Semiconductor device and method of manufacturing the same

By depositing high-k materials on the semiconductor fin structure and performing the CMP process, the short channel effect and static electricity control problems are solved, high-efficiency and low-power integrated circuit manufacturing is achieved, and the process flow is simplified.

CN118800728APending Publication Date: 2024-10-18TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311474874.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-20
Filing Date
2023-11-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In semiconductor manufacturing, as the size of electronic devices shrinks, short channel effect (SCE) and static electricity control challenges increase. Existing multi-gate devices such as FinFET and GAA devices have challenges in maintaining gate control and mitigating SCE, and the manufacturing process Increased complexity makes it difficult to implement low-cost, high-performance, and low-power integrated circuits.

Method used

By forming multiple fin structures separated by isolation materials, depositing a high dielectric constant (high-k) material on the fin structures and isolation materials, and then depositing a capping layer and removing it through a chemical mechanical planarization (CMP) process The top cap layer and the upper part of the high-k material define the high-k insulation section and optimize the gate structure.

Benefits of technology

It achieves better electrostatic control and short channel effect mitigation, improves gate control capabilities, simplifies the manufacturing process, reduces cost and power consumption, and improves the performance and scalability of integrated circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800728A_ABST
    Figure CN118800728A_ABST
Patent Text Reader

Abstract

The invention provides a semiconductor device and a manufacturing method thereof. An exemplary method includes forming a plurality of fin structures separated by an isolation material; depositing a high-k material over the plurality of fin structures and the isolation material, wherein the high-k material includes a plurality of lower portions between the plurality of fin structures and an upper portion over the plurality of fin structures; depositing a topographic modifying cap layer over the high-k material; a chemical mechanical planarization (CMP) process is performed to remove the cap layer and the upper portion of the high-k material and define a plurality of high-k insulation segments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a semiconductor device and a method for manufacturing the same. Background Art

[0002] The electronics industry has experienced a continuously increasing demand for smaller and faster electronic devices that are simultaneously capable of supporting a greater number of increasingly intricate and complex functions. Thus, there is a continuing trend in the semiconductor industry to manufacture low-cost, high-performance, and low-power integrated circuits (ICs). To date, the demand has been largely met by scaling down semiconductor IC dimensions (e.g., minimum feature size) and thereby improving production efficiency and reducing associated costs. However, such scaling has also introduced increased complexity to the semiconductor manufacturing process. Thus, the realization of continued advancements in semiconductor ICs and devices requires similar advancements in semiconductor manufacturing processes and technologies.

[0003] Multi-gate devices have been introduced in an effort to improve gate control, reduce off-state current, and reduce short-channel effect (SCE) by increasing gate-channel coupling. One such multi-gate device that has been introduced is the fin field-effect transistor (FinFET). FinFETs derive their name from the fin-like structure that extends from a substrate on which the fin-like structure is formed, and the fin-like structure is used to form the FET channel. Another multi-gate device that was introduced in part to address the performance challenges associated with FinFETs is the gate-all-around (GAA) transistor. GAA devices derive their name from the gate structure that extends completely around the channel, thereby providing better electrostatic control than FinFETs. FinFET devices and GAA devices are compatible with complementary metal-oxide-semiconductor (CMOS) processes. In addition, the three-dimensional structure of such devices allows the devices to be aggressively scaled while maintaining gate control and mitigating SCE. Summary of the invention

[0004] Some embodiments of the present disclosure provide a method for manufacturing a semiconductor device, comprising the following steps: forming a plurality of fin structures separated by an isolation material; depositing a high-k material over the plurality of fin structures and the isolation material, wherein the high-k material includes a plurality of lower portions located between the plurality of fin structures and an upper portion located over the plurality of fin structures; depositing a cap layer over the high-k material; and performing a chemical mechanical planarization process to remove the cap layer and the upper portion of the high-k material and define a plurality of high-k insulating segments.

[0005] Some embodiments of the present disclosure provide a method for manufacturing a semiconductor device, comprising the following steps: forming a fin structure; forming a high-k isolation region laterally adjacent to the fin structure, wherein the high-k isolation region has an upper surface; and removing a top layer of the fin structure to form the fin structure having an uppermost surface, the uppermost surface being located at a height below the upper surface of the high-k isolation region.

[0006] Some embodiments of the present disclosure provide a semiconductor device, comprising: a semiconductor fin structure; a gate structure located above the semiconductor fin structure; and a hafnium oxide isolation region laterally adjacent to the semiconductor fin structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] The aspects of this disclosure are in the attached Figure 1 The following detailed description is best understood when read together. It should be noted that, in accordance with standard industry practice, various features are not drawn to scale. In fact, the dimensions of the various features may be arbitrarily increased or reduced for clarity of discussion.

[0008] Figure 1 is a flow chart illustrating a method according to some embodiments;

[0009] Figures 2 to 3 is a perspective view of a device during a subsequent manufacturing stage according to some embodiments;

[0010] Figures 4 to 13 According to some embodiments Figure 3 a cross-sectional view of a partially fabricated device during a subsequent fabrication stage;

[0011] Fig.14 An isolation region above a dielectric material layer and between active regions such as fin structures, such as in Fig.12 A focused perspective view during a manufacturing stage of and according to some embodiments;

[0012] Fig.15 for Fig.14 A cross-sectional view of the structure;

[0013] Figures 16 to 18 is a schematic diagram of a multi-layer isolation region according to some embodiments;

[0014] Figures 19 to 21 is a schematic diagram of isolation regions having different bottom surfaces according to some embodiments;

[0015] Figure 22 to Figure 25 For partially manufacturing devices according to some embodiments such as in Fig.12 A simplified top view layout diagram of the manufacturing stage;

[0016] Fig.26 For devices such as Fig.12 Cross-sectional view during a manufacturing stage of and according to some embodiments.

[0017]

Explanation of symbols

[0018] 100:Substrate

[0019] 101: Bottom part

[0020] 102: Unetched part

[0021] 110: Epitaxial stacking

[0022] 114: epitaxial layer / epitaxial growth layer / semiconductor layer

[0023] 115: Top layer

[0024] 116: epitaxial layer / epitaxial growth layer / semiconductor layer

[0025] 117: Top layer

[0026] 120: Isolation / Shallow Trench Isolation Features / Isolation Features / STI Features

