Laser carving soft-touch jewel box composite material and preparation method thereof
By using a combination of heat-resistant elastomer and modified glass fiber in the jewelry box composite material, the problem of heat intolerance of existing materials is solved, the soft touch and fragrance characteristics of laser engraving are improved, and the heat resistance and heat resistance of the material are improved. Mechanical properties give the jewelry box luxury and defensive markings.
Patent Information
- Application Number
- CN202411071641.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
AI Technical Summary
Existing jewelry box composite materials are not heat-resistant, cannot be directly processed by laser engraving, and lack the performance of luxury and defensive signs.
A combination of 75-95 parts polypropylene, 20-55 parts heat-resistant elastomer, 8-15 parts modified glass fiber, 0.5-1.5 parts laser engraving powder, 0.5-2.5 parts antioxidant, and 0.5-1.3 parts lubricant , heat-resistant elastomer and modified glass fiber are prepared through solution prepolymerization and polymerization reaction to improve the heat resistance and mechanical properties of the composite material, and impart soft touch and fragrance characteristics through laser engraving powder.
It has improved the heat resistance of the composite material, given soft touch and fragrance properties, enhanced mechanical properties and slow-release properties of fragrance, and improved the quality and durability of the jewelry box.
Smart Images

Figure BDA0004981043420000031 
Figure BDA0004981043420000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic preparation, and in particular, relates to a laser-engraved soft-touch jewelry box composite material and a preparation method thereof. Background Art
[0002] With the development of plastic preparation technology, more and more wooden storage boxes are replaced by plastic boxes. This is because plastic boxes are easier to mass produce than wooden boxes, and are simpler and more convenient to manage and preserve. Replacing wooden boxes with plastic boxes can reduce the felling of a large number of trees, which is beneficial to the protection of forest resources. For example, the widely used plastic storage boxes are generally made of polyethylene PE or polypropylene PP. The base material of existing jewelry box composite materials is generally polypropylene, which is not heat-resistant and cannot be directly laser engraved. Therefore, it is necessary to perform heat-resistant modification on the existing jewelry box composite materials, and give the existing jewelry boxes luxury and defense signs through laser engraving technology. Summary of the invention
[0003] The object of the present invention is to provide a laser-engraved soft-touch jewelry box composite material and a preparation method thereof, so as to solve the problems in the background technology.
[0004] The first object of the present invention can be achieved by the following technical solutions:
[0005] A composite material for a laser-carved soft-touch jewelry box, characterized in that it comprises the following raw materials in parts by weight: 75-95 parts of polypropylene, 20-55 parts of heat-resistant elastomer, 8-15 parts of modified glass fiber, 0.5-1.5 parts of laser-carved powder, 0.5-2.5 parts of antioxidant, and 0.5-1.3 parts of lubricant;
[0006] The heat-resistant elastomer is prepared by solution polymerization of a prepolymer obtained by solution prepolymerization of polytetramethylene ether glycol, diisocyanate and a catalyst and a heat-resistant chain extender;
[0007] The heat-resistant chain extender is prepared by reacting heptaphenylsilsesquioxane trisilanol and 1,4-succinic acid under the action of an esterification reaction catalyst.
[0008] Furthermore, the mass ratio of the polytetramethylene ether diol, diisocyanate and heat-resistant chain extender is 40-65:15-23:3.5-8.5, and the catalyst is an organic tin catalyst.
[0009] Furthermore, the reaction temperature of the solution prepolymerization reaction is 50-80° C., the reaction time is 4-7 hours, and the solution in the solution prepolymerization reaction is one of acetone, tetrahydrofuran, toluene, benzene, and N,N-dimethylformamide.
[0010] Furthermore, the reaction temperature of the solution polymerization reaction is 60-85° C., the reaction time is 2-4 hours, and the solution in the solution polymerization reaction is one of acetone, tetrahydrofuran, toluene, benzene, and N,N-dimethylformamide.
