Titanium alloy with high strength and toughness martensite heterostructure as well as preparation method and application thereof
Through the combination of powder metallurgy and hot extrusion process, combined with resistance heating heat treatment, the Ti-6Al-4V titanium alloy with martensitic heterostructure is formed, which solves the problem of synergistic improvement of strength and plasticity of traditional titanium alloys and achieves high strength, toughness and material The increase in density is suitable for high-strength and high-toughness structural parts.
Patent Information
- Application Number
- CN202411077124.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-18
AI Technical Summary
The traditional Ti-6Al-4V titanium alloy increases the strength but also causes the deterioration of plasticity, and it is difficult to ensure the uniformity of the ingot composition. The presence of holes in the powder metallurgy billet affects the mechanical properties.
Using a combination of powder metallurgy and hot extrusion processes, through resistance heating heat treatment, controlling the energization time and water quenching, a martensite heterostructure is formed, including the martensite phase and primary α phase, and the microstructure of the material is optimized.
The room temperature tensile strength and elongation of titanium alloys are significantly improved, the material density is increased, and the strength and toughness are improved. It is suitable for high-strength or high-toughness structural parts in the aerospace, shipbuilding and automotive fields.
Smart Images

Figure CN118792544A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of titanium alloys, and in particular to a high-strength and toughness martensitic heterostructure titanium alloy and a preparation method and application thereof. Background Art
[0002] Ti-6Al-4V is widely used in aviation, chemical, biomedicine, marine and other fields due to its excellent comprehensive mechanical properties.
[0003] At present, after commercial TC4 titanium alloy is processed by traditional technology, the obtained organization usually presents four typical forms, including lamellar organization, dual-state organization, basket organization, and equiaxed organization. The strength and plasticity of traditional commercial TC4 titanium alloy are usually in the range of 900-1000MPa and 7%-10%. With the deeper exploration of the ocean and space, the comprehensive performance of titanium alloy materials has been challenged more, especially the synergistic improvement of its strength and toughness. At present, most traditional methods improve the strength of the material while leading to the deterioration of plasticity.
[0004] In addition, the inventors of the present application noticed that the traditional method of obtaining Ti-6Al-4V ingots by smelting is difficult to ensure the uniformity of the composition of the entire ingot. Although powder metallurgy can effectively solve the problem of uneven composition, the billets produced by powder metallurgy have many pores, which seriously affect their mechanical properties. Summary of the invention
[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, according to one embodiment of the present application, the purpose is to provide a high-strength and toughness martensitic heterostructure titanium alloy and a preparation method and application thereof.
[0006] The above purpose can be achieved by implementing the following technical solutions:
[0007] According to one aspect of the present application, a method for preparing a high-strength and tough martensitic heterostructure titanium alloy provided in the present application comprises the following steps:
[0008] Ti-6Al-4V alloy powder is used as raw material, pressed and sintered to obtain a blank;
[0009] The blank is plastically deformed by a hot extrusion process to obtain a formed part;
[0010] The formed part is heat treated by resistance heating, and a titanium alloy with a martensitic heterostructure is obtained by controlling the time.
[0011] Optionally, the step of heat treating the formed part by resistance heating and obtaining a titanium alloy with a martensitic heterostructure by controlling the time refers to processing the formed part into a plate and using it as a resistor, applying voltage for heating, controlling the power-on time, and water quenching to obtain a titanium alloy with a martensitic heterostructure.
[0012] Optionally, when the applied voltage is 110V to 220V, the power-on time is controlled to be 4s to 25s.
[0013] Optionally, the step of plastically deforming the blank by a hot extrusion process to obtain a formed part includes: heating and keeping the blank warm under a vacuum atmosphere; placing the warmed blank in a preheated extrusion die, hot extruding it, and air cooling it to room temperature to obtain a formed part.
[0014] Optionally, the insulation temperature is 900° C. to 1000° C., and the insulation time is 20 min to 60 min.
[0015] Further optionally, the extrusion ratio is 5 to 18, and the extrusion speed is 2 mm / s to 5 mm / s.
[0016] Optionally, the preheating temperature of the mold is 400°C to 500°C.
