Beta-position tetra-substituted porphyrin organic photovoltaic material as well as preparation method and application thereof

By using three bonds to connect the electricity-absorbing units at the four symmetric β positions of porphyrin and adjusting the side groups, a β-position tetra-substituted porphyrin organic photovoltaic material was designed, which solved the problem of low photoelectric conversion efficiency of existing porphyrin materials and improved The photovoltaic performance of organic solar cells achieves high photoelectric conversion efficiency.

CN118791504AActive Publication Date: 2024-10-18SOUTH CHINA UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310390304.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-18
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

The photoelectric conversion efficiency of existing beta-modified porphyrin materials in organic solar cells is low, only 3.03%, and has few applications in the field of organic solar cells, making it difficult to meet the demand for efficient and stable active materials.

Method used

By using three bonds to connect the electricity-withdrawing units at the four symmetrical β-positions of porphyrin, the planarity of the molecule is enhanced, and the absorption and energy level of the molecule are adjusted by changing the side groups of the porphyrin ring and the electricity-withdrawing unit, and a four-substitution at the β-position is designed. Porphyrin organic photovoltaic materials are prepared using specific synthesis methods to improve their performance.

Benefits of technology

The material's absorption red shift and broadening were achieved, the light absorption capacity was enhanced, and donor materials with matching energy levels were designed to improve the photovoltaic performance of organic solar cells. The photoelectric conversion efficiency reached 5.62% to 6.21%, providing new molecules. Design direction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791504A_ABST
    Figure CN118791504A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of organic small molecule photovoltaic materials, and discloses a beta-tetra-substituted porphyrin organic photovoltaic material and a preparation method and application thereof. According to the beta-position tetra-substituted porphyrin photovoltaic material, a porphyrin ring is used as a central power supply unit, and four symmetrical beta positions of tetraphenylporphyrin are connected with power absorption units to synthesize target molecules, so that a push-pull electron effect is formed, and intramolecular charge transfer and broadening absorption can be effectively enhanced. By changing side groups of a porphyrin ring and an electricity absorption unit, the absorption and energy level of molecules are effectively adjusted, and the purpose of further optimizing the material performance is achieved. The modification property of the porphyrin beta site is proved, and a new direction is provided for the molecular design of the beta-site porphyrin material of the organic solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic small molecule photovoltaic materials, and specifically relates to a type of β-position tetrasubstituted porphyrin organic photovoltaic material and a preparation method and application thereof. Background Art

[0002] On the one hand, traditional fossil energy is facing a serious crisis of energy depletion, and on the other hand, it also causes great environmental pollution during its application. Solar energy resources are abundant, easy to obtain, clean and green, and organic solar cells that convert solar energy into electrical energy have been widely studied. Organic solar cells achieve photoelectric conversion by absorbing photons through organic photoactive materials. The efficiency of single-junction devices has now exceeded 19%, and the certified efficiency of tandem cell devices has exceeded 20%. Its material structure is rich and can be prepared by solution processing and roll-to-roll large-scale printing; it is conducive to the realization of low-toxic or non-toxic device design; at the same time, it is flexible and light and can be used for wear, and can be made into semi-transparent devices for green buildings, which has great application prospects. Therefore, the development of efficient and stable active materials is the focus of current research on organic solar cells.

[0003] Porphyrin and its derivatives have a wide absorption region and a high extinction coefficient, and the molecular tunability is large. The photoelectric properties can be adjusted by introducing functional groups on the periphery of the porphyrin or introducing different metals in the center. In addition, the conjugated plane is large, has a strong electron-donating ability, and has good stability. The donor materials based on porphyrin have currently achieved an efficiency of more than 12%. Most of the efficient porphyrin materials use pyrrolopyrrole dione as the electron-absorbing unit and extend the conjugation at the meso position. But in fact, β-substituted porphyrins show unique electron transfer properties, which are of great research significance in the field of organic solar cells. However, β-modified porphyrin materials are rarely used in organic solar cells, and only one patent (China Invention Authorization Right CN113105463 B) has obtained a low photoelectric conversion efficiency (PCE) of 3.03%. Summary of the invention

[0004] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a class of β-position tetrasubstituted porphyrin organic photovoltaic materials. The present invention uses the porphyrin ring as the power supply unit, and uses triple bonds to connect the power-absorbing units at the four symmetrical β positions of the porphyrin to synthesize the donor material. The use of triple bonds to enhance the molecular planarity is beneficial to charge transfer; at the same time, by changing the porphyrin ring and the side groups of the power-absorbing units, the absorption and energy level of the molecule are effectively adjusted, thereby achieving the purpose of further optimizing the material performance.