[0011] Preferably, the heat-resistant elastomer is obtained by the following reaction:
[0012] After uniformly mixing polytetramethylene glycol, diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide, stirring and heating at 50-80°C, stirring and reacting for 4-7 hours, heating to 60-85°C, adding a heat-resistant chain extender, stirring and reacting for 2-4 hours, stopping the reaction, rotary evaporation, washing with water, and drying to obtain a heat-resistant elastomer.
[0013] Furthermore, the molar ratio of the heptaphenylsilsesquioxane trisilanol to 1,4-succinic acid is 1-1.2:1.
[0014] Furthermore, the reaction temperature of the heptaphenylsilsesquioxane trisilanol and 1,4-succinic acid is 70-95° C., and the reaction time is 8-24 hours.
[0015] Preferably, the specific operation of obtaining the heat-resistant chain extender is as follows:
[0016] Mix heptaphenylsilsesquioxane trisilanol, 1,4-succinic acid and N,N-dimethylformamide evenly, stir and heat to 70-95°C, slowly drop concentrated sulfuric acid, continue to keep warm and stir to react for 8-24 hours after the addition is complete, recover ethanol by rotary evaporation, wash with water, and dry to obtain a heat-resistant chain extender.
[0017] The molecular structural formula of the heptaphenylsilsesquioxane trisilanol is shown below.
[0018]
[0019] Furthermore, in a further technical solution of the present invention, the modified glass fiber is a glass fiber whose surface is modified by a first silane coupling agent, so as to improve the interface performance between the modified glass fiber and the base material.
[0020] The surface modification reaction of the first silane coupling agent and the glass fiber is a surface coupling modification reaction of a silane coupling agent well known in the technical field. Here, the present invention does not specifically limit this reaction. Preferably, the modified glass fiber used in the present invention is a glass fiber modified by a vinyl silane coupling agent.
[0021] Furthermore, in a further technical solution of the present invention, the modified glass fiber can also be prepared by graft coupling reaction of a loaded hyperbranched silane coupling agent and glass fiber;
[0022] The loaded hyperbranched silane coupling agent is obtained by mixing a second silane coupling agent, essence, ethanol and water, reacting under acidic conditions at 50-60° C. for 4-24 hours, and then post-treating, wherein the mass ratio of the second silane coupling agent, essence, ethanol and water is 10:4-6:12-20:40-50.
[0023] Preferably, in a further technical solution of the present invention, the specific operation of obtaining the modified glass fiber is as follows:
[0024] After mixing the second silane coupling agent, essence, ethanol and water, adjusting the pH value of the system to 5-5.5 with concentrated hydrochloric acid, heating to 50-60° C., stirring and reacting for 4-24 hours, evaporating the solvent, washing with water, and vacuum drying to obtain a loaded hyperbranched silane coupling agent;
[0025] In the above reaction, a hyperbranched silane coupling agent (the terminal group is still a siloxane group, which has high activity and high coupling property, and is surface modified) is formed by self-condensation and hydrolysis reaction of the terminal siloxane group in the second silane coupling agent under acidic conditions, and in the aforementioned self-condensation and hydrolysis reaction process, the added flavor molecules are easy to enter the large number of cavities formed by the hyperbranched silane coupling agent, thereby achieving the loading of the flavor and obtaining the loaded hyperbranched silane coupling agent;
[0026] Ultrasonic dispersion of glass fiber in a mixed solution of a loaded hyperbranched silane coupling agent and ethanol / water (v:v is 1-3:1), heating to 50-60°C, stirring the coupling reaction for 6-24 hours, stopping the reaction, filtering, washing with water and ethanol, and drying to obtain modified glass fiber, wherein the mass ratio of the glass fiber to the loaded hyperbranched silane coupling agent is 10:4-6.
[0027] In the above-mentioned further technical scheme of the present invention, the modified glass fiber not only realizes the surface modification of the glass fiber and improves the interface performance between the modified glass fiber and the base material, but also realizes the multi-dimensional loading of the flavor, enhances the controlled release ability of the flavor, and realizes the simultaneous introduction of the flavor through the modified glass fiber, thereby giving the composite material excellent mechanical properties and at the same time giving the composite material the characteristic of volatile fragrance, that is, further giving the jewelry box made of the composite material the characteristic of volatile fragrance and improving its quality.
