Epoxy resin solid plastic body and preparation method thereof

The combined transesterification catalyst improves the catalytic efficiency of epoxy resin, solves the problem that traditional thermosetting epoxy resin is difficult to recycle, realizes the recyclability, repeatable molding and degradability of epoxy resin solid plastics, and provides new Recycling pathways.

CN118791708AActive Publication Date: 2024-10-18DONGHUA UNIV

Patent Information

Application Number
CN202411037781.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-18
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Traditional thermosetting epoxy resins are difficult to recycle and cannot be molded repeatedly, and the existing ester bond dynamic exchange catalysts have low catalytic efficiency, especially when containing curing accelerators, their activity is reduced or ineffective.

Method used

A combined transesterification catalyst is used, which is composed of a main catalyst and a cocatalyst, and its mass ratio is controlled to prepare epoxy resin solid plastics, improve catalytic efficiency, and realize dynamic transesterification reaction.

Benefits of technology

The catalytic efficiency of the transesterification catalyst is significantly improved, and the prepared epoxy resin solid plastic body has excellent properties of traditional thermosetting properties, and also has the advantages of being recyclable, remoldable and degradable, providing a new way of thermosetting epoxy resin materials. Recovery and recycling pathways.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791708A_ABST
    Figure CN118791708A_ABST
Patent Text Reader

Abstract

The invention provides an epoxy resin solid plastic body and a preparation method thereof, and belongs to the technical field of thermosetting epoxy resin modification. The epoxy resin solid plastic body is prepared from epoxy resin, an anhydride curing agent, a curing accelerator and a combined ester exchange catalyst, wherein the mass ratio of the epoxy resin to the anhydride curing agent to the curing accelerator to the combined ester exchange catalyst is (30-50): (30-50): (0.1-2): (1-10); the combined ester exchange catalyst consists of a main catalyst and a cocatalyst, wherein the mass ratio of the main catalyst to the cocatalyst is 1: (0.1-0.5). The prepared epoxy resin solid plastic body not only has the excellent performance of traditional thermosetting epoxy resin, but also has the advantages of being recyclable, capable of being repeatedly formed, degradable and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermosetting epoxy resin modification, and in particular to an epoxy resin solid plastic and a preparation method thereof. Background Art

[0002] In the field of materials science, thermosetting epoxy resins are widely used in electronics, wind turbine blades, aerospace, automobile manufacturing and many other fields due to their excellent physical and chemical properties, such as high strength, high heat resistance, good electrical insulation and chemical stability. However, while the three-dimensional cross-linked structure of thermosetting epoxy resins gives them excellent performance, it also makes them difficult to recycle and reuse after their service life expires. Traditional recycling methods, such as mechanical recycling and pyrolysis recycling, often have disadvantages such as low efficiency, high energy consumption and high environmental pollution. In addition, the performance of the recycled epoxy resin materials is severely reduced and cannot meet the needs of recycling.

[0003] In recent years, as the concepts of sustainable development, circular economy and environmental protection have become more popular, researchers have begun to seek more environmentally friendly and efficient methods for recycling thermosetting epoxy resins. Among them, dynamic transesterification reaction, as a potential reversible crosslinking reaction, has attracted widespread attention. In 2011, Leibler et al. in France added zinc acetylacetonate to bisphenol A epoxy resin and cured it with unsaturated dibasic / tribasic carboxylic acids, discovered the dynamic covalent bond exchange mechanism and defined T v (Topological transition temperature), below which the resin exhibits the characteristics of traditional thermosetting resins, above which a dynamic exchange reaction occurs, and the material exhibits the characteristics of thermoplastic resins, thereby giving it the characteristics of repeatable molding and recycling. Leibler et al. named this material with both thermosetting and thermoplastic properties vitrimer, which is translated into Chinese as glass-like polymer or solid plastic material according to its physical meaning. Based on the differences in dynamic covalent bonds in the cross-linked network, solid plastic materials based on ester bonds, imine bonds, disulfide bonds, borate bonds, etc. have been developed.