[0017] Further optionally, the particle diameter of the Ti-6Al-4V alloy powder is 50-150 μm.
[0018] Optionally, the pressing and sintering are performed by cold isostatic pressing-vacuum sintering.
[0019] Further optionally, the pressing pressure is 200-400 MPa, and the holding time is 0.5-3 h.
[0020] Further optionally, the vacuum sintering temperature is 1100-1400° C., and the holding time is 1-6 hours.
[0021] Optionally, the microstructure of the titanium alloy with a martensitic heterostructure consists of a martensitic phase + a primary α phase. Further, α-Ti of different shapes and sizes and martensite of different sizes constitute the martensitic heterostructure.
[0022] Furthermore, the martensite is in the form of strips, 1 to 30 μm long, and the aspect ratio is greater than 10:1; α-Ti coexists in the form of strips and equiaxed structures, and further, in the form of strips with a length of 10 to 50 μm and an equiaxed structure with a diameter of 1 to 15 μm.
[0023] According to another aspect of the present application, a high-strength and toughness martensitic heterostructure titanium alloy provided in the present application is prepared by adopting the preparation method of the high-strength and toughness martensitic heterostructure titanium alloy.
[0024] Furthermore, the room temperature tensile strength of the titanium alloy with a martensitic heterostructure is greater than 1200MPa, and the elongation is greater than 10%. Alternatively, the room temperature tensile strength of the titanium alloy with a martensitic heterostructure is greater than 1000MPa, and the elongation is greater than 20%, which is a significant improvement over commercial TC4. For example, the room temperature tensile strength of the titanium alloy with a martensitic heterostructure is 1050MPa to 1300MPa, and the elongation is 11% to 30%. In particular, the room temperature tensile strength of the titanium alloy with a martensitic heterostructure can reach more than 1200MPa, and / or, its elongation can reach more than 20%.
[0025] According to another aspect of the present application, the present application provides an application of a high-strength and toughness martensitic heterostructure titanium alloy in high-strength and / or high-toughness structural parts in the fields of aerospace, shipbuilding, and automobiles. The high-strength and toughness martensitic heterostructure titanium alloy is prepared by the preparation method of the high-strength and toughness martensitic heterostructure titanium alloy.
[0026] Beneficial effect: According to one embodiment of the present application, by combining powder metallurgy and hot extrusion processes, not only the uniformity of the composition is ensured, but also the pores in the powder metallurgy rod blank are eliminated during the hot extrusion process, and the density of the material is improved, thereby effectively reducing the source of crack propagation and improving the strength and toughness of the material; the material is then heat treated, especially in the preferred embodiment of the present application, the heat treatment is carried out by resistance heating. By controlling the power-on time and water quenching, a titanium alloy with a martensitic heterostructure in which martensite, strip-shaped α and equiaxed α coexist can be obtained.
[0027] Compared with the prior art, the embodiments of the present invention also have the following advantages and beneficial effects:
[0028] (1) The present application combines powder metallurgy with hot extrusion and resistance heating to regulate the microstructure of the material, and can prepare a titanium alloy with a martensite heterostructure including elongated crystals, equiaxed α-Ti and martensite.
[0029] (2) The martensitic heterostructure titanium alloy of the present application has excellent mechanical properties and can be applied to high-strength or impact-resistant structural parts in the fields of aerospace, shipbuilding, and automobiles.
[0030] (3) The present invention adopts a resistance heating heat treatment method and realizes effective control of the phase transformation process in the titanium alloy by controlling the power-on time. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a phase distribution diagram of the martensitic heterostructure titanium alloy obtained in Example 1 of the present application.
[0032] Figure 2This is the IPF diagram of the martensitic heterostructure titanium alloy obtained in Example 1 of the present application.
[0033] Figure 3 This is the IPF diagram of the martensitic heterostructure titanium alloy obtained in Example 3 of the present application.
[0034] Figure 4 It is the mechanical curve diagram of Example 1, Example 2 and Example 3 of the present application. DETAILED DESCRIPTION
[0035] The technical solution of the present application will be clearly and completely described below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its application or use. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0036] The present application prepares a formed part by combining powder metallurgy and hot extrusion processes, and heat treats the formed part to obtain a titanium alloy with a martensitic heterostructure. The mechanical properties of the titanium alloy are greatly improved, and it is a TC4 titanium alloy with a high-strength and toughness martensitic heterostructure. Moreover, the preparation process of the present application is simple and fast, which reduces the time cost. The titanium alloy of the present application can be used in high-strength and / or high-toughness structural parts in the fields of aerospace, shipbuilding, and automobiles.
