Antibacterial transparent nylon composite material as well as preparation method and application thereof
By using a combination of furan antibacterial agents and other additives in nylon materials, the problem of insufficient transparency and antibacterial properties of nylon materials is solved, and the preparation of highly efficient antibacterial transparent nylon composite materials is achieved, which is suitable for a variety of electronic and home appliance applications.
Patent Information
- Application Number
- CN202411071797.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Existing nylon materials have deficiencies in transparency and antibacterial properties, and cannot meet the high standards of automotive, electronic appliances, home appliances and other fields.
Furan antibacterial agents are used as organic antibacterial agents, mixed evenly with nylon, antioxidants, lubricants and anti-yellowing agents, and granulated through a twin-screw extruder to prepare antibacterial transparent nylon composite materials.
It achieves excellent antibacterial and light transmittance properties of nylon composite materials, has simple process and low cost, is suitable for mass production, and is suitable for applications in electronic appliances, home appliances, and automotive interior and exterior decorations.
Smart Images

Figure CN118791870A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nylon composite materials, and specifically relates to an antibacterial transparent nylon composite material and a preparation method and application thereof. Background Art
[0002] Nylon (PA6) is known as one of the five major engineering plastics. It has attracted much attention for its excellent processing performance, excellent temperature resistance, excellent chemical resistance and outstanding lubrication performance. It has been deployed and applied on a large scale in home appliances, electronic and electrical fields, and automotive parts. However, due to the shortcomings of conventional nylon materials in terms of transparency and antibacterial properties, these problems have undoubtedly seriously restricted the further development and application of nylon in the fields of automobiles, electronic appliances, home appliances, etc. With the continuous expansion of the application field of nylon in society, more stringent requirements have been put forward for the transparency, antibacterial and other properties of the material.
[0003] In the traditional antibacterial flame-retardant nylon manufacturing process, commonly used antibacterial agents can be mainly divided into two categories: inorganic antibacterial agents and organic antibacterial agents. Among them, inorganic antibacterial agents are usually antibacterial agents composed of metal elements such as copper, zinc, and silver. This type of antibacterial agent has excellent antibacterial properties, but affects the transparency of the material and cannot meet the special needs of many products. Organic antibacterial agents are added in high amounts and are easily decomposed in high temperature environments, which cannot meet the transparency of the product.
[0004] For example: Patent CN200610123560.1 discloses an antibacterial nylon plastic material, which mainly improves the antibacterial properties of alloy materials by inorganic antibacterial agents, but the antibacterial agent itself is white, which will reduce the light transmittance of the material; Patent CN202110604927.6 discloses antibacterial nylon 6 containing guanidine groups. This technical solution uses 6-guanidinohexanoic acid as an antibacterial agent for nylon and adds it during the polymerization process of nylon. The cost of this solution is relatively high, and the processing technology is complicated and the cost is relatively high. Therefore, it is an urgent problem to provide an antibacterial transparent nylon composition that is economical, simple to prepare, and has good transparency. Summary of the invention
[0005] The main purpose of the present invention is to provide an antibacterial transparent nylon composite material and a preparation method and application thereof, so as to overcome the shortcomings of the prior art.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0007] The embodiment of the present invention provides an antibacterial transparent nylon composite material, and the raw materials for preparing the antibacterial transparent nylon composite material include the following components: nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent;
[0008] Wherein, the furan antibacterial agent has a structure as shown in formula (I):
[0009]
[0010] Here, R is selected from alkyl groups such as methyl, ethyl, 4-aminobutane or benzyl.
[0011] The embodiment of the present invention also provides a method for preparing the aforementioned antibacterial transparent nylon composite material, which comprises: uniformly mixing nylon, a furan antibacterial agent, an antioxidant, a lubricant and an anti-yellowing agent, and then adding the obtained mixture to a twin-screw extruder for granulation to obtain the antibacterial transparent nylon composite material.
[0012] The embodiments of the present invention also provide the use of the aforementioned antibacterial transparent nylon composite material in preparing electronic and electrical appliance housings, household appliance housings or automobile interior and exterior decorations.
[0013] The present invention also provides a furan antibacterial agent having a structure as shown in formula (I):
[0014]
[0015] Here, R is selected from alkyl groups such as methyl, ethyl, 4-aminobutane or benzyl.