[0004] Although researchers have developed epoxy resins based on the above-mentioned dynamic bond systems, most of them have too low glass transition temperatures and their mechanical strength cannot meet the needs of use. There is still a long way to go before they can be truly industrialized and commercialized. Since the most commonly used amine-cured epoxy resins do not contain covalent bonds with dynamic exchange potential, most of the epoxy resins currently containing dynamically exchangeable ester bonds are thermosetting epoxy resins based on epoxy anhydride systems, of which bisphenol A and bisphenol F epoxy resins account for the largest proportion, and the anhydride curing agent is methyl tetra / hexahydrophthalic anhydride. This type of epoxy resin is also widely used in liquid molding of fiber-reinforced composite materials due to its low viscosity characteristics, such as infusion, winding, pultrusion and wet molding. Typical ester bond dynamic exchange catalysts include zinc acetylacetonate, zinc acetate, 1,5,7-triazidebicyclo[4.4.0]dec-5-ene (TBD), triethanolamine, triphenylphosphine, titanate, imidazole compounds, etc. However, these catalysts, whether used alone or in combination, generally have the disadvantages of low catalytic efficiency and slow relaxation rate, especially when such anhydride-cured epoxy resin systems contain a curing accelerator, the chemical interference between the above-mentioned ester bond dynamic exchange catalyst and the curing accelerator causes the activity of the ester exchange catalyst to decrease or become completely ineffective. It is of great significance to study an epoxy resin solid plastic and a preparation method thereof, which can effectively catalyze the dynamic ester exchange reaction using a combined ester exchange catalyst in the presence of a curing accelerator. Summary of the invention

[0005] The object of the present invention is to provide an epoxy resin solid plastic and a preparation method thereof, so as to solve the problem that the traditional thermosetting epoxy resin in the prior art is difficult to recycle and cannot be repeatedly molded.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides an epoxy resin solid plastic, which is made of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst, wherein the mass ratio of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst is 30-50:30-50:0.1-2:1-10; the combined ester exchange catalyst is composed of a main catalyst and a co-catalyst, wherein the mass ratio of the main catalyst to the co-catalyst is 1:0.1-0.5.

[0008] Preferably, the epoxy resin comprises a glycidyl ether epoxy resin, a glycidyl ester epoxy resin, a glycidyl amine epoxy resin, an alicyclic epoxy resin or an epoxidized olefin epoxy resin.

[0009] Preferably, the acid anhydride curing agent comprises aromatic anhydride, aliphatic anhydride, alicyclic anhydride or halogen-containing anhydride; the curing accelerator comprises one or more of 2,4,6-tris(dimethylaminomethyl)phenol, chromium octoate, benzyldimethylamine, imidazole and acetylacetone metal salt.

[0010] Preferably, the main catalyst comprises one or more of zinc methacrylate, zinc acetylacetonate, zinc acetate, triphenylphosphine and titanate; and the co-catalyst comprises benzyl quaternary ammonium salt or alkyl quaternary ammonium salt.

[0011] Preferably, the chemical formula of the benzyl quaternary ammonium salt is C n H 2n-4 R1N, wherein n is an integer greater than or equal to 10, R1 is F, Cl, Br, I; the chemical formula of the alkyl quaternary ammonium salt is C m H 2m+4 R2N, wherein m is an integer greater than or equal to 4, and R2 is F, Cl, Br, or I.

[0012] The present invention provides a method for preparing the epoxy resin solid plastic body described above, comprising the following steps:

[0013] (1) mixing a co-catalyst, a main catalyst and an acid anhydride curing agent to obtain a mixed solution;

[0014] (2) The epoxy resin, the curing accelerator and the mixed solution of step (1) are mixed and then degassed and cured in sequence to obtain an epoxy resin solid plastic.

[0015] Preferably, in step (1), the co-catalyst and the acid anhydride curing agent are first mixed, and then the main catalyst is added.

[0016] Preferably, in step (2), the rotation speed of the degassing treatment is 1200 to 1800 rpm, and the time of the degassing treatment is 2 to 6 minutes.

[0017] Preferably, in step (2), the curing comprises a first curing, a second curing and a third curing.

[0018] Preferably, the temperature of the first curing is 80-100°C, and the time of the first curing is 0.5-1.5h; the temperature of the second curing is 130-150°C, and the time of the second curing is 0.5-1.5h; the temperature of the third curing is 190-210°C, and the time of the third curing is 0.5-1.5h.

[0019] Beneficial effects of the present invention:

[0020] (1) Compared with the traditional single-type ester exchange catalyst, the present invention adopts a combined ester exchange catalyst to prepare epoxy resin solid plastic. The combined ester exchange catalyst is composed of a main catalyst and a co-catalyst. By controlling the mass ratio of the main catalyst and the co-catalyst, the catalytic efficiency of the combined ester exchange catalyst is significantly improved. In particular, in the presence of a curing accelerator, it can also effectively catalyze the dynamic ester exchange reaction.