[0028] The second object of the present invention can be achieved by the following technical solutions:
[0029] A method for preparing a laser-engraved soft-touch jewelry box composite material, comprising:
[0030] The composite material is obtained by mixing polypropylene, heat-resistant elastomer, modified glass fiber, laser engraving powder and lubricant, and then extruding and granulating the mixture through a twin-screw extruder.
[0031] Beneficial effects of the present invention:
[0032] The present invention provides a laser-engraved soft-touch jewelry box composite material and a preparation method thereof. By adding a heat-resistant elastomer, the cage-type siloxane in the heat-resistant elastomer is utilized to quickly form a silicon oxide layer during the heating process, thereby improving the heat resistance of the composite material. At the same time, the cage-type siloxane is introduced in the form of a polyurethane elastomer, which can give full play to the coordinated enhancement effect of the elastomer and the modified glass fiber on the polypropylene. It is found that the joint addition of the two gives the composite material a soft touch. The rigid modified glass fiber is used as the skeleton of the composite material, the polypropylene molecule is used as the base material, and the elastomer is filled to increase the mechanical properties, elastic properties and soft touch of the composite material.
[0033] In order to further give the jewelry box made of composite materials additional fragrance properties, the present invention designs modified glass fibers to achieve multi-dimensional loading of glass fibers on fragrances, which not only improves the interface properties of the modified glass fibers, but also introduces fragrances in the form of modified glass fibers, thereby improving the heat resistance of the fragrances on the one hand and the sustained-release properties of the fragrances on the other hand, thereby giving the jewelry box made of composite materials durable fragrance-emitting properties. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] Preparation of heat-resistant elastomers:
[0037] (1) 0.1 mol heptaphenylsilsesquioxane trisilanol, 0.1 mol 1,4-succinic acid and 80 mL N,N-dimethylformamide were mixed uniformly, stirred and heated to 70° C., concentrated sulfuric acid was slowly added dropwise, and after the addition was complete, the mixture was kept warm and stirred for 24 hours. Ethanol was recovered by rotary evaporation, washed with water, and dried to obtain a heat-resistant chain extender, wherein the mass fraction of concentrated sulfuric acid was 98%, and the mass of concentrated sulfuric acid added was 3% of the total mass of heptaphenylsilsesquioxane trisilanol and 1,4-succinic acid;
[0038] (2) 40 g of polytetramethylene glycol, 15 g of diisocyanate (exemplarily toluene diisocyanate), 2 g of dibutyltin dilaurate and 120 mL of N,N-dimethylformamide were mixed uniformly, heated to 50° C. with stirring, and reacted with stirring for 7 h. The temperature was raised to 60° C., 3.5 g of a heat-resistant chain extender was added, and the reaction was stirred for 4 h. The reaction was stopped, rotary evaporated, washed with water, and dried to obtain a heat-resistant elastomer.
[0039] Example 2
[0040] Preparation of heat-resistant elastomers:
[0041] (1) 0.12 mol heptaphenylsilsesquioxane trisilanol, 0.1 mol 1,4-succinic acid and 80 mL N,N-dimethylformamide were mixed uniformly, stirred and heated to 95° C., concentrated sulfuric acid was slowly added dropwise, and after the addition was complete, the mixture was kept warm and stirred for 8 h. Ethanol was recovered by rotary evaporation, washed with water, and dried to obtain a heat-resistant chain extender, wherein the mass fraction of concentrated sulfuric acid was 98%, and the mass of concentrated sulfuric acid added was 3% of the total mass of heptaphenylsilsesquioxane trisilanol and 1,4-succinic acid;
[0042] (2) 65 g of polytetramethylene glycol, 23 g of diisocyanate (exemplarily toluene diisocyanate), 4 g of dibutyltin dilaurate and 120 mL of N,N-dimethylformamide were mixed uniformly, heated to 80° C. with stirring, and reacted for 4 h at this temperature. The temperature was raised to 85° C., 8.5 g of a heat-resistant chain extender was added, and the reaction was stirred for 2 h at this temperature. The reaction was stopped, rotary evaporated, washed with water, and dried to obtain a heat-resistant elastomer.