[0027] 130: Lining

[0028] 140: Spacer layer

[0029] 150: Dielectric material

[0030] 152: Surface

[0031] 155: Gap

[0032] 160: High dielectric constant materials / high-k materials

[0033] 161: horizontal or flat surface

[0034] 162: concave part

[0035] 165: Lower part

[0036] 168: Upper part

[0037] 170: Top cover

[0038] 180: High-k isolation area / multi-layer isolation area

[0039] 181: Top surface

[0040] 182: Bottom surface

[0041] 185: Opening

[0042] 186: Side wall

[0043] 188: Lower part

[0044] 189: Upper part

[0045] 190: Interlayer dielectric

[0046] 200: Installation

[0047] 205:Unit Cell

[0048] 210: Metal

[0049] 220: Interlayer dielectric

[0050] 230: Contact

[0051] 240: Interface

[0052] 1171: Surface

[0053] 1601: Layer

[0054] 1602: Layer

[0055] 1603: Interface

[0056] 1821: Center plane section

[0057] 1822: Angle section

[0058] 1823: Interface

[0059] 1824: Inverted angled portion

[0060] 1825: Interface

[0061] A1: Interior angle / angle

[0062] A2:Inner angle / angle

[0063] D1: Lateral distance

[0064] F10~F14: Fin structure / fin

[0065] G10: Gate

[0066] H1: Height

[0067] H2: Height

[0068] H3: Height

[0069] H4: Height

[0070] H5: Height

[0071] L1: Length

[0072] M10: Method

[0073] O11: Operation

[0074] O12: Operation

[0075] O13: Operation

[0076] O14: Operation

[0077] O15: Operation

[0078] O16: Operation

[0079] O17: Operation

[0080] O18: Operation

[0081] O19: Operation

[0082] O20: Operation

[0083] O21: Operation

[0084] O22: Operation

[0085] O23: Operation

[0086] T10~T13: Groove

[0087] T1: Thickness

[0088] W11: Width

[0089] W12: Width

[0090] W13: Width

[0091] W1: Width

[0092] W2: Width DETAILED DESCRIPTION

[0093] The following disclosure provides many different embodiments or examples for implementing different features of the subject matter. Specific examples of components and configurations are described below to simplify the present disclosure. Of course, these components and configurations are only examples and are not intended to be restrictive. For example, in the following description, forming a first feature above or on a second feature may include an embodiment in which the first and second features are formed in direct contact, and may also include an embodiment in which additional features may be formed between the first and second features so that the first and second features may not be in direct contact. In addition, the present disclosure may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.

[0094] Additionally, spatially relative terms, such as "above," "overlying," "over," "upper," "top," "below," "underlying," "beneath," "below," "lower," "bottom," "side," and the like may be used herein for ease of description to describe the relationship of one element or feature to another element or feature as illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein may likewise be interpreted accordingly.

[0095] In certain embodiments herein, a "material layer" is a layer that includes at least 50 wt.% of the identified material, such as at least 60 wt.% of the identified material, at least 75 wt.% of the identified material, or at least 90 wt.% of the identified material, or substantially 100 wt.% of the identified material; and is a layer of "material" that includes at least 50 wt.% of the identified material, such as at least 60 wt.% of the identified material, at least 75 wt.% of the identified material, or at least 90 wt.% of the identified material, or substantially 100 wt.% of the identified material. For example, each of a titanium nitride layer and a layer that is titanium nitride is a titanium nitride layer of at least 50 wt.%, at least 60 wt.%, at least 75 wt.%, or at least 90 wt.% or substantially 100 wt.%.

[0096] As used herein, the terms "approximately," "substantially," "substantially," and "about" are used to describe a value and a small change. When used in conjunction with an event or situation, the term may refer to an instance where the event or situation occurs precisely and an instance where the event or situation occurs approximately. For example, when used in conjunction with a numerical value, the term may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. For example, if the difference between the values ​​is less than or equal to ±10% of the average value of the values, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%, then two numerical values ​​may be considered to be "substantially" the same or equal. For example, "substantially" parallel may refer to an angular range relative to 0° that is less than or equal to ±10°, such as less than or equal to ±5°, less than or equal to ±4°, less than or equal to ±3°, less than or equal to ±2°, less than or equal to ±1°, less than or equal to ±0.5°, less than or equal to ±0.1°, or less than or equal to ±0.05°. For example, "substantially" perpendicular may refer to an angular range relative to 90° that is less than or equal to ±10°, such as less than or equal to ±5°, less than or equal to ±4°, less than or equal to ±3°, less than or equal to ±2°, less than or equal to ±1°, less than or equal to ±0.5°, less than or equal to ±0.1°, or less than or equal to ±0.05°.

[0097] For the sake of brevity, known techniques for the manufacture of semiconductor devices may not be described in detail herein. In addition, the various tasks and processes described herein may be incorporated into more comprehensive procedures or processes having additional functionality that is not described in detail herein. In particular, the various processes in the manufacture of semiconductor devices are well known, and therefore, for the sake of brevity, many processes will only be briefly mentioned herein, or will be omitted entirely without providing well-known process details. As will be readily apparent to those skilled in the art, after a complete reading of this disclosure, the structures disclosed herein may be used with a variety of techniques and may be incorporated into a variety of semiconductor devices and products. In addition, it should be noted that the semiconductor device structure includes a variable number of components, and a single component depicted in the diagram may represent multiple components.

[0098] Note also that the present disclosure presents embodiments in the form of multi-gate transistors. Multi-gate transistors include those transistors where gate structures are formed on at least two sides of a channel region. These multi-gate devices may include P-type metal oxide semiconductor devices, or N-type metal oxide semiconductor multi-gate devices. Specific examples may be presented and are referred to herein as FinFET devices due to their fin-like structures. Also presented herein are embodiments of a type of multi-gate transistor referred to as a gate-all-around (GAA) device. A GAA device includes any device having a gate structure or portion thereof formed on four sides of a channel region (e.g., surrounding a portion of a channel region). The devices presented herein also include embodiments having a channel region arranged in a nanosheet channel, a nanowire channel, a rod-shaped channel, and / or other suitable channel configurations. As used herein, the term "nanosheet" is intended to include nanowires and rod-shaped configurations.

[0099] The all-around gate (hereinafter, "GAA") transistor structure can be patterned by any suitable method. For example, the structure can be patterned using one or more optical lithography processes including double patterning or multiple patterning processes. Typically, the double patterning or multiple patterning process combines the optical lithography process with a self-aligned process, thereby allowing patterns to be produced, and the multiple patterns have, for example, a smaller pitch than otherwise obtainable using a single direct optical lithography process. For example, in one embodiment, a sacrificial layer is formed over a substrate and patterned using an optical lithography process. Spacers are formed along the patterned sacrificial layer using a self-aligned process. The sacrificial layer is then removed, and the remaining spacers can then be used to pattern the GAA structure.

[0100] As described herein, processes are performed to isolate adjacent fin structures. For example, high-k isolation structures are formed between adjacent fin structures, such as during front-end-of-line (FEOL) processing and before gate formation. Thus, after gate formation, no material laterally adjacent to the gate needs to be etched to form the isolation region. Additionally, the use of high-k isolation regions provides a reduction in cell height compared to other isolations.

[0101] In some embodiments, the high-k material is polished during a chemical mechanical planarization (CMP) process that is performed with a silicon oxide-based slurry that provides high selectivity. In some embodiments, the high-k material is hafnium oxide. In some embodiments, the CMP process defines the shape of the high-k isolation region.

[0102] In an exemplary embodiment, the CMP process includes three stages for selective planarization. The first stage removes the cap layer above the high-k isolation material and lands on the high-k isolation material; the second stage removes the high-k isolation material above the underlying fin structure and lands on the fin structure; and the third stage provides height control of the formed high-k isolation region. The first stage is selective to remove the cap layer, the second stage is selective to remove the high-k isolation material, and the third stage is non-selective. The three-stage CMP process with selected selectivity achieves improved within-wafer (WiW), within-die (WiD), and wafer-to-wafer (WtW) uniformity.

[0103] In an exemplary embodiment, the high-k isolation region is a multilayer structure formed of a high-k material layer and of an insertion layer, and the plurality of layers may be provided to improve certain properties of the high-k material layer. For example, the insertion layer may be formed of a material that improves the crystal uniformity of the high-k material. In some embodiments, the high-k isolation region is formed of a hafnium oxide layer and a silicon oxide insertion layer.

[0104] Embodiments of the present disclosure provide advantages over the prior art, although it should be understood that other embodiments may provide different advantages, not all advantages are necessarily discussed herein, and no particular advantage is required for all embodiments. For example, the embodiments discussed herein include fin structures and related front-end-of-line (FEOL) processing prior to forming sacrificial gates, replacement metal gates, and other processing.

