5%, MgO 9.5%, Na2O 1.7%, K2O 1.5%, MnO 3.55%, TiO2 1.65%, and unavoidable impurities content 0.05%;
[0067] The average particle size of aluminum waste slag is 0.045mm;
[0068] The average particle size of the steel slag powder is 0.05 mm.
[0069] This embodiment also provides a method for preparing the sintered aeolian sand pottery sand, comprising the following steps:
[0070] S1. Mix aluminum waste slag, steel slag powder and aeolian sand powder and place them in a disperser for 5 minutes to obtain a mixture;
[0071] S2, adding the mixture to a granulator, and adding water three times (each time with the same amount of water), stirring and granulating to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60r / min, the rotation angle is 45°, and the rotation time is 10min; the average particle size of the ceramic sand raw material balls is 2.28mm;
[0072] S3, placing the raw ceramic sand balls in an indoor environment, and curing them at a temperature of 20°C and a relative humidity of 60%RH for 1 day;
[0073] S4. Add the cured pottery sand raw material balls into a high-temperature furnace, preheat at 450°C for 30 minutes, heat to a sintering temperature of 1150°C at a heating rate of 5-20°C / min, sinter for 30 minutes, and cool to room temperature to obtain sintered aeolian sand pottery sand.
[0074] Example 3
[0075] This embodiment provides a sintered aeolian sand pottery sand, comprising the following components by weight: 70 parts of aeolian sand powder, 20 parts of aluminum waste slag, 10 parts of steel slag powder, and 30 parts of water;
[0076] Among them, the average particle size of aeolian sand powder is 0.035mm;
[0077] Aluminum waste slag is coal gangue powder;
[0078] The steel slag powder includes the following components by mass fraction: SiO2 17%, Al2O3 8.55%, Fe2O3 18%, CaO38.5%, MgO 9.5%, Na2O 1.7%, K2O 1.5%, MnO 3.55%, TiO2 1.65%, and unavoidable impurities content 0.05%;
[0079] The average particle size of aluminum waste slag is 0.045mm;
[0080] The average particle size of the steel slag powder is 0.05 mm.
[0081] This embodiment also provides a method for preparing the sintered aeolian sand pottery sand, comprising the following steps:
[0082] S1. Mix aluminum waste slag, steel slag powder and aeolian sand powder and place them in a disperser for 5 minutes to obtain a mixture;
[0083] S2, adding the mixture to a granulator, and adding water three times (each time with the same amount of water), stirring and granulating to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60r / min, the rotation angle is 45°, and the rotation time is 10min; the average particle size of the ceramic sand raw material balls is 2.36mm;
[0084] S3, placing the raw ceramic sand balls in an indoor environment, and curing them at a temperature of 20°C and a relative humidity of 60%RH for 1 day;
[0085] S4. Add the cured pottery sand raw material balls into a high-temperature furnace, preheat at 450°C for 30 minutes, heat to a sintering temperature of 1150°C at a heating rate of 5-20°C / min, sinter for 30 minutes, and cool to room temperature to obtain sintered aeolian sand pottery sand.
[0086] Example 4
[0087] This embodiment provides a sintered aeolian sand pottery sand, comprising the following components by weight: 60 parts of aeolian sand powder, 30 parts of aluminum waste slag, 10 parts of steel slag powder, and 30 parts of water;
[0088] Among them, the average particle size of aeolian sand powder is 0.035mm;
[0089] Aluminum waste slag is coal gangue powder;
[0090] The steel slag powder includes the following components by mass fraction: SiO2 17%, Al2O3 8.55%, Fe2O3 18%, CaO38.5%, MgO 9.5%, Na2O 1.7%, K2O 1.5%, MnO 3.55%, TiO2 1.65%, and unavoidable impurities content 0.05%;
[0091] The average particle size of aluminum waste slag is 0.045mm;
[0092] The average particle size of the steel slag powder is 0.05 mm.
[0093] This embodiment also provides a method for preparing the sintered aeolian sand pottery sand, comprising the following steps:
[0094] S1. Mix aluminum waste slag, steel slag powder and aeolian sand powder and place them in a disperser for 5 minutes to obtain a mixture;
[0095] S2, adding the mixture to a granulator, and adding water three times (each time with the same amount of water), stirring and granulating to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60r / min, the rotation angle is 45°, and the rotation time is 10min; the average particle size of the ceramic sand raw material balls is 2.41mm;
[0096] S3, placing the raw ceramic sand balls in an indoor environment, and curing them at a temperature of 20°C and a relative humidity of 60%RH for 1 day;
[0097] S4. Add the cured pottery sand raw material balls into a high-temperature furnace, preheat at 450°C for 30 minutes, heat to a sintering temperature of 1150°C at a heating rate of 5-20°C / min, sinter for 30 minutes, and cool to room temperature to obtain sintered aeolian sand pottery sand.
