Polymer elastomer and preparation method thereof
By adding aminosiloxane containing two amino groups as a cross-linking agent in the polymerization reaction of polyethylene glycol and dicarboxylic acid, the problem of poor mechanical properties of the polymerized elastomer is solved, and its mechanical strength and durability are improved. Abrasive, suitable for applications under high strain conditions.
Patent Information
- Application Number
- CN202411078068.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing polymeric elastomers suffer from poor mechanical properties, exhibiting low tensile strength, tear strength and abrasion resistance, limiting their use in demanding applications.
In the polymerization reaction of polyethylene glycol and dicarboxylic acid, aminosiloxane containing two amino groups is added as a cross-linking agent, and the reaction is carried out under nitrogen protection to generate ester bonds and amide bonds, thereby improving the mechanical strength of the polymerized elastomer. and wear resistance.
By introducing aminosiloxane, the flexibility and mechanical strength of the polymeric elastomer are improved, its ability to withstand high strain conditions is enhanced, and the wear resistance is improved through Si-O-Si chemical bonds.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer elastomers, and in particular to a polymer elastomer and a preparation method thereof. Background Art
[0002] Polymeric elastomers synthesized with polyethylene glycol (PEG) as raw material have good biocompatibility as well as low toxicity and immunogenicity, and are suitable for biomedical fields such as drug delivery and tissue engineering.
[0003] Polymer elastomers obtained simply by reacting dicarboxylic acids with diols exhibit low tensile strength, tear strength and wear resistance, which limits their use in certain high-demand applications. Summary of the invention
[0004] The problem in the prior art is that the mechanical properties of polymer elastomers produced by conventional methods are poor. In view of the above problems, the present invention provides a polymer elastomer, and its preparation method comprises the following steps:
[0005] Under nitrogen protection, dicarboxylic acid, polyethylene glycol, crosslinking agent and catalyst are mixed and stirred evenly, the temperature of the reaction system is raised to 160-180°C, stirred and reacted for 2 hours under normal pressure, and then stirred and reacted for 3 hours under negative pressure. During the reaction, the hydroxyl group in the reaction system reacts with the carboxyl group to form an ester bond, and the carboxyl group reacts with the amino group to form an amide bond. After the reaction is completed, a polymerized elastomer is obtained;
[0006] The crosslinking agent is aminosiloxane containing two amino groups.
[0007] Preferably, the catalyst is a mixture of stannous oxalate and a super strong solid acid.
[0008] Preferably, the mass ratio of stannous oxalate to super solid acid is 1:2.
[0009] Preferably, the super strong solid acid is aluminum silicate or lithium fluorozirconate.
[0010] Preferably, the catalyst is a mixture of stannous oxalate and an activated carbon-supported catalyst.
[0011] Preferably, the mass ratio of stannous oxalate to the activated carbon-supported catalyst is 1:1.
[0012] Preferably, the activated carbon-supported catalyst is palladium-supported activated carbon.
[0013] Preferably, the dicarboxylic acid includes one or a combination of two or more of 1,4-cyclohexanedicarboxylic acid, 1,1′-di(cyclohexyl)-4,4′-dicarboxylic acid, and decahydronaphthalene-2,6-dicarboxylic acid.
[0014] Preferably, the polyethylene glycol is PEG4000 or PEG6000.
[0015] Preferably, the aminosiloxane includes at least one of 1,3-bis(4-aminobutyl)tetramethyldisiloxane or aminopropyldimethylsilyl-terminated polydimethylsiloxane (CAS: 97917-34-5).