[0016] The embodiment of the present invention also provides a method for preparing the aforementioned furan antibacterial agent, which comprises: in a protective atmosphere, polymerizing a mixed reaction system comprising 2,5-furandicarboxaldehyde, 2-aminoalkylamide, and a solvent to obtain the furan antibacterial agent.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The furan antibacterial agent provided by the present invention is an organic antibacterial agent and has good compatibility with nylon. It can be fully dispersed in the nylon matrix under the shearing of the twin-screw, ensuring the excellent long-term antibacterial and light-transmitting properties of the composite material;
[0019] (2) The manufacturing process of the antibacterial transparent nylon composite material in the present invention is simple and easy to implement. At the same time, it is also more economical in terms of cost investment compared with other solutions. Its operation process is flexible and convenient, and it is highly practical, which is very suitable for large-scale industrial-grade production operations. DETAILED DESCRIPTION
[0020] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Specifically, as one aspect of the technical solution of the present invention, the raw materials of an antibacterial transparent nylon composite material include the following components: nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent;
[0022] Wherein, the furan antibacterial agent has a structure as shown in formula (I):
[0023]
[0024] Here, R is selected from alkyl groups such as methyl, ethyl, 4-aminobutane or benzyl.
[0025] Furthermore, R in the furan antibacterial agent is derived from any one or more combinations of 2-aminopropionamide, 2-aminobutyramide, 2-aminohexanamide, and 2-aminopentanamide, but is not limited thereto.
[0026] The furan antibacterial agent in the present invention is an organic antibacterial agent and can be fully dispersed in the matrix nylon, thereby improving the antibacterial property and toughness of the material.
[0027] In some preferred embodiments, the raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 15% to 76% nylon, 0.5% to 5% furan antibacterial agent, 0.1% to 2% antioxidant, 0.1% to 5% lubricant and 0.1% N3% anti-yellowing agent.
[0028] Furthermore, the raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 45%-65% nylon, 0.5%-4% furan antibacterial agent, 0.1%-2% antioxidant, 0.1%-5% lubricant and 0.5% N2 anti-yellowing agent.
[0029] Furthermore, the raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 45%-65% nylon, 1%-5% furan antibacterial agent, 0.2%-2% antioxidant, 0.1%-5% lubricant and 0.5%-3% anti-yellowing agent.
[0030] Furthermore, the raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 45%-65% nylon, 1%-5% furan antibacterial agent, 0.2%-2% antioxidant, 0.1%N1% lubricant and 0.5%-1% anti-yellowing agent.
[0031] In some preferred embodiments, the nylon includes semi-aromatic transparent nylon, but is not limited thereto.
[0032] In some preferred embodiments, the antioxidant comprises any one or more combinations of 1098, 1010, and 1076, but is not limited thereto.
[0033] In some preferred embodiments, the lubricant includes any one or more combinations of E wax, aluminum stearate, and silicone, but is not limited thereto.
[0034] In some preferred embodiments, the anti-yellowing agent includes any one or more combinations of tris(2,4-di-tert-butylphenyl)phosphite, di(2,2,6,6-tetramethyl-3-piperidinylamino)-isophthalamide, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and is not limited thereto.
[0035] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned antibacterial transparent nylon composite material, which comprises:
[0036] Nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent are uniformly mixed, and then the obtained mixture is added into a twin-screw extruder for granulation to prepare an antibacterial transparent nylon composite material.
[0037] In some preferred embodiments, the preparation method specifically comprises: placing nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent in a high-speed kneading device, and stirring and mixing at a rotation speed of 100-500 rpm / min for 5-25 minutes.
[0038] Furthermore, the rotation speed is 100-200 rpm / min.
[0039] For example, the high-speed kneading device may be a high-speed kneader.
[0040] In some preferred embodiments, the temperature parameters of each zone of the twin-screw extruder from the feeding port to the die include: the temperature of zone 1 is 190-210°C, the temperature of zone 2 is 260-270°C, the temperature of zone 3 is 260-270°C, the temperature of zone 4 is 260-270°C, the temperature of zone 5 is 260-270°C, the temperature of zone 6 is 245-250°C, the temperature of zone 7 is 240-250°C, the temperature of the die is 260-270°C, and the rotation speed is 300-450rpm / min.
[0041] In some more specific embodiments, the method for preparing the antibacterial transparent nylon composite material comprises the following steps:
[0042] (1) uniformly mixing nylon, a furan antibacterial agent, an antioxidant, an anti-yellowing agent, and a lubricant which may be optionally added to obtain a mixed material;
[0043] (2) The mixed materials are added into a twin-screw extruder and pelletized by a tractor to obtain an antibacterial transparent nylon composition.