[0037] The titanium alloy of the present application is a martensitic heterostructure, and the structure consists of a martensitic phase + a primary α phase.
[0038] The following is a description of the invention concept of the present application. The inventors of the present application recognize that the heterogeneous microstructure is the coexistence of grains of different scales (micrometers to millimeters). During the deformation process of this organization, the interface of grains of different scales will produce a large strain gradient, thereby inducing back stress strengthening to obtain excellent strength. And the grains of different sizes can better coordinate the deformation, thereby breaking the inversion relationship between strength and toughness, and improving the comprehensive performance of titanium alloy materials. On the other hand, the martensitic phase transformation is a diffusionless phase transformation of the high-temperature phase at a lower temperature during rapid cooling. The inventors of the present application recognize that the martensitic structure in steel can greatly improve the strength of steel, and titanium alloys also have high-temperature phases (β phases) and low-temperature phases (α phases). The martensitic structure in titanium alloys can also obtain strength enhancement. During the martensitic phase transformation, the yield strength can be significantly reduced and the plasticity can be significantly increased. Therefore, the present application adopts hot extrusion and resistance rapid heating treatment to effectively control the content and distribution of martensite, α phase and metastable β, while improving the toughness of the material. Based on this, the inventors of the present application provide a titanium alloy with a martensitic heterostructure and a process thereof.
[0039] Moreover, the present application first adopts a powder metallurgy process so that the material can have a uniform composition after plastic deformation, providing the possibility of producing a uniform equiaxed α+β structure. Furthermore, in order to overcome the problem that the blank produced by powder metallurgy has many holes that seriously affect its mechanical properties, the present application adopts a hot extrusion process to plastically deform the blank. The hot extrusion process effectively improves the density of the material, and the processing is in a three-way pressure state, which improves the plastic processing ability of the material. After hot extrusion, air cooling forms a heterogeneous structure.
[0040] In addition, the inventors of the present application further realized that the heating rate of the traditional heat treatment process is slow, and the β phase transformation rate in the titanium alloy is quite fast, making the phase transformation difficult to control. In view of this, in the preferred embodiment of the present application, firstly, the blank is made by powder metallurgy, and the hot extrusion is carried out under suitable conditions to make it more dense and undergo dynamic recrystallization, and then air cooling is used to allow some recrystallization to grow slightly, forming a heterogeneous structure in which strips and equiaxial structures of different scales coexist; then, after the bar is processed into a plate, a heat treatment method of resistance heating is used to greatly increase the heating rate, and, only by controlling the power-on time, a certain β phase can be obtained, and then martensite can be obtained by water quenching, thereby preparing a high-strength and tough martensitic heterogeneous structure TC4 titanium alloy; by controlling the power-on time of the resistance heating method, the phase transformation process control in the titanium alloy is realized.
[0041] A method for preparing a high-strength and tough martensitic heterostructure titanium alloy provided in an embodiment of the present application comprises the following steps:
[0042] Step S1, using a powder metallurgy process, using Ti-6Al-4V alloy powder as a raw material, pressing and sintering it into a blank, such as a rod blank. The blank is prepared using a powder metallurgy process to make its composition uniform and create favorable conditions for the formation of the titanium alloy structure of the present application.
[0043] Wherein, the particle diameter of the alloy element powder may be 50-150 μm.
[0044] The target titanium alloy is an α+β dual-phase titanium alloy; correspondingly, the alloy powder of the target titanium alloy composition is consistent with the composition of industrial Ti-6Al-4V.
[0045] Furthermore, the pressing and sintering forming method is cold isostatic pressing-vacuum sintering. Furthermore, during pressing, the pressing pressure is 200-400MPa, and the holding time is 0.5-3h. During vacuum sintering, the vacuum sintering temperature is 1100-1400℃, and the holding time is 1-6h. The alloy powder is prepared into blanks by cold isostatic pressing-vacuum sintering, which can shorten the cycle and reduce the equipment cost.
