Composite solid electrolyte battery for irradiation in-situ polymerization under magnetic field and preparation method of composite solid electrolyte battery
Through the method of irradiation in-situ polymerization under a magnetic field, the problem of the safety of the liquid electrolyte of lithium secondary batteries and the insufficient ion conductivity of the all-solid electrolyte is solved, the high ion conductivity and cycle stability of the battery are achieved, and the production process is simplified. , suitable for industrial production.
Patent Information
- Application Number
- CN202310394916.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-18
AI Technical Summary
The liquid electrolyte of existing lithium secondary batteries has problems such as easy leakage and chemical side reactions, and the all-solid electrolyte has insufficient ion conductivity, which limits its application at room temperature.
The composite solid-state electrolyte battery is prepared by in-situ polymerization of irradiation under a magnetic field. By mixing magnetic inorganic nanoparticles with electrolyte salts, ultrasonic treatment and magnetizing irradiation, the electrolyte precursor material is film-formed in situ in the battery semi-finished product to form an orderly of ion conduction channels.
It achieves good contact performance between the all-solid electrolyte and the pole piece, improves the ion conductivity, simplifies the production process, ensures the consistency of industrial production and high ion conductivity, and extends the cycle stability of the battery.
Smart Images

Figure BDA0004177332410000071 
Figure BDA0004177332410000091 
Figure BDA0004177332410000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of all-solid-state electrolyte batteries, and in particular relates to a composite solid-state electrolyte battery irradiated in-situ polymerized under a magnetic field and a preparation method thereof. Background Art
[0002] Lithium secondary batteries have the advantages of high energy density, good cycle performance, and high output voltage, and are receiving great attention in the field of energy storage. In the currently commonly used liquid electrolyte lithium secondary batteries, the liquid electrolyte is mainly a lithium salt such as LiPF6 and LiN (SO2C2F5) 2 dissolved in a polar aprotic organic solvent (such as a mixture of carbonates: ethylene carbonate and dimethyl carbonate, etc.). Due to its shortcomings such as easy leakage and chemical side reactions with electrodes during battery use, the safety and service life of liquid electrolyte batteries are severely restricted, and these polar organic solvents limit the operating temperature range of the battery to below 55°C.
[0003] In order to avoid the above problems, the solidification of lithium secondary batteries is the development trend of lithium batteries. Polymer lithium-ion batteries use polymer electrolytes to replace liquid electrolytes to achieve the solidification of lithium-ion batteries. Polymer electrolytes are divided into all-solid polymer electrolytes and gel polymer electrolytes. Among them, gel polymer electrolytes have been widely used in industry and have the advantages of low density, easy processing, and flexible manufacturing appearance. However, since gel polymer electrolytes belong to semi-solid batteries, they are still different from polymer electrolytes in all-solid batteries in terms of applicability and requirements. For example, the gel polymer electrolyte has a large viscosity after film formation, which will affect the film formation of the electrolyte; some groups of the gel polymer itself are easy to attract lithium ions, but the ion conductivity itself is not good, and it is unstable to metal Li; the homopolymer structure leads to high intramolecular crystallinity, which is not conducive to ion conductivity. Therefore, most gel polymers need to be modified to be effectively used in all-solid electrolyte batteries.
[0004] In addition, the current hot trend of all-solid-state polymer electrolytes is to realize the industrial production process of in-situ polymer batteries, that is, to allow the polymer electrolyte precursor material to form a film in situ in the battery semi-finished product that has been assembled with necessary components such as positive and negative electrodes through a certain method, which will have great application value in industry. However, considering the weak ion conductivity of organic solid electrolytes, the battery cannot meet the application requirements at room temperature. Therefore, so far, there is no suitable industrial production process for the preparation of in-situ batteries with high ionic conductivity that can meet the use at room temperature. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method to solve the problems in the above-mentioned background technology.
[0006] One of the technical solutions adopted by the present invention to solve the technical problem is: a method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field is provided, comprising the following steps:
[0007] (1) Preparing a precursor liquid electrolyte: mixing electrolyte monomers, stirring at a speed of 400-600 r / min for 0.5-1 hour to obtain a precursor electrolyte solvent, and adding an electrolyte salt to the solvent to obtain a precursor liquid electrolyte;
[0008] (2) preparing an organic-inorganic precursor: adding the magnetic inorganic nanoparticles to the electrolyte obtained in step (1), and ultrasonically treating for 5-24 hours to obtain an organic-inorganic precursor;
[0009] (3) Assembly of semi-finished batteries: Assemble the positive and negative electrodes, separators, electrolytes, and tabs of the battery until the final sealing step;
[0010] (4) Magnetization irradiation: The semi-finished battery treated in step (3) is subjected to magnetization irradiation, the magnetic field strength is 0.1T-5T, and the irradiation dose is 5-100KGy;
[0011] (5) Battery packaging: packaging the batteries processed in step (4).