[0043] Example 3
[0044] Preparation of modified glass fiber (glass fiber modified by surface coupling agent):
[0045] 10 g of glass fiber was ultrasonically dispersed in a mixed solution of 4 g of vinyl silane coupling agent and 30 mL of ethanol / water (v:v is 2:1), heated to 50°C, stirred for coupling reaction for 24 h, the reaction was stopped, filtered, washed with water and ethanol, and dried to obtain modified glass fiber.
[0046] Example 4
[0047] Preparation of modified glass fiber (glass fiber modified by surface coupling agent):
[0048] 10 g of glass fiber was ultrasonically dispersed in a mixed solution of 6 g of vinyl silane coupling agent and 40 mL of ethanol / water (v:v is 3:1), heated to 60°C, stirred for coupling reaction for 6 h, the reaction was stopped, filtered, washed with water and ethanol, and dried to obtain modified glass fiber.
[0049] Example 5
[0050] Preparation of modified glass fiber (loaded modified glass fiber):
[0051] (1) 10 g of a second silane coupling agent (exemplarily a vinyl silane coupling agent), 4 g of essence, 12 g of ethanol and 40 g of water were mixed, the pH value of the system was adjusted to 5-5.5 with concentrated hydrochloric acid, and the mixture was heated to 60° C. and stirred for 4 h. The solvent was evaporated, the mixture was washed with water, and vacuum dried to obtain a supported hyperbranched silane coupling agent;
[0052] (2) 10 g of glass fiber was ultrasonically dispersed in a mixed solution of 4 g of a loaded hyperbranched silane coupling agent and 30 mL of ethanol / water (v:v was 2:1), heated to 50°C, and stirred for coupling reaction for 24 h. The reaction was stopped, filtered, washed with water and ethanol, and dried to obtain modified glass fiber.
[0053] Example 6
[0054] Preparation of modified glass fiber (loaded modified glass fiber):
[0055] (1) 10 g of a second silane coupling agent (exemplarily a vinyl silane coupling agent), 6 g of essence, 20 g of ethanol and 50 g of water were mixed, the pH value of the system was adjusted to 5-5.5 with concentrated hydrochloric acid, and the mixture was heated to 50° C. and stirred for 24 h. The solvent was evaporated, the mixture was washed with water, and vacuum dried to obtain a supported hyperbranched silane coupling agent;
[0056] (2) 10 g of glass fiber was ultrasonically dispersed in a mixed solution of 6 g of a loaded hyperbranched silane coupling agent and 40 mL of ethanol / water (v:v was 4:1), heated to 60°C, and stirred for coupling reaction for 6 h. The reaction was stopped, filtered, washed with water and ethanol, and dried to obtain modified glass fiber.
[0057] Example 7
[0058] Preparation of composite materials:
[0059] (1) Prepare the following raw materials in parts by weight: 95 parts of polypropylene, 20 parts of the heat-resistant elastomer prepared in Example 1, 8 parts of the modified glass fiber prepared in Example 3, 0.5 parts of laser engraving powder, 0.5 parts of antioxidant (exemplarily antioxidant 1010), and 0.5 parts of lubricant (exemplarily polypropylene wax);
[0060] (2) Polypropylene, heat-resistant elastomer, modified glass fiber, laser engraving powder and lubricant are mixed, and then extruded and granulated by a twin-screw extruder to obtain a composite material.