[0105] For the purpose of the following discussion, Figure 1 A flow chart of a method M10 for manufacturing a semiconductor device is provided. Figure 1 Combination Figures 2 to 13 To describe, Figures 2 to 13 A semiconductor device 200 is illustrated at various stages of fabrication according to some embodiments of the present disclosure according to method M10. Method M10 is merely an example and is not intended to limit the present disclosure beyond what is expressly recited in the claims. Additional steps may be provided before, during, and after method M10, and some of the steps described may be moved, replaced, or eliminated for additional embodiments of method M10. Additional features may be added to the semiconductor devices depicted in the figures, and some of the features described below may be replaced, modified, or eliminated in other embodiments of the semiconductor device.

[0106] As with other method embodiments and exemplary devices discussed herein, it should be understood that portions of semiconductor device 200 may be fabricated by typical semiconductor technology process flows, and therefore some processes are only briefly described herein. Additionally, the exemplary semiconductor device may include various other devices and features, such as other types of devices, such as additional transistors, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, and / or other logic devices, etc., but are simplified for a better understanding of the concepts of the present disclosure. In some embodiments, the exemplary device includes a plurality of semiconductor devices (e.g., transistors) that may be interconnected, including PFETs, NFETs, etc. Additionally, please note that the process steps of method M10, including any description given with reference to the figures, as well as the remainder of the methods and exemplary figures provided in the present disclosure are generally merely illustrative and are not intended to be limited beyond what is specifically stated in the following claims.

[0107] At operation O11, method M10 ( Figure 1 ) provides a substrate 100, such as Figure 2 . In some embodiments, the substrate 100 may be a semiconductor substrate, such as a silicon (Si) substrate. The substrate 100 may include various layers, including conductive layers or insulating layers formed on the semiconductor substrate. The substrate 100 may include various doping configurations according to design requirements as known in the art. For example, different doping profiles (e.g., p-type well, n-type well) may be formed on the substrate 100 in regions designed for different device types (e.g., n-type field effect transistor (NFET), p-type field effect transistor (PFET)). Suitable doping may include ion implantation and / or diffusion processes of dopants, such as boron (B) for p-type wells and phosphorus (P) for n-type wells. In some embodiments, the substrate 100 includes a single crystalline semiconductor layer on at least a surface portion of the substrate 100. The substrate 100 may include a single crystal semiconductor material such as, but not limited to, Si, Ge, SiGe, GaAs, InSb, GaP, GaSb, InAlAs, InGaAs, GaSbP, GaAsSb, and InP. Alternatively, the substrate 100 may include a compound semiconductor and / or an alloy semiconductor. In the illustrated embodiment, the substrate 100 is made of crystalline Si.

[0108] At operation O12, method M10 forms an epitaxial layer stack over substrate 100. Epitaxial stack 110 includes an epitaxial layer 114 of a first composite intercalated by an epitaxial layer 116 of a second composite. The first composite and the second composite may be different. Embodiments are possible that include those epitaxial layers that provide first composites and second composites with different oxidation rates and / or etch selectivities. In an embodiment, epitaxial layer 114 is silicon germanium (SiGe) and epitaxial layer 116 is silicon (Si). In embodiments where epitaxial layer 114 includes SiGe and epitaxial layer 116 includes silicon, the silicon oxidation rate is less than the SiGe oxidation rate. Note that five layers of epitaxial layer 114 and four layers of epitaxial layer 116 are illustrated in FIG. Figure 2 middle, Figure 2 It is for illustrative purposes only and is not intended to be limiting beyond what is specifically described in the claims. It is understood that any number of epitaxial layers may be formed in the epitaxial stack 110; the number of layers is based on the desired number of channel regions of the GAA device 200. In some embodiments, the number of epitaxial layers 116 is between two and ten, such as six or seven.

[0109] As shown, the epitaxial stack 110 includes an uppermost or top layer 117 of the epitaxial layers 116 , and an uppermost or top layer 115 of the epitaxial layers 114 .

[0110] In some embodiments, each epitaxial layer 114 has a thickness ranging from about 5 nm to about 15 nm. The thickness of the epitaxial layer 114 can be substantially uniform. In the illustrated embodiment, the top layer 115 has a greater thickness than the other epitaxial layers 114.

[0111] In some embodiments, each epitaxial layer 116 has a thickness ranging from about 5 nm to about 15 nm. In some embodiments, the thickness of the stacked epitaxial layers 116 is substantially uniform. As described in more detail below, the epitaxial layers 116 can serve as channel regions of subsequently formed multi-gate devices and have a thickness selected based on device performance considerations. The epitaxial layer 114 can be used to define gaps between adjacent channel regions of subsequently formed multi-gate devices and have a thickness selected based on device performance considerations.

[0112] By way of example, the epitaxial growth of epitaxial stack 110 may be performed by a molecular beam epitaxy (MBE) process, a metalorganic chemical vapor deposition (MOCVD) process, and / or other suitable epitaxial growth process. In some embodiments, the epitaxially grown layers, such as epitaxial layer 116, include the same material as substrate 100. In some embodiments, epitaxially grown layers 114 and 116 include a material different from substrate 100. As stated above, in at least some embodiments, epitaxial layer 114 includes epitaxially grown Si 1-x Ge x layer (where x is about 0.10 to about 0.55), and the epitaxial layer 116 includes an epitaxially grown silicon (Si) layer. Alternatively, in some embodiments, any of the epitaxial layers 114 and 116 may include other materials, such as germanium; compound semiconductors, such as silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide and / or indium antimonide; alloy semiconductors, such as SiGe, GaAsP, AlInAs, AlGaAs, InGaAs, GaInP and / or GaInAsP; or combinations thereof. As discussed above, the materials of the epitaxial layers 114 and 116 may be selected based on providing different oxidation and etching selectivity properties. In various embodiments, the epitaxial layers 114 and 116 are substantially free of dopants (i.e., have a thickness from about 0 cm to about 10 cm). -3 About 1×10 17 cm -3 In some embodiments, the bottom layer and the top layer of the epitaxial stack 110 are SiGe layers. In an alternative embodiment, the bottom layer of the epitaxial stack 110 and the top layer of the epitaxial stack 110 are SiGe layers.

[0113] Cross-reference Figure 1 and Figure 3 , method M10 further includes: (O13) forming a fin structure extending along a first direction above the substrate 100. Specifically, at operation O13, method M10 patterns the epitaxial stack 110 to form a semiconductor fin structure F10, such as fin structures F11, F12, F13, and F14. In some embodiments, operation O13 includes: forming a mask layer (not shown) on the epitaxial stack 110; patterning the mask layer; patterning the epitaxial stack 110 through openings defined in the patterned mask layer in an etching process, such as dry etching (e.g., reactive ion etching), wet etching, and / or other suitable processes. The stacked epitaxial layers 114 and 116 and a portion 101 of the underlying substrate 100 are thereby patterned into the fin structure F10. Although Figure 3The formation of four fin structures F10 is shown, but any suitable number of fins may be formed. Trenches T10 are etched between adjacent fin structures F10, such as trench T11, trench T12, and trench T13.

[0114] In various embodiments, each fin structure F10 includes an upper portion of staggered epitaxial layers 114 and 116, and a bottom portion 101 formed from an etched substrate 100. The fin structures F10 protrude upward from an unetched portion 102 of the substrate 100 in the Z direction, extend longitudinally in the X direction, and are spaced apart in the Y direction. The sidewalls of each fin structure F10 may be straight or inclined (not shown). The fin structures F10 may have the same width or different widths.