[0044] Furthermore, in step (1), the conditions for uniform mixing are: placing each component in a high-speed kneader, maintaining a rotation speed of 100-200 rpm / min, and high-speed stirring for 5-20 minutes.
[0045] Furthermore, in step (2), the temperatures of each zone of the twin-screw extruder from the feed port to the die are: zone one temperature is 190-210°C, zone two temperature is 260-270°C, zone three temperature is 260-270°C, zone four temperature is 260-270°C, zone five temperature is 260-270°C, zone six temperature is 245-250°C, zone seven temperature is 240-250°C, die head temperature is 260-270°C, and the rotation speed is 300-450rpm / min.
[0046] Another aspect of the embodiments of the present invention further provides the use of the aforementioned antibacterial transparent nylon composite material in the preparation of electronic and electrical appliance housings, household appliance housings, or automobile interior and exterior decorations.
[0047] Another aspect of the embodiments of the present invention further provides a furan antibacterial agent having a structure as shown in formula (I):
[0048]
[0049] Here, R is selected from alkyl groups such as methyl, ethyl, 4-aminobutane or benzyl.
[0050] Another aspect of an embodiment of the present invention further provides a method for preparing the aforementioned furan antibacterial agent, which comprises: in a protective atmosphere, polymerizing a mixed reaction system comprising 2,5-furandicarboxaldehyde, 2-aminoalkylamide, and a solvent to obtain the furan antibacterial agent.
[0051] In some preferred embodiments, the 2-aminoalkylamide includes any one or more combinations of 2-aminopropionamide, 2-aminobutyramide, 2-aminohexanamide, and 2-aminopentanamide, but is not limited thereto.
[0052] In some preferred embodiments, the solvent includes tetrahydrofuran and / or toluene, but is not limited thereto.
[0053] In some preferred embodiments, the molar ratio of 2,5-furandicarboxaldehyde to 2-aminoalkylamide is 1 to 4:1.
[0054] In some more specific embodiments, the method for preparing the furan antibacterial agent comprises:
[0055] 2,5-furandicarboxaldehyde (0.1 mol), 2-aminoalkylamide (0.5 mol), tetrahydrofuran (150 ml) were added to a round-bottom flask, stirred to make a uniform solution and sealed. Then, the mixture was placed in a 60°C oil bath and sealed for polymerization for 6-12 hours. After the polymerization reaction was completed, the mixture was repeatedly washed with a solvent, filtered, and vacuum dried to a constant weight to obtain a polymerized furan antibacterial agent.
[0056] The present invention prepares an organic furan antibacterial agent by a free radical reaction method. The polymer has good dispersibility and can be fully dispersed under the shearing of a twin-screw, thereby improving the antibacterial property of a nylon composite material. On the other hand, the furan antibacterial agent is an organic antibacterial agent and has good compatibility with nylon, thereby maintaining the light transmittance of transparent nylon.
[0057] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments. This embodiment is implemented on the premise of the technical solution of the invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0058] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0059] Preparation Example 1
[0060] The preparation of the furan antibacterial agent used in the following examples specifically includes the following steps:
[0061] 2,5-furandicarboxaldehyde (0.1 mol), 2-aminobutyramide (0.4 mol), and tetrahydrofuran (150 ml) were added to a round-bottom flask, stirred to make a uniform solution and sealed. Then, the mixture was placed in a 60°C oil bath for constant temperature and sealed for polymerization. After the polymerization reaction was completed for 12 hours, the mixture was repeatedly washed with a solvent, filtered, and vacuum dried to a constant weight to obtain a polymerized furan antibacterial agent.
[0062] The prepared furan antibacterial agent was characterized by nuclear magnetic resonance. The chemical shift was δ=8.4-8.6ppm, corresponding to the hydrogen element on the carbon connected to the 2 and 5 positions of furan on the furan imine polymer; the chemical shift was δ=6.53-6.57ppm, corresponding to the two hydrogen atoms on the 3 and 4 positions of furan; the chemical shift was δ=3.39ppm, corresponding to the hydrogen atom on the carbon connected to the amino group on the furan imine polymer; the chemical shift was δδ=0.85-0.87ppm, corresponding to the hydrogen atoms on the methyl groups on both sides of the furan imine polymer, proving that the furan antibacterial agent was successfully prepared. The obtained furan antibacterial agent has the following structure:
[0063]
[0064] Preparation Example 2
[0065] 2,5-furandicarboxaldehyde (0.1 mol), 2-aminopentylamide (0.4 mol), and tetrahydrofuran (150 ml) were added to a round-bottom flask, stirred to make a uniform solution and sealed. Then, the mixture was placed in a 60°C oil bath for constant temperature and sealed for polymerization. After the polymerization reaction was completed in 12 hours, the mixture was repeatedly washed with a solvent, filtered, and vacuum dried to a constant weight to obtain a polymerized furan antibacterial agent.