[0021] (2) The epoxy resin solid plastic obtained by the present invention not only has the excellent properties of traditional thermosetting epoxy resin but also has the advantages of being recyclable, re-moldable, and biodegradable, thus providing a new way for the recycling and reuse of thermosetting epoxy resin materials and having broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The stress relaxation curves of the epoxy resin solid plastics prepared in Examples 1 to 3 and Comparative Examples 1 to 6 at 250° C.

[0023] Figure 2 The dynamic thermomechanical analysis diagram of the epoxy resin solid plastic of Example 1 and the dynamic thermomechanical analysis diagram of the sample after repeated molding;

[0024] Figure 3 This is a diagram of a repeated molding experiment of an epoxy resin solid plastic body of Example 1;

[0025] Figure 4 This is a degradation experiment diagram of the epoxy resin solid plastic of Example 1. DETAILED DESCRIPTION

[0026] The invention provides an epoxy resin solid plastic, which is made of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst, wherein the mass ratio of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst is 30-50:30-50:0.1-2:1-10; the combined ester exchange catalyst is composed of a main catalyst and a co-catalyst, wherein the mass ratio of the main catalyst to the co-catalyst is 1:0.1-0.5.

[0027] In the present invention, the mass ratio of the epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst is preferably 35-45:35-45:0.5-1.5:1.5-8, and more preferably 40-42:36-40:0.5-0.8:1.64-5; the mass ratio of the main catalyst and the co-catalyst is preferably 1:0.2-0.4, and more preferably 1:0.3.

[0028] In the present invention, the mass ratio of the main catalyst to the co-catalyst has good catalytic efficiency within a certain range, and a decrease or increase in the mass ratio will lead to a decrease in the catalytic efficiency.

[0029] In the present invention, the epoxy resin comprises a glycidyl ether epoxy resin, a glycidyl ester epoxy resin, a glycidyl amine epoxy resin, an alicyclic epoxy resin or an epoxidized olefin epoxy resin, preferably a glycidyl ether epoxy resin, a glycidyl ester epoxy resin or a glycidyl amine epoxy resin, and further preferably a glycidyl ether epoxy resin or a glycidyl ester epoxy resin.

[0030] In the present invention, the glycidyl ether epoxy resin is preferably bisphenol A epoxy resin, bisphenol F epoxy resin or bisphenol S epoxy resin, more preferably bisphenol A epoxy resin; the glycidyl ester epoxy resin is preferably diglycidyl phthalate, diglycidyl tetrahydrophthalate or triglycidyl trimellitate, more preferably diglycidyl phthalate; the glycidyl amine epoxy resin is preferably cyanuric acid epoxy resin or p-aminophenol epoxy resin, preferably p-aminophenol epoxy resin; the alicyclic epoxy resin is preferably dicyclopentadiene dioxide epoxy resin or dicyclopentenyl ether dioxide, more preferably dicyclopentenyl ether dioxide; the epoxidized olefin epoxy resin is preferably epoxidized polybutadiene.

[0031] In the present invention, the acid anhydride curing agent comprises aromatic anhydride, aliphatic anhydride, alicyclic anhydride or halogen-containing anhydride; the aromatic anhydride is preferably phthalic anhydride, trimellitic anhydride or pyrophthalic anhydride; the aliphatic anhydride is preferably polyadipic anhydride, polyazelaic anhydride or polyfumaric anhydride; the alicyclic anhydride is preferably methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride or glutaric anhydride, more preferably methyltetrahydrophthalic anhydride; the halogen-containing anhydride is preferably hexachloroendimethylenetetrahydrophthalic anhydride or 1,4,5,6-tetrabromophthalic anhydride.

[0032] In the present invention, the curing accelerator comprises one or more of 2,4,6-tris(dimethylaminomethyl)phenol, chromium octoate, benzyldimethylamine, imidazole and acetylacetone metal salt, preferably one or more of 2,4,6-tris(dimethylaminomethyl)phenol, chromium octoate and benzyldimethylamine, and more preferably 2,4,6-tris(dimethylaminomethyl)phenol.

[0033] In the present invention, the main catalyst comprises one or more of zinc methacrylate, zinc acetylacetonate, zinc acetate, triphenyl phosphine and titanate, preferably one or more of zinc methacrylate, zinc acetylacetonate and zinc acetate, and more preferably zinc methacrylate; the co-catalyst comprises benzyl quaternary ammonium salt or alkyl quaternary ammonium salt.