[0115] Figure 3 Four fin structures F10 (individually labeled as F11, F12, F13, and F14) are shown for illustration purposes but not for limitation of the present disclosure. It should be noted that the width W11 of the trench T11 formed between the fin structures F11 and F12 is greater than the width W12 of the trench T12 between the fin structures F12 and F13, and the width W11 is substantially the same as the width W13 of the trench T13 between the fin structures F13 and F14. In some embodiments, the four fin structures F11, F12, F13, and F14 are repeatedly arranged as a unit above the substrate 100, and the trench formed between the fin structure F14 and the adjacent fin structure F11 has a width substantially the same as the width W12.

[0116] Cross-reference Figure 1 and Figure 4 , the method M10 further includes: (O14) forming an isolation 120 around the fin structure F10 and above the unetched portion 102 of the substrate 100. Note that, Figure 4 and subsequent Figures 5 to 13 For clarity and ease of description provided Figure 3 FIG. 2 is a cross-sectional view of a portion of the device 200 (three fin structures F12 , F13 , and F14 ) along the YZ plane.

[0117] In an exemplary embodiment, the isolation 120 can be considered as a shallow trench isolation (STI) feature in the trench adjacent to each fin structure F10. The STI feature 120 can be formed by first filling the trench around each fin structure F10 with a dielectric material layer to cover the top surface and sidewalls of the fin structure F10 (not shown). The dielectric material layer may include one or more dielectric materials. Suitable dielectric materials for the dielectric layer may include silicon oxide, silicon nitride, silicon carbide, fluorosilicate glass (FSG), low-K dielectric materials, and / or other suitable dielectric materials. The dielectric material may be deposited by any suitable technique including thermal growth, flow CVD (FCVD), HDP-CVD, PVD, ALD and / or spin coating techniques. The dielectric material layer is then planarized by using, for example, chemical mechanical planarization (CMP) until the top surface of the mask layer (not shown) is exposed and the dielectric material layer is recessed to form shallow trench isolation (STI) features 120, such as Figure 4 . In the illustrated embodiment, the STI feature 120 is formed on the substrate 100. Any suitable etching technique including dry etching, wet etching, RIE and / or other etching methods may be used to recess the isolation feature 120, and in an exemplary embodiment, anisotropic dry etching is used to selectively remove the dielectric material of the isolation feature 120 without etching the fin structure F10. The mask layer may also be removed before, during and / or after the recessing of the isolation feature 120. In some embodiments, the mask layer is removed by a CMP process performed before recessing the isolation feature 120. In some embodiments, the mask layer is removed by an etchant used to recess the isolation feature 120.

[0118] Cross-reference Figure 1 and Figure 5 The method M10 further includes: (O15) selectively growing a semiconductor liner 130 over the fin structure F10. In an exemplary embodiment, the semiconductor liner 130 may be SiGe.

[0119] In addition, the method M10 includes: (O16) depositing a spacer layer 140 over the fin structure F10 and the STI feature 120. In an exemplary embodiment, the spacer layer 140 may include a spacer material such as silicon oxide, silicon nitride, silicon carbide, silicon oxynitride, SiCN film, silicon oxycarbide, SiOCN film and / or a combination thereof. In some embodiments, the spacer layer 140 includes a plurality of layers, such as a liner layer and a main spacer layer. By way of example, the spacer layer 140 may be formed by depositing a spacer material using a subatmospheric CVD (SACVD) process, a flow CVD process, an ALD process, a PVD process, or other suitable processes, respectively.

[0120] Cross-reference Figure 1 and Figure 6 , the method M10 further includes: (O17) depositing a dielectric material 150 over the fin structure F10. In an exemplary embodiment, the dielectric material may be silicon oxide. In an exemplary embodiment, the dielectric material 150 is blanket deposited.

[0121] In addition, the method M10 includes (O18) recessing the dielectric material 150 and the spacer layer 140 above the fin structure F10, such as Figure 6 As shown in FIG. 1 , the gap 155 is formed between the fin structures F10 and laterally adjacent to the upper portion of the fin structures F10 . The gap 155 is formed with a vertical height H1 in the Z direction. In an exemplary embodiment, the height H1 is substantially equal to the sum of the vertical thicknesses of the top layer 115 and the semiconductor liner 130 .

[0122] Cross-reference Figure 1 and Figure 7 , method M10 continues with operation O19 of depositing a high dielectric constant material 160, i.e., a high κ or high-k material, over the fin structure F10. Specifically, the high-k material 160 may be deposited on the dielectric material 150, the spacer layer 140, and the semiconductor liner 130. As used herein, a high dielectric constant material has a dielectric constant greater than 3.9. In an exemplary embodiment, the dielectric constant of the high-k material 160 is greater than 7. In an exemplary embodiment, the high-k material 160 includes a metal oxide, such as hafnium oxide (HfO2).

[0123] In an exemplary embodiment, the high-k material 160 may be deposited by atomic layer deposition (ALD). Other deposition processes may be used, such as plasma enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), metal organic chemical vapor deposition (MOCVD), plasma enhanced atomic layer deposition method (PEALD), or similar deposition processes.

[0124] In an exemplary embodiment, the high-k material 160 is conformally deposited. Therefore, the high-k material 160 forms a substantially horizontal or planar surface 161 in high pattern density areas of the device 200, such as above the fin structure F12, the trench T12, and the fin structure F13. In addition, the high-k material 160 forms a pit or recess 162 in low pattern density areas of the device 200, such as above the trench T13 between the fin structure F13 and the fin structure F14.

[0125] As shown, a lower portion 165 of the high-k material 160 is laterally adjacent to and / or positioned between adjacent fin structures F10 , and an upper portion 168 of the high-k material 160 is located above the fin structure F10 , i.e., at a greater height above the substrate 100 than the fin structure F10 .

[0126] Cross-reference Figure 1 and Figure 8 , method M10 continues with operation O20 of forming a cap layer 170 over the high-k material 160. In an exemplary embodiment, the cap layer 170 is a dielectric layer, such as a silicon oxide (SiO2) layer. In an exemplary embodiment, the cap layer 170 is provided to modify the topography of the high-k material 160. In an exemplary embodiment, the cap layer 170 is conformally deposited. For example, the cap layer 170 can be deposited by plasma enhanced chemical vapor deposition (PECVD) of another suitable process.

[0127] Cross-reference Figure 1 and Figures 9 to 11The method M10 further includes performing a chemical mechanical planarization (CMP) process at operation O21. Specifically, the exemplary CMP process includes three stages. In the first stage and as Fig. 9 , the CMP process selectively etches the cap layer 170 and lands on the high-k material 160. A portion of the cap layer 170 may remain in the recess 162. In an exemplary embodiment, the first stage of the CMP process may be performed with a chemistry that provides a removal rate of about 1000 angstroms per minute for the silicon oxide cap layer 170 and a selectivity of 50. Additionally, the amount of high-k material removed by the first stage of the CMP process may be limited to less than 1 nanometer. In an exemplary embodiment, the silicon oxide recess is 4 nanometers at a 0.3 micron spacing.

[0128] like Fig.10 As shown in FIG. 8 , the second stage of the CMP process is highly selective to etching the cap layer 170 and the high-k material 160 , and lands on the semiconductor material of the fin structure F10 , ie, the semiconductor liner 130 (not shown) or the top layer 115 .