[0016] The present invention has the following beneficial effects:
[0017] (1) In the present invention, a cross-linking agent is added during the polymerization reaction of polyethylene glycol and dicarboxylic acid. The cross-linking agent is an aminosiloxane containing two amino groups, which can participate in the polymerization reaction of polyethylene glycol and dicarboxylic acid. The amino groups in the cross-linking agent undergo an amidation reaction with the carboxyl groups in the reaction system, thereby being introduced into the molecular structure of the elastomer in the form of a chemical bond. The aminopropyldimethylsilyl-terminated polydimethylsiloxane has better flexibility than other aminosiloxanes. The introduction of its molecular structure will further improve the overall flexibility and mechanical strength of the polymerized elastomer, so that the polymerized elastomer has better tolerance under high strain conditions;
[0018] (2) In the molecular structure of the polymer elastomer obtained by the present invention, abundant Si-O-Si chemical bonds are introduced through the crosslinking agent. The presence of Si-O-Si chemical bonds can also significantly improve the wear resistance of the obtained polymer elastomer. DETAILED DESCRIPTION
[0019] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0020] Example 1
[0021] A polymer elastomer, the preparation method is as follows:
[0022] Under nitrogen protection, 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)]-4,4'-dicarboxylic acid, PEG-4000, a crosslinking agent, and a catalyst were mixed and stirred uniformly, the temperature of the reaction system was raised to 160°C, and stirred for reaction at normal pressure for 2 hours, and then stirred for reaction at -0.07 MPa for 3 hours. After the reaction was completed, a polymerized elastomer was obtained;
[0023] The molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)]-4,4'-dicarboxylic acid, and crosslinking agent is 1:0.8:0.2:0.1;
[0024] The crosslinking agent is aminopropyldimethylsilyl-terminated polydimethylsiloxane (CAS: 97917-34-5);
[0025] The catalyst is a mixture of stannous oxalate and aluminum silicate in a mass ratio of 0.5:2;
[0026] Example 2
[0027] A polymer elastomer, the preparation method is as follows:
[0028] Under nitrogen protection, 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)]-4,4'-dicarboxylic acid, PEG-4000, a crosslinking agent, and a catalyst were mixed and stirred uniformly, the temperature of the reaction system was raised to 170°C, and stirred for reaction at normal pressure for 2 hours, and then stirred for reaction at -0.09 MPa for 3 hours. After the reaction was completed, a polymerized elastomer was obtained;
[0029] The molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)]-4,4'-dicarboxylic acid, and crosslinking agent is 1:0.9:0.2:0.1;
[0030] The crosslinking agent is aminopropyldimethylsilyl-terminated polydimethylsiloxane (CAS: 97917-34-5);
[0031] The catalyst is a mixture of stannous oxalate and aluminum silicate in a mass ratio of 1:1;
[0032] Example 3
[0033] A polymer elastomer, the preparation method is as follows:
[0034] Under nitrogen protection, 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)]-4,4'-dicarboxylic acid, PEG-4000, a crosslinking agent, and a catalyst were mixed and stirred uniformly, the temperature of the reaction system was raised to 180°C, and stirred for reaction at normal pressure for 2 hours, and then stirred for reaction at -0.09 MPa for 3 hours. After the reaction was completed, a polymerized elastomer was obtained;
[0035] The molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)]-4,4'-dicarboxylic acid, and crosslinking agent is 1:0.7:0.3:0.1;
[0036] The cross-linking agent is aminopolydimethylsiloxane;
[0037] The catalyst is a mixture of stannous oxalate and aluminum silicate in a mass ratio of 2:1;
[0038] Example 4
[0039] A polymer elastomer, the preparation method is as follows:
[0040] Under nitrogen protection, 1,4-cyclohexanedicarboxylic acid, decahydronaphthalene-2,6-dicarboxylic acid, PEG-4000, a crosslinking agent, and a catalyst were mixed and stirred uniformly, the temperature of the reaction system was raised to 170°C, and stirred and reacted at normal pressure for 2 hours, and then stirred and reacted at -0.08 MPa for 3 hours. After the reaction was completed, a polymerized elastomer was obtained;
[0041] The molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid, decahydronaphthalene-2,6-dicarboxylic acid, and crosslinking agent is 1:0.8:0.3:0.1;
[0042] The crosslinking agent is aminopropyldimethylsilyl-terminated polydimethylsiloxane (CAS: 97917-34-5);
[0043] The catalyst is a mixture of stannous oxalate and aluminum silicate in a mass ratio of 1:2;
[0044] Example 5
[0045] A polymer elastomer, the preparation method is as follows:
[0046] Under nitrogen protection, 1,4-cyclohexanedicarboxylic acid, decahydronaphthalene-2,6-dicarboxylic acid, PEG-6000, a crosslinking agent, and a catalyst were mixed and stirred uniformly, the temperature of the reaction system was raised to 170°C, and stirred and reacted at normal pressure for 2 hours, and then stirred and reacted at -0.08 MPa for 3 hours. After the reaction was completed, a polymerized elastomer was obtained;
[0047] The molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid, decahydronaphthalene-2,6-dicarboxylic acid, and crosslinking agent is 1:0.9:0.3:0.1;
[0048] The crosslinking agent is aminopropyldimethylsilyl-terminated polydimethylsiloxane (CAS: 97917-34-5);
[0049] The catalyst is a mixture of stannous oxalate and aluminum silicate in a mass ratio of 1:2;
[0050] Comparative Example 1 is the same as Example 1, except that the crosslinking agent in Comparative Example 1 is 1,3-bis(4-aminobutyl)tetramethyldisiloxane.
[0051] Comparative Example 2 is the same as Example 5, except that the crosslinking agent in Comparative Example 2 is 1,3-bis(4-aminobutyl)tetramethyldisiloxane.