[0034] In the present invention, the chemical formula of the benzyl quaternary ammonium salt is C n H 2n-4 R1N, wherein n is an integer greater than or equal to 10, preferably 10, 13, 16, 19, 22, 25; R1 is F, Cl, Br, I, preferably Cl, Br; the chemical formula of the alkyl quaternary ammonium salt is C m H 2m+4 R2N, wherein m is an integer greater than or equal to 4, preferably 4, 8, 12, 16, 20, 24, and R2 is F, Cl, Br, I, preferably Cl, Br. The cocatalyst used in the embodiment of the present invention is benzyltriethylammonium chloride.

[0035] The present invention provides a method for preparing the epoxy resin solid plastic body described above, comprising the following steps:

[0036] (1) mixing a co-catalyst, a main catalyst and an acid anhydride curing agent to obtain a mixed solution;

[0037] (2) The epoxy resin, the curing accelerator and the mixed solution of step (1) are mixed and then degassed and cured in sequence to obtain an epoxy resin solid plastic.

[0038] In the present invention, in the step (1), the co-catalyst and the acid anhydride curing agent are first mixed, and then the main catalyst is added.

[0039] In the present invention, the co-catalyst and the anhydride curing agent are first mixed, and then the main catalyst is added, and the epoxy resin and the curing accelerator are added to the obtained mixed solution, which can improve the mechanical properties of the epoxy resin solid plastic and the catalytic efficiency of the catalyst. The co-catalyst and the anhydride curing agent are mixed to obtain the mixed solution 1, the main catalyst and the epoxy resin are mixed to obtain the mixed solution 2, and finally the mixed solution 1, the mixed solution 2 and the curing accelerator are mixed, which is different from the order of adding materials in the present application, which will lead to a decrease in the catalytic performance of the catalyst and a decrease in the performance of the product.

[0040] In the present invention, in the step (2), the rotation speed of the degassing treatment is 1200-1800 rpm, preferably 1200 rpm, 1400 rpm, 1600 rpm, 1800 rpm, and more preferably 1600 rpm, 1800 rpm; the time of the degassing treatment is 2-6 min, preferably 3-5 min, and more preferably 4 min.

[0041] In the present invention, in the step (2), the curing includes a first curing, a second curing and a third curing.

[0042] In the present invention, the temperature of the first curing is 80-100°C, preferably 85-95°C, and more preferably 90°C, and the time of the first curing is 0.5-1.5h, and more preferably 1h; the temperature of the second curing is 130-150°C, preferably 135-145°C, and more preferably 130°C, and the time of the second curing is 0.5-1.5h, and more preferably 1h; the temperature of the third curing is 190-210°C, preferably 195-205°C, and more preferably 200°C, and the time of the third curing is 0.5-1.5h, and more preferably 1h.

[0043] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0044] Example 1

[0045] 18.05 g of methyltetrahydrophthalic anhydride was placed in a beaker, 0.37 g of benzyltriethylammonium chloride was added, the beaker was heated to 100° C., and the mixture was stirred at 500 rpm for 10 min at 100° C. until the benzyltriethylammonium chloride was completely dissolved in the methyltetrahydrophthalic anhydride. After cooling to room temperature, 1.27 g of zinc methacrylate was added, the beaker was heated to 100° C., and the mixture was stirred at 600 rpm for 10 min at this temperature until the zinc methacrylate was completely dissolved. The mixture was cooled to room temperature to obtain a mixed solution.

[0046] 20.00g of bisphenol A epoxy resin and 0.5g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator are added to the above mixed solution, stirred evenly, and placed in a vacuum degassing machine for degassing at a speed of 1800rpm for 4 minutes. The degassed resin liquid is poured into a mold, and then placed in an oven for curing. The process parameters of the curing process are: the first curing temperature is 90°C and the time is 1h; the second curing temperature is 140°C and the time is 1h; the third curing temperature is 200°C and the time is 1h, and an epoxy resin solid plastic is obtained.

[0047] Example 2

[0048] 18.05 g of phthalic anhydride was placed in a beaker, 0.3 g of tetraethylammonium chloride was added, the beaker was heated to 100° C., and the mixture was stirred at 500 rpm for 10 min at 100° C. until the tetraethylammonium chloride was completely dissolved in the phthalic anhydride. After cooling to room temperature, 1.86 g of zinc acetylacetonate was added, the beaker was heated to 100° C., and the mixture was stirred at 600 rpm for 10 min at this temperature until the zinc acetylacetonate was completely dissolved. The mixture was cooled to room temperature to obtain a mixed solution.