[0129] In an exemplary embodiment, the second stage of the CMP process is performed with a slurry formulation containing a silicon oxide (SiO2) abrasive. In addition, in an exemplary embodiment, a silicon oxide-based slurry is used with HNO3. In an exemplary embodiment, the pH value of the slurry formulation is from 1 to 5, such as from 2 to 4, for example, from 2.5 to 3.5, such as a pH value of 3. In an exemplary embodiment, the second stage of the CMP process provides a controlled pH value to increase a removal rate of high-k materials while suppressing the removal rate of fin structures. Therefore, the second stage of the CMP process is highly selective for etching high-k materials.

[0130] like Fig.11 As shown in FIG. 1 , the third stage of the CMP process is then performed to provide selective height control of the high-k material 160. In an exemplary embodiment, the third stage is non-selective to etch the high-k material 160 or the semiconductor material of the fin structure F10.

[0131] Cross-reference Figure 1 and Fig.12 , method M10 continues with operation O22 of removing the top layer 115 of semiconductor material, including laterally adjacent portions of the semiconductor liner 130. For example, the top layer 115 and laterally adjacent portions of the semiconductor liner 130 may be removed by an etching process that is selective to the material of the top layer 115 and the liner 130, such as SiGe.

[0132] therefore, Fig.12The partially fabricated semiconductor device 200 has high-k isolation regions 180 separated in a lateral direction along the Y direction by openings 185. In addition, each high-k isolation region 180 is formed with an uppermost or top surface 181 that is located at a vertical height H2 above the uppermost surface 1171 of the top layer 117 of the fin structure F10.

[0133] Please note that Fig.12 1, the top surface of the top layer 117 and the bottom surface of the high-k isolation region 180 are substantially coplanar, that is, the height H2 of the high-k isolation region 180 is equal to the height H3 of the opening 185 or the removed top layer 115. However, it is contemplated that the height H2 and the height H3 are different. In some embodiments, the height H3 of the opening 185 is less than the height H2 of the high-k isolation region 180.

[0134] Cross-reference Figure 1 and Fig.13 , method M10 continues with operation O23 for further processing of manufacturing semiconductor device 200. For example, further processing may include: depositing polysilicon, patterning the polysilicon to define a polysilicon gate, depositing an interlayer dielectric (ILD) 190 around the polysilicon gate, performing a CMP process to open the polysilicon gate, removing the polysilicon gate, removing the semiconductor layer 114 and defining the remaining semiconductor layer 116 as separated nanosheets, depositing metal 210 between and over the remaining semiconductor layer 116 to form a metal gate G10 over the fin structure F10, forming an interlayer dielectric 220 over the metal gate G10, and forming a contact 230 to the metal gate G10. This further processing produces Fig.13 The structure of the semiconductor device 200 is manufactured in part.

[0135] As shown, when the metal gate material 210 is deposited over the fin structure F10, the high-k isolation region 180 is already present adjacent to the metal gate G10 and isolates the adjacent metal gate G10 from each other. Therefore, the method M10 does not include etching a trench laterally adjacent to the metal gate G10 after the metal gate material 210 is deposited.

[0136] Figures 14 to 21 Other embodiments of high-k isolation regions 180 formed of a high-k material 160 such as hafnium oxide (HfO 2 ) are shown. Fig.14 Provide a portion of the manufacturing apparatus 200 in a manner similar to Fig.12 A perspective view of a stage at a stage of manufacturing. Fig.15 supply Fig.14 A cross-sectional view of the high-k isolation region 180 of the device 200, such as along the YZ plane. Fig.14 and Fig.15The spacer layer 140 in Fig.14 and Fig.15 The portion of the dielectric material 150 is shown in FIG.

[0137] Cross-reference Fig.14 and Fig.15 , each high-k isolation region 180 is formed with a vertical height H2 from the bottom surface 182 to the top surface 181. As shown, the top surface 181 of each high-k isolation region 180 is located at a vertical height H4 from the top surface 1171 of the fin structure F10. In the illustrated embodiment, the vertical height H2 is greater than the vertical height H4. Therefore, the high-k isolation region 180 includes a lower portion 188 located below the surface 1171 of the fin structure F10 and an upper portion 189 located above the surface 1171 of the fin structure F10. The lower portion 188 has a vertical height H5 from the bottom surface 182 to the surface 1171. The upper portion 189 has a vertical height H4 from the top surface 181 to the surface 1171. The total height H2 is equal to the sum of the height H4 and the height H5.

[0138] In an exemplary embodiment, the vertical height H4 is from 5 nanometers (nm) to 100 nanometers (nm). For example, the vertical height H4 may be at least 5 nm, at least 10 nm, at least 15 nm, at least 20 nm, at least 25 nm, at least 30 nm, at least 35 nm, at least 40 nm, at least 45 nm, at least 50 nm, at least 60 nm, at least 70 nm, at least 80 nm, or 90 nm. In addition, the vertical height H4 may be at most 10 nm, at most 15 nm, at most 20 nm, at most 25 nm, at most 30 nm, at most 35 nm, at most 40 nm, at most 45 nm, at most 50 nm, at most 60 nm, at most 70 nm, at most 80 nm, at most 90 nm, or at most 100 nm.

[0139] In an exemplary embodiment, the vertical height H5 is from 0 nanometers (nm) to 20 nanometers (nm). For example, the vertical height H5 may be at least 1 nm, at least 5 nm, at least 10 nm, or at least 15 nm, and may be at most 20 nm, at most 15 nm, at most 10 nm, or at most 5 nm. It is further contemplated that the bottom surface 182 may be located at a vertical height above the surface 1171 of the fin structure F10. In such embodiments, the vertical height H5 may be considered negative and may be between 0 nanometers (nm) and -20 nanometers (nm). In such embodiments, the vertical height H2 from the bottom surface 182 to the top surface 181 is less than the vertical height H4 from the surface 1171 to the top surface 181.

[0140] In certain embodiments, the ratio of height H4:height H5 is from 1:10 to 10: 1. For example, the ratio of H4:H5 can be at least 1:10, at least 2:10, at least 3:10, at least 4:10, at least 5:10; at least 6:10; at least 7:10; at least 8:10; at least 9:10; at least 10:10; at least 10:9; at least 10:8; at least 10:7; at least 10:6; at least 10:5; at least 10:4; at least 10:3; or at least 10:2. In addition, the H4:H5 ratio may be at most 2:10, at most 3:10, at most 4:10, at most 5:10; at most 6:10; at most 7:10; at most 8:10; at most 9:10; at most 10:10; at most 10:9; at most 10:8; at most 10:7; at most 10:6; at most 10:5; at most 10:4; at most 10:3; or at most 10:2, or at most 10:1.

[0141] As shown, each high-k isolation region 180 is formed with a longitudinal length L1 in the X direction and a lateral width W1 in the Y direction. In addition, the high-k isolation regions 180 are separated by a lateral distance D1 in the Y direction.