[0046] Step S2, using a hot extrusion process to perform a certain plastic deformation on the rod blank, and air-cooling it to room temperature to obtain a formed part.
[0047] Furthermore, the plastic deformation method uses a hot extrusion process. Specifically, the blank can be heated and kept warm in a vacuum atmosphere; the kept warm blank is placed in an extrusion die preheated to 400-500°C, hot extruded, and air-cooled to room temperature to obtain a formed part. After a blank with uniform composition is prepared by powder metallurgy, a hot extrusion process is used to make it denser and dynamically recrystallize, and then air cooling is used to allow some recrystallization to grow slightly, forming a heterogeneous structure in which strips and equiaxed structures of different scales coexist.
[0048] Furthermore, a vacuum atmosphere furnace is selected for heating and heat preservation. The heat preservation temperature is 900-1000°C and the heat preservation time is 20-60min. In addition, the heating rate can be controlled to 5-10s / °C. Before heating, the blank obtained after sintering can be placed in a sheath and then placed in a vacuum atmosphere furnace for heating. During hot extrusion forming, the extrusion ratio is controlled to 5-18 and the extrusion speed is 2-5mm / s. By selecting the above hot extrusion process conditions, the material density is further improved and a heterogeneous structure is obtained.
[0049] Step S3, heat treating and water quenching the formed part to obtain a titanium alloy with a martensitic heterostructure.
[0050] Furthermore, heat treatment is performed by resistance heating. The resistance heating method refers to processing the formed part into a plate and using it as a resistor, applying voltage for heating, and controlling the power-on time to achieve the heat treatment effect on the formed part. The present application performs heat treatment by resistance heating, which increases the heating rate, and the transformation of the β phase can be controlled by changing the heating time. Since the resistivity of the material is fixed, under a certain voltage, the temperature of the material can be controlled by controlling the time, that is, the heat treatment of the formed part can be completed, thereby obtaining a titanium alloy with a martensitic heterostructure.
[0051] Exemplarily, for example, for the material described in the present invention (resistivity is fixed), when the voltage is 110V-220V, the power-on time can be controlled to be no more than 25s. Further, the power-on time is controlled to be 4s-25s, and the heating is immediately cooled to room temperature. The power-on time is controlled to be no more than 25s under this voltage, which can prevent the sheet from melting. In addition, the resistance heating heat treatment method in the present invention can also be applied to other materials. When it is other materials, the power-on time can be appropriately adjusted in combination with the resistance difference between the material and the material of the present invention. For example, when the ratio of the finished length to the cross-sectional area of a certain material is less than the ratio of the material of the present invention, the heat treatment effect corresponding to the material can be obtained by appropriately extending the power-on time.
[0052] The microstructure of the titanium alloy of the present application is composed of martensite phase + primary α phase. Among them, the martensite shape is 1-30μm long, and the aspect ratio is greater than 10:1; α-Ti exists in a strip structure with a length of 15-40μm and an equiaxed structure with a diameter of 1-10μm. α-Ti of different shapes and sizes and martensite of different sizes constitute a martensitic heterostructure.
[0053] The titanium alloy with a martensitic heterostructure has high strength and toughness, and its room temperature tensile strength is greater than 1000MPa, and its elongation is greater than 10%; in particular, the titanium alloy with a martensitic heterostructure has a room temperature tensile strength of 1050MPa to 1300MPa, and an elongation of 11% to 30%. Further, the titanium alloy with a martensitic heterostructure has a room temperature tensile strength greater than 1200MPa and an elongation greater than 10%; or, the titanium alloy with a martensitic heterostructure has a room temperature tensile strength greater than 1000MPa and an elongation greater than 20%.
[0054] The high-strength and toughness martensitic heterostructure titanium alloy described in the present application can be used in high-strength structural parts, impact-resistant structural parts, high-strength and toughness structural parts, etc. in the fields of aerospace, shipbuilding, and automobiles.
[0055] The present application is further described in more detail below in conjunction with specific examples, but the embodiments of the present invention are not limited thereto. The materials involved in the following examples can be obtained from commercial channels unless otherwise specified. The methods described are conventional methods unless otherwise specified.