[0049] 25.00g of diglycidyl phthalate and 0.5g of benzyldimethylamine curing accelerator are added to the above mixed solution, and after stirring evenly, it is placed in a vacuum degassing machine at a speed of 1600rpm for degassing for 5 minutes, and the degassed resin liquid is poured into the mold, and then placed in an oven for curing. The process parameters of the curing process are: the first curing temperature is 80°C, and the time is 1.5h; the second curing temperature is 130°C, and the time is 1.5h; the third curing temperature is 190°C, and the time is 1.5h, to obtain an epoxy resin solid plastic.

[0050] Example 3

[0051] Place 15 g of hexachloromethylenetetrahydrophthalic anhydride in a beaker, add 0.5 g of benzyltriethylammonium bromide, heat the beaker to 100°C, stir at 500 rpm for 10 min at 100°C until benzyltriethylammonium bromide is completely dissolved in the hexachloromethylenetetrahydrophthalic anhydride, cool to room temperature, add 1.29 g of zinc acetate, heat the beaker to 100°C again, stir at 600 rpm for 10 min at this temperature until the zinc acetate is completely dissolved, cool to room temperature to obtain a mixed solution.

[0052] 15.00g of cyanuric acid epoxy resin and 0.3g of chromium octanoate curing accelerator are added to the above mixed solution, and after stirring evenly, it is placed in a vacuum degassing machine at a speed of 1700rpm for degassing for 3 minutes, and the degassed resin liquid is poured into a mold, and then placed in an oven for curing. The process parameters of the curing process are: the first curing temperature is 100°C, and the time is 0.5h; the second curing temperature is 150°C, and the time is 0.5h; the third curing temperature is 210°C, and the time is 0.5h, to obtain an epoxy resin solid plastic.

[0053] Comparative Example 1

[0054] 1.29 g of zinc acetate and 20.00 g of bisphenol A epoxy resin were mixed, heated to 140° C., stirred at 500 rpm for 10 min at this temperature until the zinc acetate was completely dissolved, and cooled to room temperature to obtain a mixed solution 1.

[0055] 18.05 g of methyltetrahydrophthalic anhydride and 0.5 g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator were added to the mixed solution 1, and after stirring evenly, the mixture was placed in a vacuum degassing machine and degassed at a speed of 1800 rpm for 4 minutes. The degassed resin liquid was poured into a mold, and then placed in an oven for curing. The process parameters of the curing process were: the first curing temperature was 90° C. and the time was 1 hour; the second curing temperature was 140° C. and the time was 1 hour; the third curing temperature was 200° C. and the time was 1 hour, and an epoxy resin-based material was obtained.

[0056] Comparative Example 2

[0057] 1.86 g of zinc acetylacetonate and 20.00 g of bisphenol A epoxy resin were mixed, heated to 140° C., stirred at 500 rpm for 10 min at this temperature until the zinc acetylacetonate was completely dissolved, and cooled to room temperature to obtain a mixed solution 1.

[0058] 18.05 g of methyltetrahydrophthalic anhydride and 0.5 g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator were added to the mixed solution 1, and after stirring evenly, the mixture was placed in a vacuum degassing machine and degassed at a speed of 1800 rpm for 4 minutes. The degassed resin liquid was poured into a mold, and then placed in an oven for curing. The process parameters of the curing process were: the first curing temperature was 90° C. and the time was 1 hour; the second curing temperature was 140° C. and the time was 1 hour; the third curing temperature was 200° C. and the time was 1 hour, and an epoxy resin-based material was obtained.

[0059] Comparative Example 3

[0060] 18.05g of methyltetrahydrophthalic anhydride was placed in a beaker, 0.37g of benzyltriethylammonium chloride was added, the beaker was heated to 100°C, and the mixture was stirred at 500rpm for 10min at 100°C until the benzyltriethylammonium chloride was completely dissolved in the methyltetrahydrophthalic anhydride, and the mixture was cooled to room temperature, 20.00g of bisphenol A epoxy resin and 0.5g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator were added, and the mixture was placed in a vacuum degassing machine for degassing at 1800rpm for 4min after stirring. The degassed resin liquid was poured into a mold, and then placed in an oven for curing. The process parameters of the curing process were as follows: the temperature of the first curing was 90°C and the time was 1h; the temperature of the second curing was 140°C and the time was 1h; the temperature of the third curing was 200°C and the time was 1h, and an epoxy resin-based material was obtained.