[0142] In an exemplary embodiment, the high-k isolation region 180 independently has a length L1 of 10 nanometers (nm) to 500 nanometers (nm) in the X direction. For example, the length L1 may be at least 10 nm, at least 15 nm, at least 20 nm, at least 25 nm, at least 30 nm, at least 35 nm, at least 40 nm, at least 45 nm, at least 50 nm, at least 60 nm, at least 70 nm, at least 80 nm, at least 90 nm, at least 100 nm, at least 120 nm, at least 140 nm, at least 160 nm, at least 180 nm, at least 200 nm, at least 250 nm, at least 300 nm, at least 350 nm, at least 400 nm, or at least 450 nm. In addition, the length L1 may be at most 15 nm, at most 20 nm, at most 25 nm, at most 30 nm, at most 35 nm, at most 40 nm, at most 45 nm, at most 50 nm, at most 60 nm, at most 70 nm, at most 80 nm, at most 90 nm, at most 100 nm, at most 120 nm, at most 140 nm, at most 160 nm, at most 180 nm, at most 200 nm, at most 250 nm, at most 300 nm, at most 350 nm, at most 400 nm, at most 450 nm or at most 500 nm.

[0143] In an exemplary embodiment, the high-k isolation region 180 independently has a width W1 of 10 nm to 500 nm in the Y direction. For example, the width W1 may be at least 10 nm, at least 15 nm, at least 20 nm, at least 25 nm, at least 30 nm, at least 35 nm, at least 40 nm, at least 45 nm, at least 50 nm, at least 60 nm, at least 70 nm, at least 80 nm, at least 90 nm, at least 100 nm, at least 120 nm, at least 140 nm, at least 160 nm, at least 180 nm, at least 200 nm, at least 250 nm, at least 300 nm, at least 350 nm, at least 400 nm, or at least 450 nm. In addition, the width W1 may be at most 15nm, at most 20nm, at most 25nm, at most 30nm, at most 35nm, at most 40nm, at most 45nm, at most 50nm, at most 60nm, at most 70nm, at most 80nm, at most 90nm, at most 100nm, at most 120nm, at most 140nm, at most 160nm, at most 180nm, at most 200nm, at most 250nm, at most 300nm, at most 350nm, at most 400nm, at most 450nm or at most 500nm.

[0144] In an exemplary embodiment, the high-k isolation regions 180 are spaced a distance D1 of 5 nm to 100 nm from each other in the Y direction. For example, the distance D1 may be at least 5 nm, at least 10 nm, at least 15 nm, at least 20 nm, at least 25 nm, at least 30 nm, at least 35 nm, at least 40 nm, at least 45 nm, at least 50 nm, at least 60 nm, at least 70 nm, at least 80 nm, or at least 90 nm. In addition, the distance D1 may be at most 10 nm, at most 15 nm, at most 20 nm, at most 25 nm, at most 30 nm, at most 35 nm, at most 40 nm, at most 45 nm, at most 50 nm, at most 60 nm, at most 70 nm, at most 80 nm, at most 90 nm, or at most 100 nm.

[0145] It should be appreciated that the dielectric material 150 underlying the high-k isolation region 180 may be formed with a non-planar or angled surface 152, as depicted. Such a surface 152 may result from an etching process used to recess the dielectric material 150 during operation O18. As depicted, the high-k isolation region 180 may be formed with a mutually non-planar or angled bottom surface 182. Specifically, the bottom surface 182 may have a central planar portion 1821 and an angled portion 1822 interconnecting the central planar portion 1821 to respective sidewalls 186 of the high-k isolation region 180.

[0146] As shown, the central plane portion 1821 of the bottom surface 182 has a lateral width W2 in the Y direction. In an exemplary embodiment, the lateral width W2 is from 1 nanometer (nm) to 400 nanometers (nm). For example, the width W2 can be at least 1 nm, at least 5 nm, at least 10 nm, at least 15 nm, at least 20 nm, at least 25 nm, at least 30 nm, at least 35 nm, at least 40 nm, at least 45 nm, at least 50 nm, at least 60 nm, at least 70 nm, at least 80 nm, at least 90 nm, at least 100 nm, at least 120 nm, at least 140 nm, at least 160 nm, at least 180 nm, at least 200 nm, at least 250 nm, at least 300 nm, or at least 350 nm. In addition, width W2 may be at most 5nm, at most 10nm, at most 15nm, at most 20nm, at most 25nm, at most 30nm, at most 35nm, at most 40nm, at most 45nm, at most 50nm, at most 60nm, at most 70nm, at most 80nm, at most 90nm, at most 100nm, at most 120nm, at most 140nm, at most 160nm, at most 180nm, at most 200nm, at most 250nm, at most 300nm, at most 350nm or at most 400nm.

[0147] As shown, the angled portion 1822 of the bottom surface 182 forms an interior angle A1 with the sidewall 186. In an exemplary embodiment, the angle A1 is from 60 degrees to 180 degrees. For example, the angle A1 can be at least 60 degrees, at least 65 degrees, at least 70 degrees, at least 75 degrees, at least 80 degrees, at least 85 degrees, at least 90 degrees, at least 95 degrees, at least 100 degrees, at least 105 degrees, at least 110 degrees, at least 115 degrees, at least 120 degrees, at least 125 degrees, at least 130 degrees, at least 135 degrees, at least 140 degrees, at least 145 degrees, at least 150 degrees, at least 155 degrees, at least 160 degrees, at least 165 degrees, at least 170 degrees, or at least 175 degrees. In addition, angle A1 may be at most 65 degrees, at most 70 degrees, at most 75 degrees, at most 80 degrees, at most 85 degrees, at most 90 degrees, at most 95 degrees, at most 100 degrees, at most 105 degrees, at most 110 degrees, at most 115 degrees, at most 120 degrees, at most 125 degrees, at most 130 degrees, at most 135 degrees, at most 140 degrees, at most 145 degrees, at most 150 degrees, at most 155 degrees, at most 160 degrees, at most 165 degrees, at most 170 degrees, at most 175 degrees or at most 180 degrees.

[0148] In an exemplary embodiment, a top surface 181 of high-k isolation region 180 is planar and horizontal, i.e., in an XY plane with a constant Z value. Top surface 181 forms an interior angle A2 with each respective sidewall 186. In an exemplary embodiment, top surface 181 is horizontal, sidewalls 186 are vertical, and angle A2 is 90 degrees. In other exemplary embodiments, angle A2 is from 60 degrees to 120 degrees. For example, angle A1 may be at least 60 degrees, at least 65 degrees, at least 70 degrees, at least 75 degrees, at least 80 degrees, at least 85 degrees, at least 90 degrees, at least 95 degrees, at least 100 degrees, at least 105 degrees, at least 110 degrees, or at least 115 degrees. In addition, angle A1 may be at most 65 degrees, at most 70 degrees, at most 75 degrees, at most 80 degrees, at most 85 degrees, at most 90 degrees, at most 95 degrees, at most 100 degrees, at most 105 degrees, at most 110 degrees, at most 115 degrees, or at most 120 degrees.

[0149] like Fig.15 As shown in FIG. 1 , the high-k isolation region 180 is a multilayer structure formed of multiple layers such as layer 1601 and layer 1602. As shown in the figure, an interface 1603 is formed between layer 1601 and layer 1602. Fig.15 In the embodiment, the high-k isolation region 180 includes three layers; however, it is contemplated that the high-k isolation region 180 includes one to twenty layers. Each layer may have a thickness T1 of 3 nanometers (nm) to 20 nanometers (nm). For example, each layer may independently have a thickness T1 of at least 3 nm, at least 4 nm, at least 5 nm, at least 6 nm, at least 7 nm, at least 8 nm, at least 9 nm, at least 10 nm, at least 11 nm, at least 12 nm, at least 13 nm, at least 14 nm, at least 15 nm, at least 16 nm, at least 17 nm, at least 18 nm, or at least 19 nm. In addition, each layer may independently have a thickness T1 of at most 4 nm, at most 5 nm, at most 6 nm, at most 7 nm, at most 8 nm, at most 9 nm, at most 10 nm, at most 11 nm, at most 12 nm, at most 13 nm, at most 14 nm, at most 15 nm, at most 16 nm, at most 17 nm, at most 18 nm, at most 19 nm or at most 20 nm.