[0012] In a preferred embodiment of the present invention, the magnetization irradiation in step (4) adopts pre-irradiation and full irradiation: ① Pre-irradiation: the semi-finished battery is pre-irradiated at a magnetic field strength of 0.1T-5T, and the irradiation dose is 2.5-50KGy;
[0013] ② Exhaust: Exhaust the semi-finished battery after pre-irradiation treatment, and the pressure in the cavity is -0.1 to -0.2MPa;
[0014] ③ Full irradiation: The semi-finished batteries after degassing are pre-irradiated under a magnetic field strength of 0.1T-5T, and the irradiation dose is 2.5-50KGy.
[0015] In a preferred embodiment of the present invention, the electrolyte monomer includes one or more of polyethylene oxide, polypropylene carbonate, polyethylene carbonate, polybutylene carbonate, polypropylene carbonate-polycyclohexene carbonate copolymer, and polycyclohexene carbonate.
[0016] In a preferred embodiment of the present invention, in step (1), the mass fraction of the electrolyte salt in the precursor liquid electrolyte is 5-15%.
[0017] In a preferred embodiment of the present invention, the magnetic inorganic nanoparticles include Ti2O3, TiO2, ZrO2, VO, V2O3, VO2, V2O5, NbO, NbO2, Nb2O5, CrO, Cr2O3, CrO2, MoO2, MoO3, CoO, Co3O4, Co2O3, NiO, Ni2O3, Cu2O, CuO, Cu2O3, ZnO, Mn2O3, and Fe3O4.
[0018] In a preferred embodiment of the present invention, in step (2), the mass fraction of the magnetic inorganic nanoparticles in the organic-inorganic precursor is 1-20%, and the particle size of the magnetic inorganic nanoparticles is preferably 100nm-200nm.
[0019] In a preferred embodiment of the present invention, in step (4), the magnetic field source is generated by one or more of an electromagnetic coil, a rubidium magnet, and a rubidium alloy magnet.
[0020] In a preferred embodiment of the present invention, the pre-irradiation and irradiation are performed by an aerobic co-irradiation method or an anaerobic co-irradiation method.
[0021] The second technical solution adopted by the present invention to solve its technical problem is: providing a composite solid electrolyte battery that is irradiated in-situ polymerized under a magnetic field, which is prepared by the above method.
[0022] In a preferred embodiment of the present invention, it is an all-solid-state lithium, sodium, or potassium ion secondary battery.
[0023] In a preferred embodiment of the present invention, magnetic inorganic nanoparticles are arranged in a directional manner in the composite solid electrolyte.
[0024] Compared with the background technology, this technical solution has the following advantages:
[0025] 1. The present invention forms a film of the polymer electrolyte precursor material in situ in the battery under a magnetic field, which can obtain good contact performance with the positive and negative electrodes of the battery, eliminate interface impedance, and solve the interface problem between the all-solid electrolyte and the pole piece;
[0026] 2. The present invention utilizes the selected magnetic field to arrange the magnetic inorganic nano-ions in the semi-finished battery in an orderly manner to form an ion conduction channel, thereby solving the problem of weak ion conduction ability of traditional organic solid electrolytes;
[0027] 3. The present invention combines the process steps of polymer electrolyte membrane production and assembly with other battery components in the preparation of in-situ batteries. By utilizing the high penetrability of ionizing radiation, it can penetrate other battery components and directly act on the electrolyte precursor material to solidify it in situ, so that the inorganic nanoparticles in the semi-finished battery are arranged in a directionally and controllably, greatly simplifying the production process and saving time and other costs.