[0061] Comparative Example 4

[0062] 18.05g of methyltetrahydrophthalic anhydride was placed in a beaker, 1.27g of zinc methacrylate was added, the beaker was heated to 100°C, and the mixture was stirred at 600rpm for 10min at 100°C until the zinc methacrylate was completely dissolved in the methyltetrahydrophthalic anhydride, and the mixture was cooled to room temperature, 20.00g of bisphenol A epoxy resin and 0.5g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator were added, and the mixture was placed in a vacuum degassing machine for degassing at 1800rpm for 4min after stirring evenly, the degassed resin liquid was poured into a mold, and then placed in an oven for curing, wherein the process parameters of the curing process were as follows: the temperature of the first curing was 90°C and the time was 1h; the temperature of the second curing was 140°C and the time was 1h; the temperature of the third curing was 200°C and the time was 1h, and an epoxy resin-based material was obtained.

[0063] Comparative Example 5

[0064] 18.05 g of methyltetrahydrophthalic anhydride was placed in a beaker, 0.12 g of benzyltriethylammonium chloride was added, the beaker was heated to 100° C., and the mixture was stirred at 500 rpm for 10 min at 100° C. until the benzyltriethylammonium chloride was completely dissolved in the methyltetrahydrophthalic anhydride. After cooling to room temperature, 1.27 g of zinc methacrylate was added, the beaker was heated to 100° C., and the mixture was stirred at 600 rpm for 10 min at this temperature until the zinc methacrylate was completely dissolved. The mixture was cooled to room temperature to obtain a mixed solution.

[0065] 20.00g of bisphenol A epoxy resin and 0.5g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator are added to the above mixed solution, stirred evenly, and placed in a vacuum degassing machine for degassing at a speed of 1800rpm for 4 minutes. The degassed resin liquid is poured into a mold, and then placed in an oven for curing. The process parameters of the curing process are: the first curing temperature is 90°C and the time is 1h; the second curing temperature is 140°C and the time is 1h; the third curing temperature is 200°C and the time is 1h, and an epoxy resin solid plastic is obtained.

[0066] Comparative Example 6

[0067] 18.05 g of methyltetrahydrophthalic anhydride was placed in a beaker, 0.7 g of benzyltriethylammonium chloride was added, the beaker was heated to 100° C., and the mixture was stirred at 500 rpm for 10 min at 100° C. until the benzyltriethylammonium chloride was completely dissolved in the methyltetrahydrophthalic anhydride. After cooling to room temperature, 1.27 g of zinc methacrylate was added, the beaker was heated to 100° C., and the mixture was stirred at 600 rpm for 10 min at this temperature until the zinc methacrylate was completely dissolved. The mixture was cooled to room temperature to obtain a mixed solution.

[0068] 20.00g of bisphenol A epoxy resin and 0.5g of 2,4,6-tris(dimethylaminomethyl)phenol curing accelerator are added to the above mixed solution, stirred evenly, and placed in a vacuum degassing machine for degassing at a speed of 1800rpm for 4 minutes. The degassed resin liquid is poured into a mold, and then placed in an oven for curing. The process parameters of the curing process are: the first curing temperature is 90°C and the time is 1h; the second curing temperature is 140°C and the time is 1h; the third curing temperature is 200°C and the time is 1h, and an epoxy resin solid plastic is obtained.

[0069] The raw material formulas of Examples 1 to 3 and Comparative Examples 1 to 6 are shown in Table 1 and Table 2 respectively:

[0070] Table 1 Raw material formula of Examples 1 to 3

[0071]

[0072] Note: In Examples 1 to 3 in Table 1, the epoxy resins are bisphenol A epoxy resin, diglycidyl phthalate epoxy resin, and cyanuric acid epoxy resin, respectively; the anhydride curing agents are methyltetrahydrophthalic anhydride, phthalic anhydride, and hexachloromethylenetetrahydrophthalic anhydride, respectively; the curing accelerators are 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, and chromium octanoate, respectively; the main catalysts are zinc methacrylate, zinc acetylacetonate, and zinc acetate, respectively; and the co-catalysts are benzyltriethylammonium chloride, tetraethylammonium chloride, and benzyltriethylammonium bromide, respectively.

[0073] Table 2 Raw material formula of comparative examples 1 to 6

[0074]

[0075] Note: In Table 2, 550E is bisphenol A epoxy resin, MTHPA is methyltetrahydrophthalic anhydride, TEBAC is benzyltriethylammonium chloride, C is 2,4,6-tris(dimethylaminomethyl)phenol, ZADM is zinc methacrylate, Zn(oAc)2 is zinc acetate, and Zn(acac)2 is zinc acetylacetonate.

[0076] The performance tests were performed on the epoxy resin solid plastics of Examples 1 to 3 and the epoxy resin-based materials of Comparative Examples 1 to 6:

[0077] (1) Stress relaxation test:

[0078] The stress relaxation effect of the cured epoxy resin casting was tested using an American TA Q800 dynamic mechanical analyzer (DMA). The sample size was 15mm×5mm×1mm. A tensile film fixture was used for the test. The test pre-tension was 0.001N, the fixed strain was 1%, the equilibrium time was 5min, and the test temperature was 250℃.