[0061] Example 8
[0062] Preparation of composite materials:
[0063] (1) Prepare the following raw materials in parts by weight: 80 parts of polypropylene, 40 parts of the heat-resistant elastomer prepared in Example 2, 11 parts of the modified glass fiber prepared in Example 4, 1 part of laser engraving powder, 1 part of antioxidant (exemplarily antioxidant 1010), and 1 part of lubricant (exemplarily polypropylene wax);
[0064] (2) Polypropylene, heat-resistant elastomer, modified glass fiber, laser engraving powder and lubricant are mixed, and then extruded and granulated by a twin-screw extruder to obtain a composite material.
[0065] Example 9
[0066] Preparation of composite materials:
[0067] (1) Prepare the following raw materials in parts by weight: 75 parts of polypropylene, 55 parts of the heat-resistant elastomer prepared in Example 1, 15 parts of the modified glass fiber prepared in Example 3, 1.5 parts of laser engraving powder, 0.5-2.5 parts of antioxidant (exemplarily antioxidant 1010), and 1.3 parts of lubricant (exemplarily polypropylene wax);
[0068] (2) Polypropylene, heat-resistant elastomer, modified glass fiber, laser engraving powder and lubricant are mixed, and then extruded and granulated by a twin-screw extruder to obtain a composite material.
[0069] Example 10
[0070] Preparation of composite materials: Compared with Example 7, an equal amount of modified glass fibers were replaced with glass fibers prepared in Example 4, and the rest were the same.
[0071] Embodiment 11
[0072] Preparation of composite materials: Compared with Example 8, an equal amount of modified glass fibers were replaced with glass fibers prepared in Example 5, and the rest were the same.
[0073] Comparative Example 1
[0074] Preparation of composite material: Compared with Example 7, the modified glass fiber was deleted and the rest was the same.
[0075] Comparative Example 2
[0076] Preparation of composite material: Compared with Example 7, the heat-resistant elastomer was deleted, and the rest was the same.
[0077] Comparative Example 3
[0078] Preparation of composite material: Compared with Example 7, the heat-resistant elastomer was replaced with the product obtained by the following reaction, and the rest was the same:
[0079] 40 g of polytetramethylene glycol, 15 g of diisocyanate (exemplarily toluene diisocyanate), 2 g of dibutyltin dilaurate and 120 mL of N,N-dimethylformamide were mixed evenly, heated to 50° C. with stirring, and reacted for 7 h with stirring, and then rotary evaporated, washed with water, and dried to obtain a prepolymer.
[0080] Comparative Example 4
[0081] Preparation of composite materials
[0082] Preparation of composite material: Compared with Example 7, 1.8 parts by weight of flavor was added, and the rest was the same.
[0083] The composite materials obtained in Examples 7-11 and Comparative Examples 1-4 were subjected to physical property tests, wherein Shore hardness: tested according to ISO 7619; tensile strength test: tested according to ISO 527; heat deformation temperature: tested according to ASTM D648; touch evaluation: the composite material was injection molded into a sample piece (2cm×2cm×1cm), and after being placed at room temperature for 24 hours, the surface was touched by hand to determine whether the touch was soft, relatively soft, relatively hard or hard; laser engraving mark performance test and evaluation: the composite material was injection molded into a sample piece (2cm×2cm×1cm), and laser engraved patterns (the pattern example was a circle), and the pattern marking effect was characterized by visual inspection, and the characterization results were divided into four grades, namely very good, good, relatively good and poor; wherein, good means that the mark is clear, relatively good means that the mark is basically clear, and poor means that the mark is blurred; odor evaluation: the composite material was injection molded into a sample piece (2cm×2cm×1cm), and after being placed at room temperature for 24 hours, the sample piece was smelled, and the sample piece was smelled after an interval of 6 months and 1 year;
[0084] The above performance tests are detailed in Table 1.
[0085] Table 1
[0086]
[0087] From the data in Table 1, it can be seen that the composite materials obtained in Examples 7-11 of the present invention have excellent heat resistance and clear laser engraved patterns. Among them, the composite materials obtained in Examples 10-11 have fragrance, and the fragrance is long-lasting.