[0005] Another object of the present invention is to provide a method for preparing a type of β-position tetrasubstituted porphyrin organic photovoltaic material.

[0006] Another object of the present invention is to provide application of the above-mentioned β-position tetrasubstituted porphyrin organic photovoltaic material in organic solar cells.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A class of β-tetrasubstituted porphyrin organic photovoltaic materials has the following chemical structure:

[0009]

[0010] Wherein, A is an electron-withdrawing group having a conjugated structure; and R is hydrogen or an alkyl or alkoxy group having 1 to 4 carbon atoms.

[0011] Preferably, A is one of the following structural units:

[0012]

[0013] Preferably, R is at least one of an H atom, a methyl group, a methoxy group, an isopropyl group, an n-butyl group, and a tert-butyl group.

[0014] The preparation method of the above-mentioned β-position tetrasubstituted porphyrin organic photovoltaic material comprises the following steps:

[0015] (1) dissolving compound (I) in an organic solvent and reacting with N-bromosuccinimide (NBS) at 60-70° C. for 3-5 hours to obtain a compound represented by formula (II);

[0016]

[0017] (2) dissolving compound (II) in an organic solvent, adding zinc acetate and reacting at 60-70° C. for 8-15 hours to obtain compound (III);

[0018]

[0019] (3) dissolving compound (III) in an organic solvent, adding triisopropylsilyl acetylene, reacting at 60-70° C. for 18-30 hours in the presence of a catalyst to obtain an intermediate product (IV);

[0020] (4) The intermediate product (IV) is dissolved in an organic solvent, and a tetrabutylammonium fluoride (THF) solution is added at room temperature and stirred for 5-30 minutes. Water is added to quench the reaction, and the mixture is extracted, dried by spin drying, and directly used for the next step of reaction;

[0021] (5) The spin-dried product in step (4) and the diketopyrrolidine monomer of the receptor molecule A are heated under reflux in an organic solvent for 48-72 hours in the presence of a catalyst to obtain the target compound.

[0022] Wherein, R and A have the same definitions as above.

[0023] Preferably, the organic solvent in step (1) is one of chloroform and dichloromethane;

[0024] Preferably, the molar ratio of compound (I) to N-bromosuccinimide in step (1) is 1:5-1:7;

[0025] Preferably, the organic solvent in step (2) is a mixed solution of chloroform and methanol; the molar amount of chloroform is 3000-4000 times the molar amount of compound (II), and the volume ratio of chloroform to methanol is 6:1-3:1;

[0026] Preferably, the molar ratio of compound (II) to zinc acetate in step (2) is 1:5-1:8;

[0027] Preferably, the organic solvent in step (3) is a mixed solvent of tetrahydrofuran and triethylamine; the molar amount of tetrahydrofuran is 1000-3000 times the molar amount of compound (III), and the volume ratio of tetrahydrofuran to triethylamine is 2:1-5:1;

[0028] Preferably, the molar ratio of compound (III) to triisopropylsilyl acetylene in step (3) is 1:8-1:12;

[0029] Preferably, the catalyst in step (3) is bis(triphenylphosphine)palladium dichloride and cuprous iodide, and the molar amount of both is 0.15 times the molar amount of compound (III);

[0030] Preferably, the organic solvent in step (4) is tetrahydrofuran; the molar amount of tetrahydrofuran is 1000-3000 times the molar amount of compound (IV);

[0031] Preferably, the molar ratio of the intermediate product (IV) to tetrabutylammonium fluoride in step (4) is 1:6-1:8;

[0032] Preferably, the molar ratio of the spin-dried product in step (5) to the diketopyrrolidine monomer of the receptor molecule A is 1:6-1:8;

[0033] The organic solvent in step (5) is a mixed solvent of tetrahydrofuran and triethylamine; the molar amount of tetrahydrofuran is 1000-3000 times the molar amount of the spin-dried product, and the volume ratio of tetrahydrofuran to triethylamine is 2:1-5:1

[0034] Preferably, the catalyst in step (5) is tetrakis(triphenylphosphine)palladium and cuprous iodide; the molar amount of both is 0.15 times the molar amount of the spin-dried product.