[0056] The specific test methods of the following embodiments are as follows: the microstructure of the sample is observed by an electron backscattering device; the yield strength, tensile strength and fracture strain of the sample are tested for tensile properties according to international standards (Chinese GB / T228-2002).
[0057] Embodiment 1:
[0058] A method for preparing a high-strength and high-toughness martensitic heterostructure titanium alloy comprises the following steps:
[0059] The raw materials used in this embodiment are as follows: Ti-6Al-4V alloy powder (65.68 μm).
[0060] (1) Alloy powder processing: The target alloy composition of this embodiment is Ti-6Al-4V alloy. First, the alloy powder is pressed by cold isostatic pressing at a pressing force of 300 MPa for 1.5 hours to form a rod blank with a diameter of 50 mm and a height of 100 mm.
[0061] (2) Sintering of rod blanks: The rod blanks pressed in step (1) are placed in a vacuum sintering furnace and sintered at 1250° C. for 1.5 h.
[0062] (3) Rod encapsulation: The rod sintered in step (2) is machined into two cylinders with a diameter of 47.5 mm and a height of 48 mm, and placed in a sheath made of 45 steel. The diameter of the sheathed parts is 49.5 mm and the height is 50 mm.
[0063] (4) Heating the rod blank: The sheathed blank of step (3) is placed in a vacuum atmosphere furnace and kept at 950° C. for 30 min. The vacuum atmosphere furnace needs to be filled with argon in advance, and argon is introduced into the furnace throughout the insulation process.
[0064] (5) Hot extrusion molding: The billet after heat preservation in step (4) was taken out from the vacuum atmosphere furnace, quickly placed in a preheated extrusion die, and extruded the sample at an extrusion ratio of 9.76 and an extrusion speed of 20 mm / s, and air-cooled.
[0065] (6) Resistance heating quenching: The finished product of step (5) was cut into strips with a length of 55 mm, a width of 7 mm, and a thickness of 1.7 mm and used as a resistor. The voltage was 220 V and the power-on time was 4.3 s. After the time was reached, the product was immediately dropped into water for water quenching.
[0066] Figure 1 and Figure 2 They are the phase distribution diagram and IPF diagram of the martensitic heterostructure titanium alloy obtained in Example 1. Figure 1 It can be seen that in this martensitic heterostructure, the alloy matrix phase is α phase, and a small amount of β phase exists at the α phase boundary; Figure 2 It can be seen that: the orientation information of each martensite and primary α.
[0067] The titanium alloy with martensitic heterostructure prepared in this embodiment is as follows Figure 2 As shown, the matrix is composed of martensite with a length of 1-30 μm and an aspect ratio greater than 10:1; α-Ti exists in a strip structure with a length of 15-40 μm and an equiaxed structure with a diameter of 1-10 μm. The room temperature tensile yield strength, tensile strength and elongation are 1201 MPa, 1260 MPa and 17.9% respectively (as shown in Figure 1). Figure 4 The strength and plasticity of the Ti-6Al-4V alloy prepared in this embodiment are much higher than those of the Ti-6Al-4V alloy prepared by conventional sintering and the commercial Ti-6Al-4V alloy.
[0068] Embodiment 2:
[0069] A method for preparing a high-strength and high-toughness martensitic heterostructure titanium alloy comprises the following steps:
[0070] The raw materials used in this embodiment are as follows: Ti-6Al-4V alloy powder (50.23 μm).
[0071] (1) Alloy powder processing: The target alloy composition of this embodiment is Ti-6Al-4V alloy. First, the alloy powder is pressed by cold isostatic pressing at a pressing force of 350 MPa for 1 hour to form a rod blank with a diameter of 50 mm and a height of 100 mm.
[0072] (2) Sintering of rod blanks: The rod blanks pressed in step (1) are placed in a vacuum sintering furnace and sintered at 1300° C. for 2 h.
[0073] (3) Rod encapsulation: The rod sintered in step (2) is machined into two cylinders with a diameter of 47.5 mm and a height of 48 mm, and placed in a sheath made of 45 steel. The diameter of the sheathed parts is 49.5 mm and the height is 50 mm.