[0066] Preparation Example 3
[0067] 2,5-furandicarboxaldehyde (0.1 mol), 2-aminopentylamide (0.3 mol), and tetrahydrofuran (150 ml) were added to a round-bottom flask, stirred to make a uniform solution and sealed. Then, the mixture was placed in a 60°C oil bath for constant temperature and sealed for polymerization. After the polymerization reaction was completed for 12 hours, the mixture was repeatedly washed with a solvent, filtered, and vacuum dried to a constant weight to obtain a polymerized furan antibacterial agent.
[0068] Example 1
[0069] Weigh the components according to Table 1 below:
[0070] Table 1
[0071]
[0072] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0073] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0074] (3) adding the mixed material obtained in step (2) into a feeding hopper of a twin-screw extruder, wherein the parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0075] Example 2
[0076] Weigh the components according to Table 2 below:
[0077] Table 2
[0078]
[0079] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0080] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0081] (3) adding the mixed material obtained in step (2) into a feeding hopper of a twin-screw extruder, wherein the parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0082] Example 3
[0083] Weigh the components according to Table 3 below:
[0084] Table 3
[0085]
[0086] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0087] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0088] (3) adding the mixed material obtained in step (2) into a feeding hopper of a twin-screw extruder, wherein the parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0089] Example 4
[0090] Weigh the components according to Table 4 below:
[0091] Table 4
[0092]
[0093] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0094] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0095] (3) adding the mixed material obtained in step (2) into a feeding hopper of a twin-screw extruder, wherein the parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0096] Example 5
[0097] Weigh the components according to Table 5 below:
[0098] Table 5
[0099]
[0100]
[0101] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0102] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0103] (3) adding the mixed material obtained in step (2) into a feeding hopper of a twin-screw extruder, wherein the parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0104] Comparative Example 1
[0105] Weigh the components according to Table 6 below:
[0106] Table 6
[0107]
[0108] (1) According to the weight percentage formula, the dried furan antibacterial agent, antioxidant, E wax, anti-yellowing agent, and lubricant are weighed;
[0109] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0110] (3) adding the mixed material obtained in step (2) into a feeding hopper of a twin-screw extruder, wherein the parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0111] Comparative Example 2
[0112] Weigh the components according to Table 7 below:
[0113] Table 7
[0114]
[0115]
[0116] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0117] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0118] (3) adding the mixed material obtained in step (2) into the feeding funnel of a twin-screw extruder. The parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0119] Comparative Example 3
[0120] Weigh the components according to Table 8 below:
[0121] Table 8
[0122]
[0123] (1) According to the weight percentage formula, the dried nylon, the prepared furan antibacterial agent, the antioxidant, the E wax, the anti-yellowing agent, and the lubricant are weighed;
[0124] (2) The weighed components were placed in a high-speed mixer at a speed of 350 rpm / min for 20 min;
[0125] (3) adding the mixed material obtained in step (2) into the feeding funnel of a twin-screw extruder. The parameters of the twin-screw extruder are: temperature of zone 1: 195° C., temperature of zone 2: 260° C., temperature of zone 3: 260° C., temperature of zone 4: 260° C., temperature of zone 5: 260° C., temperature of zone 6: 250° C., temperature of zone 7: 250° C., head temperature: 270° C., rotation speed: 300 rpm / min, and after being pulled and pelletized by a traction machine, a nylon composite material is obtained.
[0126] The composite materials prepared in Examples 1-5 and Comparative Examples 1-3 were tested, and the results are shown in Table 9: Table 9
[0127]
[0128] From the data in Table 9, the antibacterial and light transmittance properties of the nylon composite material prepared by the present invention meet the requirements. It can be seen from Examples 1-5 that when the furan antibacterial agent is added, the antibacterial property of the resin can be improved. It can be seen from Example 3, Example 4, Example 5, Comparative Example 1, Comparative Example 2, and Comparative Example 3 that after adding the furan antibacterial agent, the composite material has a more excellent transparency.