[0035] The application of the above-mentioned β-position tetrasubstituted porphyrin organic photovoltaic material is preferably application in organic solar cells.

[0036] The above-mentioned β-position tetrasubstituted porphyrin organic photoelectric material is used as a donor photovoltaic material, with the porphyrin ring as the electron-donating group, and the electron-withdrawing unit is connected by triple bonds to form an effective push-pull electron effect to regulate molecular absorption and energy levels.

[0037] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0038] (1) The present invention uses triple bonds to connect electron-withdrawing units at four symmetrical β positions of porphyrin to maintain the molecular planar structure, effectively increase the molecular conjugation and intramolecular charge transfer (ICT), red-shift and broaden the absorption of the material, and enhance the light absorption capacity of the active layer material.

[0039] (2) The present invention changes the electron-withdrawing ability of the electron-withdrawing group conjugated with porphyrin, effectively adjusting the energy level of the material, thereby designing a donor-acceptor material with a better energy level match.

[0040] (3) The present invention changes the length of the side alkyl chain of the porphyrin electron-withdrawing unit, improves the solubility of the molecule, changes the stacking structure of the molecule, and affects the photovoltaic performance of the organic solar cell device prepared later.

[0041] (4) The β-site tetrasubstituted porphyrin material designed by the present invention further demonstrates the modifiability of porphyrin at multiple sites and provides a new direction for the molecular design of β-site porphyrin materials for organic solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is the H NMR spectrum of Example 1.

[0043] Figure 2 This is the mass spectrum (MALDI-TOF) of Example 1.

[0044] Figure 3 This is the H NMR spectrum of Example 2.

[0045] Figure 4 This is the mass spectrum (MALDI-TOF) of Example 2.

[0046] Figure 5 The UV-visible absorption spectra of the solution and film of Example 1 are shown in FIG.

[0047] Figure 6 The UV-visible absorption spectra of the solution and film of Example 2 are shown in FIG.

[0048] Figure 7 The photovoltaic cells prepared from the materials obtained in Examples 1 and 2 were subjected to AM 1.5 and 100 mW / cm 2 Current-voltage curve under illumination. DETAILED DESCRIPTION

[0049] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0050] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.

[0051] Example 1

[0052] Preparation of EHDPP-Por molecules: R is H atom, and A unit is 2-ethylhexyl substituted diketopyrrolopyrrole (EHDPP).

[0053] The reaction process of Example 1 is as follows:

[0054]

[0055] (1) Compound 1 (800 mg, 1.3 mmol) and NBS (1.39 g, 7.8 mmol) were added to a two-necked flask, 100 mL of chloroform solution was used as solvent, and the mixture was refluxed at 65° C. for 4 hours. The reaction was terminated after detection on a TLC plate. The solvent was dried by a rotary evaporator, and the mixture was purified by silica gel chromatography using petroleum ether and dichloromethane as eluents. Compound 2 (725 mg, yield 60%) was obtained by recrystallization.

[0056] (2) Compound 2 (720 mg, 0.77 mmol) and zinc acetate (706 mg, 3.85 mmol) were added to a 250 mL reaction bottle, and a mixed solvent of 100 ml of chloroform and 20 ml of methanol was added. The mixture was refluxed at 65° C. overnight. The reaction was terminated by TLC plate detection. The mixture was passed through a short silica gel column and chloroform was used as the eluent. The mixture was recrystallized to obtain compound 3 (612 mg, yield 80%).

[0057] (3) Under argon, compound 3 (600 mg, 0.6 mmol), 50 ml of ultra-dry tetrahydrofuran (THF) and 10 ml of ultra-dry triethylamine (NEt3) were added to a two-necked bottle, and then 63 mg (0.15 eq) of bis(triphenylphosphine)palladium dichloride and 17 mg (0.15 eq) of cuprous iodide were added. After argon was passed for 10 min, triisopropylsilyl acetylene was injected with a long needle, and the mixture was heated to reflux at 65° C. for 24 hours under light-proof conditions. After the reaction was completed, the solvent was dried by rotary evaporation, and the mixture was purified by silica gel chromatography using petroleum ether and dichloromethane as eluents, and recrystallized from chloroform and methanol to obtain compound 4 as a green solid (411 mg, yield 49%).