[0079] (2) Determination of thermomechanical properties:

[0080] The thermomechanical properties of the cured casting specimens were tested using the Q800 dynamic mechanical analyzer (DMA) from TA Instruments, USA. The storage modulus and the tangent of the loss angle were tested in tensile mode with a frequency of 20 Hz and a heating rate of 3 °C / min from room temperature to 200 °C. In order to ensure test consistency, the size of the test specimens was fixed at 15 mm × 5 mm × 1 mm.

[0081] (3) Repeated molding experiment:

[0082] The epoxy resin solid plastic obtained in Example 1 was cut into small pieces and put into a ball mill, and ball milled at a speed of 1200 rpm for 6 minutes to make it into powder. The powder was placed in a mold and hot-pressed at 240°C, 2 hours, and 7 MPa. The molding experiment process was repeated as shown in FIG. Figure 3 .

[0083] (4) Degradation experiment:

[0084] The epoxy resin solid plastic obtained in Example 1 was cut into strips with a size of 20 mm×10 mm×1 mm, placed in a transparent glass bottle filled with 25 g of ethylene glycol, and placed in an oven at a temperature of 190° C. for 12 hours.

[0085] Generally speaking, thermosetting polymer resins cannot be reprocessed and repeatedly molded because of their internal three-dimensional covalent bond cross-linked network structure, while the characteristic of solid plastic materials is that they can rearrange their molecular topology through dynamic covalent bond exchange reactions at a certain temperature so that the modulus drops to less than 1 / e of the initial modulus, giving the material the ability to be repeatedly molded. Stress relaxation experiments are also an important way to distinguish thermosetting materials from solid plastic materials. Figure 1 It can be seen that the epoxy resin-based materials prepared by using zinc methacrylate (Comparative Example 4) and benzyl triethyl ammonium chloride (Comparative Example 3) as catalysts alone cannot relax stress to 1 / e of the initial modulus, but when the two are combined in a certain proportion and used synergistically, the material can relax stress, that is, the modulus can be reduced to 1 / e of the initial modulus (Example 1). Compared with Comparative Example 3, the relaxation modulus of Comparative Example 4 is reduced more, so zinc methacrylate is determined as the main catalyst and benzyl triethyl ammonium chloride is determined as the co-catalyst. On the other hand, from Figure 1It can also be seen that the relaxation time of Example 1 at 250°C is only 18 minutes. Compared with Comparative Examples 1 and 2, the relaxation time of Example 1 is shorter, indicating that the combined catalyst composed of zinc methacrylate and benzyltriethylammonium chloride has a higher catalytic efficiency than the single-component catalysts of zinc acetate and zinc acetylacetonate of equal mass. It can be seen from Examples 2 and 3 and Comparative Examples 2 and 3 that adding a co-catalyst on the basis of using a single-component catalyst can achieve the effect of synergistic catalysis to improve the catalytic efficiency. In addition, from Figure 1 From the stress relaxation conditions of Example 1, Comparative Examples 5 and 6 at 250°C, the ratio of the main catalyst to the co-catalyst in Comparative Example 5 is less than 1:0.1, so the relaxation modulus cannot drop below the initial modulus 1 / e, while the ratio of the main catalyst to the co-catalyst in Comparative Example 6 is greater than 1:0.5. Although the modulus can relax to below the initial modulus 1 / e, its relaxation time of 37 min is doubled compared with that of Example 1 (relaxation time 18 min). Therefore, the combined catalyst needs to reach a certain ratio to have a catalytic effect and has the best catalytic efficiency within a certain range.

[0086] Figure 2 The thermomechanical properties of the epoxy resin solid plastic are shown in Figure 1. g is 146℃, and the T g 138℃, T g It only dropped by about 5%, indicating that the epoxy resin solid plastic after repeated molding still has good heat resistance. Figure 3 It can be seen from the figure that the epoxy resin solid plastic of Example 1 is an amber transparent solid. The resin strips after repeated hot pressing molding are no different from those before repeated molding and still have light transmittance, indicating that the epoxy resin solid plastic after adding the combined transesterification catalyst has very good repeatability. Figure 4 It can be seen that the epoxy resin solid plastic of Example 1 can be completely degraded into oligomers under the action of the small molecule solvent ethylene glycol, indicating that the epoxy resin solid plastic after adding the combined ester exchange catalyst has the property of being recyclable.