[0150] In an exemplary embodiment, layer 1601 and layer 1602 are formed of the same material, such as high-k material 160, for example, hafnium oxide. In other exemplary embodiments, layer 1601 and layer 1602 are formed of different materials. For example, one layer may be formed of high-k material 160, and the other layer may be an intervening layer formed of another type of material, such as a material used to improve the crystal uniformity of the material of the other layer.

[0151] Figures 16 to 18Three schematic diagrams of an exemplary high-k isolation region 180 are provided as a multi-layer structure formed of multiple layers and located above the dielectric material 150. Fig.16 In FIG. 1 , two layers 1601 are formed of a high-k material, such as hafnium oxide. In addition, two layers 1602 are formed of a uniformity improving material. The exemplary uniformity improving material in layer 1602 reduces the crystal non-uniformity in layer 1601. For example, layer 1602 may be formed of silicon dioxide (SiO2). Fig.16 In an exemplary embodiment of , layers 1601 may each have a thickness of 14 nanometers (nm), and layers 1602 may each have a thickness of 6 nanometers (nm). Thus, high-k isolation regions 180 have a thickness of 40 nanometers (nm).

[0152] exist Fig.17 In FIG. 1 , four layers 1601 are formed of a high-k material, such as hafnium oxide. In addition, two layers 1602 are formed of a uniformity improving material. The exemplary uniformity improving material in layer 1602 reduces the crystal non-uniformity in layer 1601. For example, layer 1602 may be formed of silicon dioxide (SiO2). Fig.17 In an exemplary embodiment of , layers 1601 may each have a thickness of 9 nanometers (nm), and layers 1602 may each have a thickness of 4 nanometers (nm). Thus, high-k isolation regions 180 have a thickness of 44 nanometers (nm).

[0153] exist Fig.18 In FIG. 1 , three layers 1601 are formed of a high-k material, such as hafnium oxide. In addition, two layers 1602 are formed of a uniformity improving material. The exemplary uniformity improving material in layer 1602 reduces the crystal non-uniformity in layer 1601. For example, layer 1602 may be formed of silicon dioxide (SiO2). Fig.17 In an exemplary embodiment of , layers 1601 may each have a thickness of 12 nanometers (nm), and layers 1602 may each have a thickness of 4 nanometers (nm). Thus, high-k isolation regions 180 have a thickness of 44 nanometers (nm).

[0154] Although Figures 16 to 18 A multilayer structure is provided for high-k isolation region 180, but other suitable structures are contemplated and may be selected to provide desired isolation and processing properties. Note that the high-k material layer may be formed only as an interior layer, such as Fig.17 and Fig.18 in general; or formed as an internal layer, such as Fig.16 Average.

[0155] Cross-reference Figures 15 to 18 , it can be seen that the top surface 181 of the high-k isolation region 180 can be formed by the layer 1601 and the layer 1602, so that the top surface 181 can be formed by the hafnium oxide layer and the silicon oxide layer.

[0156] In an exemplary embodiment, the insertion layer 1602 improves the quality of the high-k material layer 1601 and the multi-layer isolation region 180. Specifically, the device 200 formed with the multi-layer isolation region 180 may have reduced intra-grain "WiD" variation, that is, increased WiD uniformity, compared to the device 200 formed with a single material isolation region.

[0157] Although Figures 11 to 13 A semi-square high-k isolation region 180 is shown having a planar bottom surface 182, and Figure 14 to Figure 15 A semi-octagonal high-k isolation region 180 is shown having a bottom surface 182 formed with a central planar portion 1821 and an angled portion 1822 , although other high-k isolation regions 180 are contemplated.

[0158] For example, Fig.19 An illustration of a semi-circular high-k isolation region 180 having a semi-circular bottom surface 182 is provided. In addition, Fig. 20 An illustration of a semi-hexagonal high-k isolation region 180 having a bottom surface 182 formed by angled portions 1822 intersecting at an interface 1823 is provided. Fig.21 An illustration is provided of a semi-hexagonal high k isolation region 180 having a bottom surface 182 formed by inverted angled portions 1824 that intersect at an interface 1825. Although these shapes are illustrated and described, the high k isolation region 180 may be formed with a bottom surface 182 having another shape.

[0159] In addition, the high-k isolation region 180 may be formed in a desired layout shape. Figure 22 to Figure 25 Provide a portion of a manufacturing apparatus 200 such as in Fig.12 A simplified top view of the layout of the manufacturing stage. Fig. 22 , the unit cell 205 of the device 200 is formed with the following two: a high-k isolation region 180 extending completely across the unit cell 205 in the X direction; and a fin structure F10 extending completely across the unit cell 205 in the X direction. The high-k isolation regions 180 have equal widths in the Y direction and are equally spaced from each other in the Y direction.

[0160] exist Fig.23 , the unit cell 205 of the device 200 is formed with the following two: a high-k isolation region 180 extending completely across the unit cell 205 in the X direction; and a fin structure F10 extending completely across the unit cell 205 in the X direction. The high-k isolation regions 180 have different widths in the Y direction and are equally spaced from each other in the Y direction.

[0161] exist Fig.24, the device 200 includes a high-k isolation region 180 having a rectangular footprint. The exemplary high-k isolation region 180 has equal length in the X direction and equal width in the Y direction. In addition, the high-k isolation regions 180 are equally spaced from each other in the X direction and equally spaced from each other in the Y direction. Fig.24 The layout can be described as a grid.

[0162] exist Fig.25 , the device 200 includes a high-k isolation region 180 having a rectangular footprint, thereby forming a continuous layer interrupted by a fin structure F10. The exemplary fin structures F10 have equal lengths in the X direction and equal widths in the Y direction; and are equally spaced from each other in the X direction and equally spaced from each other in the Y direction.

[0163] View now Fig.26 , another embodiment of the semiconductor device 200 is shown. Fig.26 In the embodiment, the fin structure F10 is a hybrid fin structure formed of a hybrid fin material, such as SiCN. In an exemplary embodiment, the hybrid fin structure F10 contacts the gate G10 at an interface 240 coplanar with the top surface 181 of the high-k isolation region 180 . Fig.26 The method for manufacturing device 200 is similar to method M10, but is directed to forming a hybrid fin structure F10 instead of a nanosheet fin structure, and producing Fig.12 Thus, the gate G10 is formed above the hybrid fin F10 at a height equal to the height of the high-k isolation region 180 .

[0164] Therefore, one of the embodiments of the present disclosure describes a method, which includes: forming a plurality of fin structures separated by an isolation material; depositing a high-k material over the plurality of fin structures and the isolation material, wherein the high-k material includes a plurality of lower portions located between the plurality of fin structures and an upper portion located above the plurality of fin structures; depositing a topography-modified cap layer over the high-k material; and performing a chemical mechanical planarization (CMP) process to remove the cap layer and the upper portion of the high-k material and define a plurality of high-k insulating segments.

[0165] In certain embodiments of the method, the high-k material is hafnium oxide.

[0166] In some embodiments of the method, the step of depositing the high-k material includes the step of forming a multi-layer structure including a plurality of hafnium oxide layers and an intervening uniformity improving layer.

[0167] In certain embodiments of the method, the high-k material is hafnium oxide and the cap layer is silicon oxide.