[0058] (4) Compound 4 (400 mg, 0.28 mmol) was dissolved in 10 mL of THF, and tetrabutylammonium fluoride solution (TBAF) (0.8 mL, 1 M in THF) was added. The mixture was reacted at room temperature for 5 min, and water was added to terminate the reaction. After post-treatment, the mixture was extracted with water / chloroform and dried to obtain compound 5, which was directly used in the next step.

[0059] (5) Compound 5 (0.14 mmol) and compound EHDPP (506 mg, 0.84 mmol) (purchased from Nanjing Zhiyan Technology Co., Ltd.) were added to a 100 mL double-necked round-bottom flask under argon protection, dissolved in 20 mL THF and 10 ml Et3N ultra-dry solvent, and then tetrakis(triphenylphosphine)palladium (24.3 mg, 0.021 mmol) and cuprous iodide (4 mg, 0.021 mmol) were added. The reaction system was ventilated three times and reacted at 65°C in the dark for 72 hours. After the reaction was completed, the mixture was dried by rotation, and the mixture was passed through a silica gel column using petroleum ether and dichloromethane as eluents, and GPC column chromatography was performed using THF as an eluent, and then recrystallized from chloroform methanol to obtain the final product EHDPP-Por (272 mg, yield 68%). 1H NMR (400MHz, CDCl3) δ8.92 (dd, J = 7.9, 3.7Hz, 8H), 8.60 (s, 4H), 8.12 (d, J = 7.0Hz, 8H), 7.78 (t, J = 7.4Hz, 4H), 7.70 (t, J = 6.8Hz, 8H), 7.62 (d, J = 5.0Hz, 4H), 7.29 (d, J = 4.1Hz, 4H), 7.24 (d, J = 4.9Hz, 4H), 4.02 (d, J = 7.7Hz, 16H), 1.96-1.79 (m, 8H), 1.39-1.19 (m, 64H), 0.85 (m, J = 14.0, 9.0, 4.8Hz, 48H), H NMR spectrum see Figure 1 .

[0060] Matrix-assisted laser desorption ionization time-of-flight mass spectrometry: experimental value 2864.4; calculated value C 172 H 180 N 12 O8S8Zn2865.27, see Figure 2 .

[0061] The porphyrin organic small molecule photovoltaic material prepared in this example is dissolved in chloroform solution at a concentration of (10 -5 -10 -4 mol / L), the UV-visible absorption spectrum of the obtained chloroform solution is shown in Figure 5 .

[0062] The porphyrin organic small molecule photovoltaic material prepared in this example was prepared into a thin film with a thickness of about 70 nm by spin coating. The ultraviolet-visible absorption spectrum of the thin film is shown in FIG. Figure 5 .

[0063] Using the porphyrin molecules of this example as donor materials and small molecule Y6 (CAS: 2304444-49-1) as acceptor materials, a positive device was prepared to study photovoltaic performance. The structure of the device is ITO / PEDOT:PSS / active layer / PFN-Br / Ag, and the mass ratio of the active layer to the acceptor is 1:0.9. The current-voltage curve (JV curve) under illumination is shown in FIG. Figure 7 The photoelectric conversion efficiency of the prepared device is 5.62%, and the short-circuit current is 15.66 mA / cm 2 , the open circuit voltage is 0.78V and the fill factor is 45.98%.

[0064] The photoelectric conversion efficiency achieved by the heterojunction battery prepared in this embodiment is the highest photoelectric conversion efficiency achieved by optimizing the donor-acceptor ratio, using an active layer material prepared with a donor-acceptor mass ratio of 1:0.9, and performing thermal annealing.

[0065] Example 2

[0066] Preparation of BODPP-Por molecule: R is H atom, and A unit is 2-butyloctyl substituted diketopyrrolopyrrole (BODPP).