[0074] (4) Heating the rod blank: The sheathed blank of step (3) is placed in a vacuum atmosphere furnace and kept at 950° C. for 30 min. The vacuum atmosphere furnace needs to be filled with argon in advance, and argon is introduced into the furnace throughout the insulation process.
[0075] (5) Hot extrusion forming: The billet after heat preservation in step (4) is taken out from the vacuum atmosphere furnace, quickly placed in a preheated extrusion die, and the sample is extruded at an extrusion ratio of 9.76 and an extrusion speed of 20 mm / s. After air cooling, a heterostructure titanium alloy is obtained.
[0076] (6) Resistance heating quenching: The finished product of step (5) was cut into strips with a length of 55 mm, a width of 7 mm, and a thickness of 1.7 mm and used as a resistor. The voltage was 220 V and the power-on time was 4.8 s. After the time was reached, the product was immediately dropped into water for water quenching.
[0077] The titanium alloy with martensitic heterostructure prepared in this embodiment has a matrix with a martensite length of 1-30 μm and an aspect ratio greater than 10:1; α-Ti exists in a strip structure with a length of 15-40 μm and an equiaxed structure with a diameter of 1-10 μm. The room temperature tensile yield strength, tensile strength and elongation are 1153 MPa, 1216 MPa and 14.9% respectively (as shown in Figure 2). Figure 4 The strength and plasticity of the Ti-6Al-4V alloy prepared in this embodiment are much higher than those of the Ti-6Al-4V alloy prepared by conventional sintering and the commercial Ti-6Al-4V alloy.
[0078] Embodiment 3:
[0079] A method for preparing a high-strength and high-toughness martensitic heterostructure titanium alloy comprises the following steps:
[0080] The raw materials used in this embodiment are as follows: Ti-6Al-4V alloy powder (80.23 μm).
[0081] (1) Alloy powder processing: The target alloy composition of this embodiment is Ti-6Al-4V alloy. First, the alloy powder is pressed by cold isostatic pressing at a pressing force of 300 MPa for 1 hour to form a rod blank with a diameter of 50 mm and a height of 100 mm.
[0082] (2) Sintering of rod blanks: The rod blanks pressed in step (1) are placed in a vacuum sintering furnace and sintered at 1300° C. for 2 h.
[0083] (3) Rod encapsulation: The rod sintered in step (2) is machined into two cylinders with a diameter of 47.5 mm and a height of 48 mm, and placed in a sheath made of 45 steel. The diameter of the sheathed parts is 49.5 mm and the height is 50 mm.
[0084] (4) Heating the rod blank: The sheathed blank of step (3) is placed in a vacuum atmosphere furnace and kept at 1000° C. for 30 min. The vacuum atmosphere furnace needs to be filled with argon in advance, and argon is introduced into the furnace throughout the insulation process.
[0085] (5) Hot extrusion molding: The billet after heat preservation in step (4) was taken out from the vacuum atmosphere furnace, quickly placed in a preheated extrusion die, and extruded the sample at an extrusion ratio of 6.25 and an extrusion speed of 20 mm / s, and air-cooled.
[0086] (6) Resistance heating quenching: The rod obtained in step (5) was cut into plates with a length of 55 mm, a width of 7 mm, and a thickness of 1.7 mm, and used as a resistor. Resistance heating was performed at a voltage of 110 V for 15 s. After water quenching, a high-strength and tough martensitic heterostructure TC4 titanium alloy was obtained.
[0087] The titanium alloy with martensitic heterostructure prepared in this embodiment is as follows Figure 3 As shown in the figure, the matrix is composed of martensite with a length of 1-25 μm and an aspect ratio greater than 10:1; α-Ti exists in a strip structure with a length of 5-30 μm and an equiaxed structure with a diameter of 1-15 μm. Figure 4 As shown, the room temperature tensile yield strength, tensile strength and elongation are 858MPa, 1097MPa and 24.2% respectively. The strength of the Ti-6Al-4V alloy prepared in this embodiment is slightly higher than that of the Ti-6Al-4V prepared by conventional sintering and the commercial Ti-6Al-4V alloy, while the plasticity is much higher than that of the Ti-6Al-4V prepared by conventional sintering and the commercial Ti-6Al-4V alloy.