[0168] In certain embodiments of the method, the CMP process includes: a first stage that is selective to etching the cap layer and lands on the high-k material; a second stage that is selective to etching the high-k material and lands on the multiple fin structures; and a third stage that is non-selective.

[0169] In certain embodiments of the method, the CMP process provides a controlled pH value to increase a removal rate of the high-k material while suppressing a removal rate of the plurality of fin structures.

[0170] In certain embodiments of the method, the CMP process uses a slurry formulation comprising silicon oxide abrasive and HNO 3 , and a pH value of the slurry formulation is from about 1 to about 5.

[0171] In some embodiments, the method further includes: removing a top layer from each fin structure so that each fin structure has an uppermost surface, which is located at a height below an upper surface of the multiple high-k insulating segments; and forming a metal gate above each fin structure and between the multiple high-k insulating segments.

[0172] In another embodiment, a method includes: forming a fin structure; forming a high-k isolation region laterally adjacent to the fin structure, wherein the high-k isolation region has an upper surface; and removing a top layer of the fin structure to form the fin structure having an uppermost surface located at a height below the upper surface of the high-k isolation region.

[0173] In certain embodiments of the method, the fin structure comprises multiple alternating layers of a first fin material and a second fin material, and wherein the method further comprises the following steps: forming a sacrificial gate above the uppermost surface of the fin structure; depositing a dielectric material around the sacrificial gate; removing the sacrificial gate; removing multiple layers of a fin material selected from the first fin material and the second fin material, wherein multiple layers of a non-selected fin material remain; and forming a metal gate around the multiple layers of the non-selected fin material and above the multiple layers.

[0174] In some embodiments of the method, the high-k isolation region includes hafnium oxide.

[0175] In some embodiments of the method, the step of forming the high-k isolation region includes the step of forming a multi-layer structure, the multi-layer structure including a plurality of hafnium oxide layers and an intervening uniformity improving layer.

[0176] In some embodiments of the method, the step of forming the high-k isolation region includes the step of forming a multi-layer structure, the multi-layer structure including a plurality of hafnium oxide layers and an intercalated silicon oxide layer.

[0177] In certain embodiments of the method, the step of forming the high-k isolation region includes: depositing hafnium oxide above and around the fin structure; forming a cap layer above the hafnium oxide; and performing a chemical mechanical planarization (CMP) process to remove the cap layer and an upper portion of the hafnium oxide and form the high-k isolation region and the top layer of the fin structure having a planar upper surface.

[0178] In another embodiment, a semiconductor device is provided and includes: a semiconductor fin structure; a gate structure located above the semiconductor fin structure; and a hafnium oxide isolation region laterally adjacent to the semiconductor fin structure.

[0179] In certain embodiments of the device, the semiconductor fin structure comprises a plurality of separated nanosheets of semiconductor material, the plurality of nanosheets including an upper nanosheet defining an uppermost surface of the semiconductor fin structure; the gate structure is positioned between and above the plurality of nanosheets; and the hafnium oxide isolation region has a top surface at a height above the uppermost surface of the semiconductor fin structure.

[0180] In certain embodiments of the device, the semiconductor fin structure is a hybrid fin structure comprising SiCN and having an uppermost surface; and the hafnium oxide isolation region has a top surface that is substantially coplanar with the uppermost surface of the semiconductor fin structure.

[0181] In certain embodiments of the device, the hafnium oxide isolation region includes alternating layers of hafnium oxide and a uniformity improving material.

[0182] In certain embodiments of the device, the hafnium oxide isolation region includes alternating layers of hafnium oxide and silicon oxide.

[0183] In certain embodiments of the device, the hafnium oxide isolation region comprises alternating layers of hafnium oxide and silicon oxide; the hafnium oxide isolation region has a top surface; and the top surface is formed by at least two hafnium oxide layers and at least one silicon oxide layer.

[0184] The foregoing summarizes the features of several embodiments so that those skilled in the art can better understand the aspects of the present disclosure. Those skilled in the art will appreciate that they can readily use the present disclosure as a basis for designing or modifying other processes and structures for implementing the same purposes and / or achieving the same advantages of the embodiments introduced herein. Those skilled in the art will also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and such equivalent constructions may be variously modified, substituted, and replaced herein without departing from the spirit and scope of the present disclosure.

Claims

1. A method for manufacturing a semiconductor device, characterized in that: The following steps are involved: forming a plurality of fin structures separated by an isolation material; Depositing a high-k material over the plurality of fin structures and the isolation material, wherein the high-k material includes a plurality of lower portions located between the plurality of fin structures and an upper portion located over the plurality of fin structures; depositing a cap layer over the high-k material; and A chemical mechanical planarization process is performed to remove the cap layer and the upper portion of the high-k material and define a plurality of high-k insulating sections.

2. The method according to claim 1, characterized in that The step of depositing the high-k material includes the following steps: forming a multi-layer structure, wherein the multi-layer structure includes a plurality of hafnium oxide layers and a plurality of inserted uniformity improvement layers.

3. The method according to claim 1, characterized in that The chemical mechanical planarization process includes: a first stage that is selective to etching the cap layer and lands on the high-k material; a second stage that is selective to etching the high-k material and lands on the plurality of fin structures; and Non-selective-third stage.

4. The method according to claim 1, characterized in that Further comprising the following steps: removing a top layer from each fin structure so that each fin structure is formed with an uppermost surface located at a height below an upper surface of the plurality of high-k insulating segments; and A metal gate is formed above each fin structure and between the plurality of high-k insulating sections.

5. A method for manufacturing a semiconductor device, characterized in that: The following steps are involved: forming a fin structure; forming a high-k isolation region laterally adjacent to the fin structure, wherein the high-k isolation region has an upper surface; and A top layer of the fin structure is removed to form the fin structure having an uppermost surface at a height below the upper surface of the high-k isolation region.

6. The method according to claim 5, characterized in that A fin structure includes a plurality of alternating layers of a first fin material and a second fin material, and the method further includes the following steps: forming a sacrificial gate over the uppermost surface of the fin structure; depositing a dielectric material around the sacrificial gate; removing the sacrificial gate; removing multiple layers of a fin material selected from the first fin material and the second fin material, wherein multiple layers of a non-selected fin material remain; and A metal gate is formed around and over the multiple layers of non-selected fin material.

7. A semiconductor device, characterized in that: Include: a semiconductor fin structure; a gate structure located above the semiconductor fin structure; and A hafnium oxide isolation region is laterally adjacent to the semiconductor fin structure.

8. The semiconductor device according to claim 7, wherein: in: The semiconductor fin structure comprises a plurality of separated nanosheets of semiconductor material, the plurality of nanosheets including an upper nanosheet defining an uppermost surface of the semiconductor fin structure; The gate structure is positioned between and above the plurality of nanosheets; and The hafnium oxide isolation region has a top surface at a height above the uppermost surface of the semiconductor fin structure.

9. The semiconductor device according to claim 7, wherein: in: The semiconductor fin structure is a hybrid fin structure, the hybrid fin structure includes SiCN and has an uppermost surface; and The hafnium oxide isolation region has a top surface that is substantially coplanar with the uppermost surface of the semiconductor fin structure.

10. The semiconductor device according to claim 7, wherein: in: The hafnium oxide isolation region comprises a plurality of alternating layers of hafnium oxide and silicon oxide; The hafnium oxide isolation region has a top surface; and The top surface is formed of at least two hafnium oxide layers and at least one silicon oxide layer.