[0067]

[0068] Under argon protection, compound 5 (0.14mmol) and compound BODPP (601mg, 0.84mmol) (purchased from Nanjing Zhiyan Technology Co., Ltd.) were added to a 100mL double-mouthed round-bottom flask, dissolved with 20mL THF and 10ml Et3N ultra-dry solvent, and then tetrakis(triphenylphosphine)palladium (24.3mg, 0.021mmol) and cuprous iodide (4mg, 0.021mmol) were added. After the reaction system was ventilated three times, it was reacted at 65°C in the dark for 72 hours. After the reaction was completed, it was spin-dried, and a silica gel column was used as an eluent with petroleum ether and dichloromethane, and GPC column chromatography was performed using THF as an eluent, and then recrystallized from chloroform methanol to obtain the final product BODPP-Por (301mg, 65% yield). 1H NMR (500 MHz, CDCl3) δ 8.92-8.87 (m, 8H), 8.59 (s, 4H), 8.12 (d, J = 6.9 Hz, 8H), 7.79 (t, J = 7.6 Hz, 4H), 7.71 (t, J = 7.5 Hz, 8H), 7.61 (dd, J = 5.0, 0.9 Hz, 4H), 7.28 (d, J = 4.7 Hz, 4H), 7.24 (d, J = 4.9 Hz, 4H), 4.02 (t, J = 6.6 Hz, 16H), 1.94 (m, J = 24.0 Hz, 8H), 1.32-1.17 (m, 128H), 0.85-0.74 (m, 48H), H NMR spectrum see Figure 3 .

[0069] Matrix-assisted laser desorption ionization time-of-flight mass spectrometry: experimental value 3314.4; calculated value C 204 H 244 N 12 O8S8Zn3314.13, see Figure 4 .

[0070] The donor photovoltaic material prepared in this example was dissolved in a chloroform solution with a mass concentration of (10 -5 -10 - 4 mol / L), the UV-visible absorption spectrum of the obtained chloroform solution is shown in Figure 6 .

[0071] The donor photovoltaic material prepared in this example was prepared into a thin film by spin coating, and the film thickness was about 70nm. The ultraviolet-visible absorption spectrum of the thin film was shown in FIG. Figure 6 .

[0072] Using the porphyrin molecule of this example as the donor material and the small molecule Y6 as the acceptor material, a positive device was prepared to study the photovoltaic performance. The structure of the device is ITO / PEDOT:PSS / active layer / PFN-Br / Ag, and the mass ratio of the active layer to the acceptor is 1:0.9. The JV curve under illumination is shown in FIG. Figure 7 The photoelectric conversion efficiency of the prepared device is 6.21%, and the short-circuit current is 16.72 mA / cm 2 , the open circuit voltage is 0.79V and the fill factor is 47.01%.

[0073] The photoelectric conversion efficiency achieved by the heterojunction battery prepared in this embodiment is the highest photoelectric conversion efficiency achieved by optimizing the donor-acceptor ratio, using an active layer material prepared with a donor-acceptor mass ratio of 1:0.9, and performing thermal annealing.

[0074] Through the small molecule donors prepared in Example 1 and Example 2, it can be seen that the two donor photovoltaic materials have similar absorption. In the solution, the absorption peaks of the Soret band and the Q band are located at about 480nm and 700nm, respectively, indicating that there is intramolecular charge transfer between the porphyrin core and the DPP end group, and the absorption peak of about 570nm is attributed to the absorption of the DPP unit; in the thin film state, the absorption of the Soret band and the Q band becomes stronger, the absorption has a red shift of about 20nm, and the absorption peak is broadened, which is attributed to the enhancement of molecular stacking in the solid state. The absorption margin of the molecule EHDPP-Por in Example 1 is 796nm, and the absorption margin of the molecule BODPP-Por in Example 2 is 789nm.

[0075] By comparing the efficiency of the heterojunction batteries prepared in Example 1 and Example 2 with Y6, it can be seen that the molecule BODPP-Por has a higher open circuit voltage, short circuit current and fill factor than EHDPP-Por, and therefore has a higher PCE value, extends the alkyl side chain, and optimizes the performance of the material.

[0076] The synthesis methods of other small molecule photovoltaic materials based on porphyrin with four β-position substitutions to connect the energy-absorbing units are similar to the above method and will not be repeated here.

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A type of β-tetrasubstituted porphyrin organic photovoltaic material, characterized in that: It has the following chemical structure: Wherein, A is an electron-withdrawing group having a conjugated structure; and R is hydrogen or an alkyl or alkoxy group having 1 to 4 carbon atoms.

2. The β-position tetrasubstituted porphyrin organic photovoltaic material according to claim 1, characterized in that: The specific structure of A is at least one of the following:

3. The β-tetrasubstituted porphyrin organic photovoltaic material according to claim 1, characterized in that: The R is at least one of a hydrogen atom, a methyl group, a methoxy group, an isopropyl group, an n-butyl group, and a tert-butyl group.