[0088] The description of the present application is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the present application to the disclosed form. Many modifications and variations are obvious to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present application, and to enable those of ordinary skill in the art to understand the present application and thus design various embodiments with various modifications suitable for specific purposes.
Claims
1. A method for preparing a high-strength and high-toughness martensitic heterostructure titanium alloy, It is characterized in that The following steps are involved: Ti-6Al-4V alloy powder is used as raw material, pressed and sintered to obtain a blank; The blank is plastically deformed by a hot extrusion process to obtain a formed part; The formed part is heat treated by resistance heating, and a titanium alloy with a martensitic heterostructure is obtained by controlling the time.
2. The method for preparing the high-strength and tough martensitic heterostructure titanium alloy according to claim 1, It is characterized in that The step of heat treating the formed part by resistance heating and obtaining a titanium alloy with a martensitic heterostructure by controlling the time is to process the formed part into a plate and use it as a resistor, apply voltage for heating, control the power-on time, and water quench to obtain a titanium alloy with a martensitic heterostructure.
3. The method for preparing the high-strength and tough martensitic heterostructure titanium alloy according to claim 2, It is characterized in that When the applied voltage is 110V to 220V, the controlled power-on time is 4s to 25s.
4. The method for preparing the high-strength and toughness martensitic heterostructure titanium alloy according to claim 1, It is characterized in that The step of plastically deforming the blank by a hot extrusion process to obtain a formed part comprises: heating and keeping the blank warm in a vacuum atmosphere; The heat-insulated billet is placed in a preheated extrusion die, hot extruded and formed, and air-cooled to room temperature to obtain a formed part.
5. The method for preparing the high-strength and tough martensitic heterostructure titanium alloy according to claim 4, It is characterized in that The holding temperature is 900℃~1000℃, and the holding time is 20min~60min; The extrusion ratio is 5 to 18, and the extrusion speed is 2 mm / s to 5 mm / s; The mold preheating temperature is 400℃~500℃.
6. The method for preparing the high-strength and tough martensitic heterostructure titanium alloy according to claim 1, It is characterized in that The particle diameter of the Ti-6Al-4V alloy powder is 50-150 μm.
7. The method for preparing the high-strength and tough martensitic heterostructure titanium alloy according to claim 1, It is characterized in that The pressing and sintering adopts the cold isostatic pressing-vacuum sintering method; Among them, the pressing pressure is 200-400MPa, and the holding time is 0.5-3h; The vacuum sintering temperature is 1100-1400°C and the holding time is 1-6h.
8. The method for preparing the high-strength and toughness martensitic heterostructure titanium alloy according to claim 1, It is characterized in that The microstructure of the titanium alloy with a martensitic heterostructure consists of a martensitic phase + an initial α phase; Among them, the martensite is in the shape of strips, 1 to 30 μm long, and the aspect ratio is greater than 10:1; α-Ti exists in the form of strip structures with a length of 10 to 50 μm and equiaxed structures with a diameter of 1 to 15 μm.
9. A high-strength and tough martensitic heterostructure titanium alloy prepared according to the method for preparing a high-strength and tough martensitic heterostructure titanium alloy according to any one of claims 1 to 8.
10. The high-strength and tough martensitic heterostructure titanium alloy according to claim 9, It is characterized in that The room temperature tensile strength of the titanium alloy with a martensitic heterostructure is greater than 1200 MPa, and the elongation is greater than 10%; or the room temperature tensile strength of the titanium alloy with a martensitic heterostructure is greater than 1000 MPa, and the elongation is greater than 20%.
11. Application of a high-strength and tough martensitic heterostructure titanium alloy prepared by the method for preparing a high-strength and tough martensitic heterostructure titanium alloy according to any one of claims 1 to 8 in high-strength and / or high-toughness structural parts in the fields of aerospace, shipbuilding, and automobiles.
Citation Information
Cited By
Laser powder bed molten high-strength and high-plasticity TA15 titanium alloy and preparation method and application thereof
CN121315280A
Preparation method of microtexture heterostructure titanium alloy and microtexture heterostructure titanium alloy
CN121826421A