[0088] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0089] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A composite material for a laser-engraved soft-touch jewelry box, characterized in that: The invention comprises the following raw materials in parts by weight: 75-95 parts of polypropylene, 20-55 parts of heat-resistant elastomer, 8-15 parts of modified glass fiber, 0.5-1.5 parts of laser engraving powder, 0.5-2.5 parts of antioxidant, and 0.5-1.3 parts of lubricant; The heat-resistant elastomer is prepared by solution polymerization of a prepolymer obtained by solution prepolymerization of polytetramethylene ether glycol, diisocyanate and a catalyst and a heat-resistant chain extender; The heat-resistant chain extender is prepared by reacting heptaphenylsilsesquioxane trisilanol and 1,4-succinic acid under the action of an esterification reaction catalyst.
2. The composite material for a laser-engraved soft-touch jewelry box according to claim 1, characterized in that: The mass ratio of the polytetramethylene ether diol, diisocyanate and heat-resistant chain extender is 40-65:15-23:3.5-8.5, and the catalyst is an organic tin catalyst.
3. The composite material for a laser-engraved soft-touch jewelry box according to claim 1, characterized in that: The reaction temperature of the solution prepolymerization reaction is 50-80° C., the reaction time is 4-7 hours, and the solution in the solution prepolymerization reaction is one of acetone, tetrahydrofuran, toluene, benzene, and N,N-dimethylformamide.
4. The composite material for a laser-engraved soft-touch jewelry box according to claim 1, characterized in that: The reaction temperature of the solution polymerization reaction is 60-85° C., the reaction time is 2-4 hours, and the solution in the solution polymerization reaction is one of acetone, tetrahydrofuran, toluene, benzene, and N,N-dimethylformamide.
5. The composite material for laser-engraved soft-touch jewelry boxes according to claim 1, characterized in that: The molar ratio of the heptaphenylsilsesquioxane trisilanol to 1,4-succinic acid is 1-1.2:
1.
6. The composite material for laser-engraved soft-touch jewelry boxes according to claim 1, characterized in that: The reaction temperature of the reaction of heptaphenylsilsesquioxane trisilanol and 1,4-succinic acid is 70-95° C., and the reaction time is 8-24 hours.
7. The composite material for laser-engraved soft-touch jewelry boxes according to claim 1, characterized in that: The modified glass fiber is a glass fiber whose surface is modified by a first silane coupling agent.
8. The composite material for laser-engraved soft-touch jewelry boxes according to claim 7, characterized in that: The modified glass fiber is prepared by graft coupling reaction of a loaded hyperbranched silane coupling agent and glass fiber; The loaded hyperbranched silane coupling agent is obtained by mixing a second silane coupling agent, essence, ethanol and water, reacting under acidic conditions at 50-60° C. for 4-24 hours, and then post-treating.
9. The composite material for laser-engraved soft-touch jewelry boxes according to claim 8, characterized in that: The mass ratio of the glass fiber to the loaded hyperbranched silane coupling agent is 10:4-6; the mass ratio of the second silane coupling agent, essence, ethanol and water is 10:4-6:12-20:40-50.
10. The method for preparing a composite material for a laser-engraved soft-touch jewelry box according to claim 1, characterized in that: include: The composite material is obtained by mixing polypropylene, heat-resistant elastomer, modified glass fiber, laser engraving powder and lubricant, and then extruding and granulating the mixture through a twin-screw extruder.
Citation Information
Patent Citations
Process for preparing hydroxyl polyhedral oligomeric silsesquioxane modified polyurethane
CN102617823A
Environmental-protection self-aromatic and continuously volatile polypropylene material and preparation method thereof
CN105086146A
Hyperbranched polyamide modified polypropylene composite material and preparation method thereof
CN106995550A
Fragrant flame-retardant antibacterial composite plastic packaging material
CN109337328A
Phenyl vinyl siloxane resin, high-refractive-index light-emitting diode (LED) packaging silicon resin composition and preparation method of silicon resin composition
CN110229339A
Cited By
Fragrance-lasting soft-touch jewel box composite material and preparation method thereof
CN121182060A