[0052] Comparative Example 3 is the same as Example 1, except that Comparative Example 3 does not contain 1,1'-di(cyclohexyl)-4,4'-dicarboxylic acid, and the molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid and the crosslinking agent is 1:1:0.1.
[0053] Comparative Example 4 is the same as Example 5, except that Comparative Example 4 does not contain decahydronaphthalene-2,6-dicarboxylic acid, and the molar ratio of PEG-4000 to 1,4-cyclohexanedicarboxylic acid and the cross-linking agent is 1:1.2:0.1.
[0054] Comparative Example 5 is the same as Example 1, except that the PEG-4000 in Example 1 is replaced by PEG-2000 in an equal molar amount.
[0055] Comparative Example 6 is the same as Example 5, except that the PEG-4000 in Example 5 is replaced by PEG-2000 in an equal molar amount.
[0056] Performance Testing
[0057] The polymerized elastomers obtained in Examples 1-5 of the present invention and Comparative Examples 1-6 were respectively subjected to relevant performance tests, and the specific test results are shown in Table 1.
[0058] Tensile strength: According to GB / T 1040-2006 standard, the test was carried out using an INSTRON-1185 universal tensile testing machine. The test sample was made into a standard dumbbell-shaped specimen with a tensile speed of 20 mm / min.
[0059] Elongation at break: According to GB / T 1040-2006 standard, measured by INSTRON-1185 universal tensile testing machine, the test sample was made into a standard dumbbell-shaped specimen, and the tensile speed was 20 mm / min.
[0060] Recovery rate: According to GB / T 1040-2006 standard, the recovery rate was measured by INSTRON-1185 universal tensile testing machine, and the test samples were made into standard dumbbell-shaped specimens.
[0061] Table 1
[0062] Test items Tensile strength(MPa) Elongation at break (%) Recovery rate (%) Example 1 27.3 965.34 86.43 Example 2 25.45 987.21 86.29 Example 3 38.35 996.64 87.63 Example 4 29.38 841.42 81.23 Example 5 30.23 832.35 80.98 Comparative Example 1 25.34 921.33 79.61 Comparative Example 2 23.12 813.15 73.23 Comparative Example 3 22.44 820.24 71.33 Comparative Example 4 27.65 854.33 82.34 Comparative Example 5 22.11 993.45 88.64 Comparative Example 6 23.61 873.41 83.22
[0063] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A polymeric elastomer, characterized in that The preparation method comprises the following steps: Under nitrogen protection, dicarboxylic acid, polyethylene glycol, crosslinking agent and catalyst are mixed and stirred evenly, the temperature of the reaction system is raised to 160-180°C, stirred and reacted for 2 hours under normal pressure, and then stirred and reacted for 3 hours under negative pressure. During the reaction, the hydroxyl group in the reaction system reacts with the carboxyl group to form an ester bond, and the carboxyl group reacts with the amino group to form an amide bond. After the reaction is completed, a polymerized elastomer is obtained; The crosslinking agent is aminosiloxane containing two amino groups.
2. A polymeric elastomer according to claim 1, characterized in that: The catalyst is a mixture of stannous oxalate and a super strong solid acid.
3. A polymeric elastomer according to claim 2, characterized in that: The mass ratio of stannous oxalate to super strong solid acid is 1:
2.
4. A polymeric elastomer according to claim 3, characterized in that: The super strong solid acid is aluminum silicate or lithium fluorozirconate.
5. A polymeric elastomer according to claim 1, characterized in that: The catalyst is a mixture of stannous oxalate and an activated carbon-supported catalyst.
6. A polymeric elastomer according to claim 5, characterized in that: The mass ratio of stannous oxalate to activated carbon-supported catalyst is 1:
1.
7. A polymeric elastomer according to claim 6, characterized in that: The activated carbon-supported catalyst is palladium-supported activated carbon.
8. A polymeric elastomer according to claim 1, characterized in that: The dicarboxylic acid includes one or a combination of two or more of 1,4-cyclohexanedicarboxylic acid, 1,1'-di(cyclohexyl)-4,4'-dicarboxylic acid, and decahydronaphthalene-2,6-dicarboxylic acid.
9. A polymeric elastomer according to claim 1, characterized in that: The polyethylene glycol is PEG4000 or PEG6000.
10. A polymeric elastomer according to claim 1, characterized in that: The aminosiloxane includes at least one of 1,3-bis(4-aminobutyl)tetramethyldisiloxane or aminopropyldimethylsilyl-terminated polydimethylsiloxane.
Citation Information
Patent Citations
Polyester elastomer and preparation method thereof
CN105524261A
Hydrolysis-resistant polyester elastomer and preparation method thereof
CN117209738A
Random siloxane copolymer, process for production thereof, and resin composition containing the copolymer
US6103837A