[0087] It can be seen from the above embodiments that the present invention provides an epoxy resin solid plastic and a preparation method thereof. The epoxy resin solid plastic of the present invention is made of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst, wherein the mass ratio of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst is 30-50:30-50:0.1-2:1-10; the combined ester exchange catalyst is composed of a main catalyst and a co-catalyst, wherein the mass ratio of the main catalyst to the co-catalyst is 1:0.1-0.5. The present invention significantly improves the catalytic efficiency of the combined ester exchange catalyst by controlling the mass ratio of the main catalyst and the co-catalyst, especially in the case of containing a curing accelerator, it can also effectively catalyze the dynamic ester exchange reaction. The epoxy resin solid plastic prepared by the present invention not only has the excellent properties of traditional thermosetting epoxy resins but also has the advantages of being recyclable, reproducible, and degradable.

[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An epoxy resin solid plastic, characterized in that: The epoxy resin solid plastic is made of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst, wherein the mass ratio of epoxy resin, anhydride curing agent, curing accelerator and combined ester exchange catalyst is 30-50:30-50:0.1-2:1-10; the combined ester exchange catalyst is composed of a main catalyst and a co-catalyst, wherein the mass ratio of the main catalyst to the co-catalyst is 1:0.1-0.

5.

2. The epoxy resin solid plastic according to claim 1, characterized in that: The epoxy resin includes glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin or epoxidized olefin epoxy resin.

3. The epoxy resin solid plastic according to claim 2, characterized in that: The acid anhydride curing agent comprises aromatic anhydride, aliphatic anhydride, alicyclic anhydride or halogen-containing anhydride; the curing accelerator comprises one or more of 2,4,6-tris(dimethylaminomethyl)phenol, chromium octanoate, benzyldimethylamine, imidazole and acetylacetone metal salt.

4. The epoxy resin solid plastic according to any one of claims 1 to 3, characterized in that: The main catalyst comprises one or more of zinc methacrylate, zinc acetylacetonate, zinc acetate, triphenylphosphine and titanate; the co-catalyst comprises benzyl quaternary ammonium salt or alkyl quaternary ammonium salt.

5. The epoxy resin solid plastic according to claim 4, characterized in that: The chemical formula of the benzyl quaternary ammonium salt is C n H 2n-4 R1N, wherein n is an integer greater than or equal to 10, R1 is F, Cl, Br, I; the chemical formula of the alkyl quaternary ammonium salt is C m H 2m+ 4R2N, wherein m is an integer greater than or equal to 4, and R2 is F, Cl, Br, or I.

6. The method for preparing the epoxy resin solid plastic according to any one of claims 1 to 5, characterized in that: The steps include: (1) mixing a co-catalyst, a main catalyst and an acid anhydride curing agent to obtain a mixed solution; (2) The epoxy resin, the curing accelerator and the mixed solution of step (1) are mixed and then degassed and cured in sequence to obtain an epoxy resin solid plastic.

7. The method for preparing an epoxy resin solid plastic according to claim 6, characterized in that: In the step (1), the co-catalyst and the acid anhydride curing agent are first mixed, and then the main catalyst is added.

8. The method for preparing an epoxy resin solid plastic according to claim 6 or 7, characterized in that: In the step (2), the rotation speed of the degassing treatment is 1200 to 1800 rpm, and the time of the degassing treatment is 2 to 6 minutes.

9. The method for preparing an epoxy resin solid plastic according to claim 8, characterized in that: In the step (2), the curing includes a first curing, a second curing and a third curing.

10. The method for preparing an epoxy resin solid plastic according to claim 9, characterized in that: The temperature of the first curing is 80-100°C, and the time of the first curing is 0.5-1.5h; the temperature of the second curing is 130-150°C, and the time of the second curing is 0.5-1.5h; the temperature of the third curing is 190-210°C, and the time of the third curing is 0.5-1.5h.

Citation Information

Patent Citations

  • Transesterification type dynamic transfer autocatalysis thermosetting resin as well as preparation method and application thereof

    CN113201117A

  • Application of covalent bond dynamic exchange catalyst and modified epoxy resin capable of being repeatedly formed, degraded and recycled

    CN114853984A

  • Epoxy compound and its production and photocurable resin composition

    JP1999071365A

  • Curable composition

    JP2019026800A

  • Process for curing epoxy resin anhydride blends at moderately elevated temperatures

    US4954196A

Cited By

  • Epoxy resin-based composite material capable of being repeatedly shaped, preparation method and repeated shaping method

    CN121086472A