[0028] 4. The present invention can use the magnetization irradiation method to perform assembly line magnetization and irradiation treatment on battery semi-finished products through the reasonable arrangement of radiation sources, radiation action space, transmission devices, etc. Each battery semi-finished product receives exactly the same magnetic field strength and similar irradiation dose, and its production consistency is controllable; through the magnetization ionization radiation in-situ battery production process, high ion conductivity can be achieved, and no heating is required during the production process, and no impurities such as initiators, cross-linking agents, and catalysts are added, so that the electrolyte precursor material is solidified in situ, thereby ensuring the consistency of industrial production and realizing rapid large-scale production. DETAILED DESCRIPTION
[0029] The present invention selects high-energy ionizing radiation such as gamma rays or electron beams to irradiate the semi-finished battery. The semi-finished battery is irradiated with a certain radiation dose at a certain dose rate for a certain time under a certain magnetic field strength, so that the magnetic inorganic nanoparticles therein are arranged in order, and then the electrolyte precursor material is in-situ cured through chemical processes such as cross-linking, polymerization, and grafting while maintaining the orderly arrangement of the magnetic inorganic nanoparticles, so as to prepare an in-situ battery.
[0030] The battery production process provided by the present invention includes the following elements: 1. A battery semi-finished product that is infused with electrolyte precursor materials and magnetic inorganic nanoparticles and contains other components necessary for realizing this process. 2. A magnetic field with controllable magnetic field strength, a radiation source of controllable ionizing radiation and its supporting radiation shielding facilities and ionizing radiation action space. 3. A conveying device that can continuously or intermittently deliver the battery semi-finished product into the ionizing radiation action space. 4. Other safety supporting facilities to ensure production safety, especially to ensure that the magnetic field and ionizing radiation are controllable and not leaked.
[0031] The specific necessary components of the semi-finished battery include:
[0032] 1. One or more inorganic solid electrolyte materials or other magnetic inorganic materials.
[0033] 2. The electrolyte precursor materials include, but are not limited to, various reaction precursor materials that can be cross-linked, polymerized, or grafted by irradiation, and one or more of solvents and lithium salts.
[0034] 3. Various positive electrode materials and negative electrode materials.
[0035] 4. A separator element that can be used to separate the positive electrode and the negative electrode to prevent short circuit, such as a porous electronic insulating film, a support structure for fixing and separating the positive and negative electrode materials, etc.
[0036] 5. Battery semi-finished product shell
[0037] It should be noted that the aforementioned necessary elements are only examples of some easy-to-think necessary elements, and do not mean that the battery semi-finished product only contains the aforementioned elements or includes all the aforementioned elements. The battery semi-finished product refers to an object to be irradiated that contains all the necessary elements required to realize a feasible and simple overall preparation process of the battery and can be subjected to in-situ curing by magnetic irradiation.
[0038] The controllable magnetic field source is an electromagnetic coil, a strong magnet, etc. that can provide a magnetic field with a stable magnetic field strength; the controllable radiation source is a radiation source that can stably provide ionizing radiation such as gamma rays, beta rays, and high-energy X-rays, such as decay elements, accelerators, etc. The magnetic field strength of the magnetic field source must be controllable, and at least one parameter of the radiation intensity, irradiation dose, and dose rate of the radiation source should be predictable or controllable.
[0039] The magnetized radiation shielding facilities and radiation action space are any appropriate facilities that can meet safety requirements and production needs and are magnetized radiation action spaces that are large enough to carry out assembly-line magnetized radiation in-situ curing to produce in-situ batteries. The specific implementation method is not specifically limited.
[0040] The conveying device is any conveying device that can intermittently or continuously deliver semi-finished battery products into the irradiation action space, including but not limited to conveyor belts, conveying pods, etc., as long as it can cooperate with the magnetic field source, the magnetic field shielding device, the magnetic field action space, the radiation source, the radiation shielding facilities, and the irradiation action space to achieve a stable and controllable magnetic field intensity for the product, a controllable radiation dose, and the ability to continuously or intermittently enter and exit the magnetized irradiation action space, and to keep the magnetic field and radiation from leaking during the entry and exit process.
[0041] The other safety facilities are all necessary safety facilities for eliminating potential safety hazards and preventing radiation leakage, which are not particularly limited herein. The present invention will be described in more detail below by way of examples. In the following description of specific embodiments, a large number of specific details are provided to facilitate a deeper understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details. The scope of protection of the present invention is not limited to these embodiments.