[0129] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0130] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. An antibacterial transparent nylon composite material, characterized in that: The raw materials for preparing the antibacterial transparent nylon composite material include the following components: nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent; Wherein, the furan antibacterial agent has a structure as shown in formula (I): Here, R is selected from alkyl groups such as methyl, ethyl, 4-aminobutane or benzyl.
2. The antibacterial transparent nylon composite material according to claim 1, characterized in that: The raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 15% to 76% nylon, 0.5% to 5% furan antibacterial agent, 0.1% to 2% antioxidant, 0.1% to 5% lubricant and 0.1% to 3% anti-yellowing agent.
3. The antibacterial transparent nylon composite material according to claim 2, characterized in that: The raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 45%-65% nylon, 0.5%-4% furan antibacterial agent, 0.1%-2% antioxidant, 0.1%-5% lubricant and 0.5%-2% anti-yellowing agent; And / or, the raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 45% to 65% nylon, 1% to 5% furan antibacterial agent, 0.2% to 2% antioxidant, 0.1% to 5% lubricant and 0.5% to 3% anti-yellowing agent; And / or, the raw materials for preparing the antibacterial transparent nylon composite material include the following components calculated by weight percentage: 45% to 65% nylon, 1% to 5% furan antibacterial agent, 0.2% to 2% antioxidant, 0.1% to 1% lubricant and 0.5% to 1% anti-yellowing agent.
4. The antibacterial transparent nylon composite material according to claim 1, characterized in that: The nylon includes semi-aromatic transparent nylon; And / or, the antioxidant agent includes any one or more combinations of 1098, 1010, and 1076; And / or, the lubricant includes any one or more combinations of E wax, aluminum stearate, and silicone; And / or, the anti-yellowing agent includes any one or more combinations of tris(2,4-di-tert-butylphenyl)phosphite, bis(2,2,6,6-tetramethyl-3-piperidinylamino)-isophthalamide, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite.
5. The method for preparing the antibacterial transparent nylon composite material according to any one of claims 1 to 4, characterized in that: include: Nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent are uniformly mixed, and then the obtained mixture is added into a twin-screw extruder for granulation to prepare an antibacterial transparent nylon composite material.
6. The preparation method according to claim 5, characterized in that: Specifically include: Place nylon, furan antibacterial agent, antioxidant, lubricant and anti-yellowing agent in a high-speed kneading device, and stir and mix at a speed of 100-500 rpm / min for 5-25 minutes; And / or, the temperature parameters of each zone of the twin-screw extruder from the feeding port to the die include: the temperature of zone one is 190-210°C, the temperature of zone two is 260-270°C, the temperature of zone three is 260-270°C, the temperature of zone four is 260-270°C, the temperature of zone five is 260-270°C, the temperature of zone six is 245-250°C, the temperature of zone seven is 240-250°C, the temperature of the die head is 260-270°C, and the rotation speed is 300-450rpm / min.
7. Use of the antibacterial transparent nylon composite material according to any one of claims 1 to 4 in the preparation of electronic and electrical appliance housings, household appliance housings or automobile interior and exterior decorations.
8. A furan antibacterial agent, characterized in that: The furan antibacterial agent has a structure as shown in formula (I): Here, R is selected from alkyl groups such as methyl, ethyl, 4-aminobutane or benzyl.
9. The method for preparing a furan antibacterial agent according to claim 8, wherein: include: In a protective atmosphere, a mixed reaction system comprising 2,5-furandicarboxaldehyde, 2-aminoalkylamide and a solvent is polymerized to obtain a furan antibacterial agent.
10. The preparation method according to claim 9, characterized in that: The 2-aminoalkylamide includes any one or more combinations of 2-aminopropionamide, 2-aminobutyramide, 2-aminohexanamide, and 2-aminovaleramide; and / or, the solvent comprises tetrahydrofuran and / or toluene; And / or, the molar ratio of the 2,5-furandicarboxaldehyde to the 2-aminoalkylamide is 1 to 4:1.
Citation Information
Patent Citations
Antibacterial nylon 6 containing guanidyl group and preparation method thereof
CN114181389A
Antibacterial nylon plastic material and its preparation method
CN1970631A
Methods for producing nylon 7
CN106029781A
Furan skeleton-containing imine guanidine derivatives and preparation and application thereof
CN108003120A
Brivaracetam intermediate and preparation method thereof
CN110615744A