4. A method for preparing a β-position tetrasubstituted porphyrin organic photovoltaic material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) dissolving compound I in an organic solvent and reacting with N-bromosuccinimide at 60-70° C. for 3-5 hours to obtain a compound represented by formula II; (2) dissolving compound II in an organic solvent, adding zinc acetate and reacting at 60-70° C. for 8-15 hours to obtain compound III; (3) dissolving compound III in an organic solvent, adding triisopropylsilyl acetylene, reacting at 60-70° C. for 18-30 hours in the presence of a catalyst, to obtain an intermediate product IV; (4) The intermediate product IV is dissolved in an organic solvent, and a tetrabutylammonium fluoride solution is added at room temperature and stirred for reaction for 5-30 minutes. The reaction is terminated, and the product is extracted, spin-dried, and directly used for the next reaction; (5) heating and refluxing the product after spin drying in step (4) and the acceptor molecule pyrrolopyrrole diketo monomer of A in an organic solvent for 48-72 hours under the action of a catalyst to obtain the β-tetrasubstituted porphyrin organic photovoltaic material; The definitions of R and A are consistent with those in any one of claims 1-3.

5. The method for preparing a β-position tetrasubstituted porphyrin organic photovoltaic material according to claim 4, characterized in that: The organic solvent in step (1) is at least one of chloroform and dichloromethane; The molar ratio of compound I to N-bromosuccinimide in step (1) is 1:5-1:

7.

6. The method for preparing a β-tetrasubstituted porphyrin organic photovoltaic material according to claim 4, characterized in that: The organic solvent in step (2) is a mixed solution of chloroform and methanol; the molar amount of chloroform is 3000-4000 times the molar amount of compound (II), and the volume ratio of chloroform to methanol is 6:1-3:1; The molar ratio of compound (II) to zinc acetate in step (2) is 1:5-1:

8.

7. The method for preparing a β-position tetrasubstituted porphyrin organic photovoltaic material according to claim 4, characterized in that: The organic solvent in step (3) is a mixed solvent of tetrahydrofuran and triethylamine; the molar amount of tetrahydrofuran is 1000-3000 times the molar amount of compound (III), and the volume ratio of tetrahydrofuran to triethylamine is 2:1-5:1; In step (3), the molar ratio of compound III to triisopropylsilyl acetylene is 1:8-1:12; The catalyst in step (3) is bis(triphenylphosphine)palladium dichloride and cuprous iodide; the molar amount of both is 0.15 times the molar amount of compound (III).

8. The method for preparing a β-tetrasubstituted porphyrin organic photovoltaic material according to claim 4, characterized in that: The organic solvent in step (4) is tetrahydrofuran; the molar amount of tetrahydrofuran is 1000-3000 times the molar amount of the intermediate product IV; The molar ratio of the intermediate product IV to tetrabutylammonium fluoride in step (4) is 1:6-1:

8.

9. The method for preparing a β-tetrasubstituted porphyrin organic photovoltaic material according to claim 4, characterized in that: The molar ratio of the spin-dried product in step (5) to the diketopyrrolidine monomer of the receptor molecule A is 1:6-1:8; The organic solvent in step (5) is a mixed solvent of tetrahydrofuran and triethylamine; the molar amount of tetrahydrofuran is 1000-3000 times the molar amount of the spin-dried product, and the volume ratio of tetrahydrofuran to triethylamine is 2:1-5:1; The catalyst in step (5) is tetrakis(triphenylphosphine)palladium and cuprous iodide; the molar amount of both is 0.15 times the molar amount of the spin-dried product.

10. Use of the β-tetrasubstituted porphyrin organic photovoltaic material according to any one of claims 1 to 3 in an organic solar cell.

Citation Information

Patent Citations

  • Porphyrin organic small molecular photovoltaic material and preparation method thereof

    CN103724355A

  • Multiporphyrin organic small molecule photovoltaic material and preparation method thereof

    CN107312021A

  • Porphyrin organic small molecular photovoltaic material as well as preparation method and application thereof

    CN107344948A

  • Asymmetrical porphyrin organic micromolecular cathode interface material and preparation method and application thereof

    CN108516978A

  • Efficient ternary organic solar cell based on porphyrin material and preparation method thereof