[0042] Example 1
[0043] A method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field, using an electromagnetic coil as a magnetic field source, Co-60 as a gamma-ray radiation source point source, using a continuous feeding conveyor belt, and setting an appropriate conveyor belt-magnetic radiation source distance and conveying speed in a magnetized irradiation chamber to control the magnetic induction intensity of the semi-finished battery to 0.5T, and the radiation dose to 25KGy per entry and exit of the radiation chamber. The specific steps are as follows:
[0044] (1) preparing a precursor liquid electrolyte: mixing a small molecule PEG with a molecular weight of 500 with a solvent dimethyl carbonate (DMC), stirring at a speed of 400-600 r / min for 0.5-1 hour to obtain a precursor electrolyte solvent, and adding a lithium salt of bistrifluorosulfonyl imide lithium (TFSILi) to the solvent to obtain a precursor liquid electrolyte;
[0045] (2) preparing an organic-inorganic precursor: adding magnetized silica nanoparticles with a particle size of 200 nm to the electrolyte obtained in step (1), and ultrasonically treating for 5-24 hours to obtain an organic-inorganic precursor;
[0046] (3) Assembly of semi-finished batteries: Assemble the positive and negative electrodes, separators, electrolytes, and tabs of the battery until the final step of sealing; in this embodiment, the nickel-cobalt-manganese ternary material NCM622 electrode is used as the positive electrode, the graphite electrode is used as the negative electrode, the porous cellulose membrane is used as the isolation device to isolate the positive electrode and the negative electrode to prevent short circuit, and the battery shell adopts 18650 cylindrical batteries to prepare a batch of semi-finished batteries;
[0047] (4) In-situ curing by irradiation under magnetic field: The batch of semi-finished batteries is placed on a continuous conveyor belt and run for two turns, so that the semi-finished batteries are sent to the magnetization irradiation room twice for pre-irradiation and full irradiation, and are irradiated with a magnetic field intensity of 0.5T and a total irradiation dose of 50KGy to form in-situ batteries. In this embodiment, pre-irradiation is used to control the degree of polymerization of the organic monomer, and the magnetized silica nanoparticles are driven to be oriented and orderly arranged under the guidance of the magnetic field; then full irradiation is performed to further deepen the order of the magnetized silica nanoparticles, further solidify the organic monomer, and effectively control the consistency of production.
[0048] Comparative Example 1
[0049] The main difference between Comparative Example 1 and Example 1 is that a different curing method is used, in which a thermal curing method without a magnetic field is adopted.
[0050] In-situ batteries were prepared by thermal curing, with NCM622 pole pieces as positive pole pieces, graphite pole pieces as negative pole pieces, cellulose porous membranes as isolation devices to prevent short circuits between positive and negative poles, small molecule PEG with a molecular weight of 600 as cross-linking precursors, ammonium persulfate as initiator, magnetized silica nanoparticles with a particle size of 200 nm as inorganic fillers, bistrifluorosulfonyl imide lithium (TFSILi) as lithium salt, and an appropriate amount of dimethyl carbonate (DMC) as solvent. A batch of semi-finished batteries were prepared by using 18650-shaped cylindrical batteries as battery shells. The batch of semi-finished batteries was placed in a conveying pod and conveyed to a heating device for thermally induced in-situ curing to form in-situ batteries.
[0051] Comparative Example 2
[0052] The main difference between Comparative Example 2 and Example 1 is that a different curing method is used, in which a radiation curing method without a magnetic field is adopted.
[0053] Co-60 is used as a point source of γ-ray radiation, a continuous feeding type conveyor belt is used, and in a magnetizing irradiation chamber, an appropriate conveyor belt-magnetizing radiation source distance and a conveying speed are set to control the radiation dose received by the semi-finished battery to be 25KGy per entry and exit of the radiation chamber, a nickel-cobalt-manganese ternary material NCM622 pole piece is used as a positive pole piece, a graphite pole piece is used as a negative pole piece, a porous cellulose membrane is used as an isolation device to isolate the positive and negative poles to prevent short circuits, a small molecule PEG with a molecular weight of 500 is used as a cross-linking precursor, a magnetized silica nanoparticle with a particle size of 200nm is used as an inorganic filler, bistrifluorosulfonyl imide lithium (TFSILi) is used as a lithium salt, an appropriate amount of dimethyl carbonate (DMC) is used as a solvent, and a battery shell uses a 18650-shaped cylindrical battery to prepare a batch of semi-finished batteries. The batch of semi-finished batteries are placed on a continuous conveyor belt and run for two turns, so that the semi-finished batteries are sent into the magnetizing irradiation chamber twice, and irradiated with a total radiation dose of 50KGy to make in-situ batteries.