[0098] Performance Testing
[0099] The sintered aeolian sand prepared in Examples 1 to 4 was tested for cylinder compressive strength, apparent density, bulk density and water absorption with reference to Light Aggregate and Test Methods Thereof Part 2: Light Aggregate Test Method (GB / T 17431.2-2010). The results are shown in Table 1.
[0100] Table 1 - Properties of sintered aeolian sand prepared in Examples 1 to 4
[0101]
[0102]
[0103] It can be seen from Table 1 that the cylinder compressive strength of the sintered aeolian sand prepared in Example 1 is 22.6 MPa and the apparent density is 1929 kg / m 3 , bulk density is 1157kg / m 3 , 1h water absorption rate is 4.0%; the cylinder compressive strength of the sintered aeolian sand prepared in Example 2 is 20.3MPa, and the apparent density is 1868kg / m 3 , bulk density is 1183kg / m 3 , 1h water absorption rate is 6.2%; the cylinder compressive strength of the sintered aeolian sand prepared in Example 3 is 20.5MPa, and the apparent density is 1795kg / m 3 , bulk density is 1071kg / m 3 , 1h water absorption rate is 8.5%; the cylinder compressive strength of the sintered aeolian sand prepared in Example 4 is 18.9MPa, and the apparent density is 1753kg / m 3 , bulk density is 1066kg / m 3The water absorption rate in 1h is 9.3%. The bulk density of the sintered aeolian sand prepared in Examples 1 to 4 is less than 1200 kg / m 3 The maximum cylinder pressure strength reaches 22.6MPa, and the 1h water absorption rate is less than 10%. It is a high-strength lightweight aggregate with high application value.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A sintered aeolian sand pottery sand, characterized in that: The invention comprises the following components in parts by weight: 50 to 80 parts of aeolian sand powder, 10 to 40 parts of aluminum waste slag, 10 to 20 parts of steel slag powder and 25 to 30 parts of water.
2. The sintered aeolian sand pottery sand according to claim 1, characterized in that: The particle size of the aeolian sand powder is ≤0.075 mm.
3. The sintered aeolian sand pottery sand according to claim 1, characterized in that: The aluminum waste slag includes at least one of coal gangue powder and fly ash.
4. The sintered aeolian sand pottery sand according to claim 1, characterized in that: The steel slag powder comprises the following components by mass fraction: SiO2 14%-18%, Al2O3 7%-9%, Fe2O3 16%-20%, CaO36%-40%, MgO 8%-10%, Na2O1%-2%, K2O 1%-2%, MnO 3%-5%, TiO21%-2%, and the content of inevitable impurities is less than 0.1%.
5. The sintered aeolian sand pottery sand according to claim 1, characterized in that: The particle size of the aluminum waste slag is ≤0.075mm; And / or, the particle size of the steel slag powder is ≤0.075 mm.
6. A method for preparing sintered aeolian sand pottery sand according to any one of claims 1 to 5, characterized in that: The following steps are involved: Mixing aluminum waste slag, steel slag powder and aeolian sand powder to obtain a mixture; The mixed material is added to a granulator, and water is added to granulate the mixture to obtain ceramic sand raw material balls; Place the raw clay balls in an indoor environment for natural curing; The naturally cured pottery sand raw material balls are sintered to obtain sintered aeolian sand pottery sand.
7. The method for preparing sintered aeolian sand pottery sand according to claim 6, characterized in that: Sintering the naturally cured raw clay balls specifically includes: The ceramic sand raw material balls are added into a high temperature furnace and preheated at 300-500° C. for 10-60 minutes, and then heated to a sintering temperature of 1050-1200° C. at a heating rate of 5-20° C. / min, and sintered for 1-60 minutes.
8. The method for preparing sintered aeolian sand pottery sand according to claim 6, characterized in that: The natural curing of ceramic sand raw material balls in indoor environment specifically includes: Place the raw clay balls in an indoor environment and cure them at a temperature of 20±3°C and a relative humidity of 60±5%RH for 1 to 3 days.
9. The method for preparing sintered aeolian sand pottery sand according to claim 6, characterized in that: The mixed material is added into a granulator for granulation, and water is added several times for stirring and granulation to obtain ceramic sand raw material balls; during the granulation process, the rotation speed of the granulator is 60-120r / min, the rotation angle is 30-60°, and the rotation time is 5-25min; the particle size of the ceramic sand raw material balls is 1.18-4.75mm.
10. The method for preparing sintered aeolian sand pottery sand according to claim 6, characterized in that: Aluminum waste slag, steel slag powder and aeolian sand powder are mixed and placed in a disperser for 3 to 5 minutes to obtain a mixture.
Citation Information
Patent Citations
Ceramic brick prepared from aeolian sand
CN102211922A
Aeolian sand cement
CN103319104A
Method for preparing quartz ceramic by using desert wind-accumulated sand
CN103755330A
Partition wall batten prepared by using wind-blown sand and preparation method thereof
CN108218385A
High-performance cement clinker made by effectively utilizing aeolian sand
CN109437620A