[0054] Table 1 Capacity retention rate of in-situ batteries in Example 1 and Comparative Examples 1 and 2
[0055]
[0056] It can be seen that compared with Comparative Examples 1 and 2, the first cycle efficiency of Example 1 is significantly higher than that of Comparative Examples 1 and 2, and the capacity retention rate in the long cycle test is also very excellent, much higher than that of Comparative Examples 1 and 2. It shows that the battery prepared by the organic-inorganic composite solid electrolyte irradiated in situ under a magnetic field has good cycle stability and ion transport performance; radiation curing is better than the in-situ curing method of thermal curing, and radiation curing in a magnetic field is better than the in-situ curing method without magnetic field irradiation.
[0057] Example 2
[0058] The electromagnetic coil is used as the magnetic field source, Co-60 is used as the gamma ray radiation plane source, and an indirect feeding type transmission pod is used to make multiple pods stay at multiple fixed positions in the radiation room in turn for a certain fixed time, and then move to the next fixed position or leave the radiation room in turn. The time and position of the pod staying in the radiation room are controlled so that the magnetic induction intensity received by the semi-finished battery in each pod is 1T, and the radiation dose received is 70KGy once entering and leaving the radiation room. The lithium cobalt oxide material pole piece is used as the positive electrode, the lithium metal is used as the negative electrode, the PVDF porous membrane is used as the isolation device to isolate the positive electrode and the negative electrode to prevent short circuit, the PEO with a molecular weight of 60w is used as the cross-linking precursor, the magnetized silica nanoparticles with a particle size of 100nm are used as the inorganic filler, the 2-acrylamide-2-methylpropanesulfonic acid lithium (AMPSLi) monomer is used as the graft copolymer monomer of the lithium salt, an appropriate amount of acetonitrile is used as the solvent, and the battery shell is in the form of a button battery, and a batch of semi-finished battery products are prepared. The semi-finished batteries of this batch are placed in a conveying pod and sent to the irradiation room for irradiation once. The magnetic induction intensity received is 1T and the total irradiation dose is 70KGy to make in-situ batteries.
[0059] Comparative Example 3
[0060] The main difference between Comparative Example 3 and Example 2 is that a different photocuring method induced by ultraviolet rays under a magnetic field is adopted.
[0061] In-situ batteries were prepared by ultraviolet initiation, with lithium cobalt oxide pole pieces as positive electrodes, lithium metal as negative electrodes, PVDF porous membranes as isolation devices to prevent short circuits between positive and negative electrodes, PEO with a molecular weight of 60w as a cross-linking precursor, magnetized silica nanoparticles with a particle size of 100nm as inorganic fillers, 2-acrylamide-2-methylpropanesulfonic acid lithium (AMPSLi) monomers as graft copolymers of lithium salts, appropriate amounts of acetonitrile as solvents, ultraviolet light initiators, button batteries as battery shells, and a batch of semi-finished batteries were prepared under a magnetic field with a magnetic induction intensity of 1T. The batch of semi-finished batteries was placed in a transport pod and transported to a high-power ultraviolet lamp device for ultraviolet-induced in-situ curing to form in-situ batteries.
[0062] Table 2 Capacity retention rate of in-situ batteries in Example 2 and Comparative Example 3
[0063]
[0064] It can be seen that the solid-state battery in Example 2 has a better capacity retention rate than that in Comparative Example 3, which means that compared with ultraviolet light curing, the solid-state polymer battery obtained by radiation curing has better cycle stability.
[0065] Example 3
[0066] The difference between Example 3 and Example 1 is that: an electromagnetic coil is used as a magnetic field source, an electron accelerator is used as an electron beam radiation source, and an indirect feeding type transmission pod is used, so that each pod is sequentially placed at a fixed position in the direction of the electron beam generation in the radiation chamber for a certain period of time. The time the pod stays in the radiation chamber and the distance between the pod and the electron accelerator are controlled so that the magnetic induction intensity received by the semi-finished battery in each cabin is 0.5T, and the radiation dose received is 45KGy once entering and leaving the radiation chamber. A lithium iron phosphate material pole piece is used as a positive electrode, a silicon-carbon negative electrode material pole piece is used as a negative electrode, a polypropylene (PP) porous membrane is used as an isolation device to isolate the positive electrode and the negative electrode to prevent short circuit, a small molecule polyethylene glycol (PEG) with a molecular weight of 499w is a cross-linking precursor, an acrylonitrile (AN) monomer is a comonomer, a magnetized silica nanoparticle with a particle size of 200nm is an inorganic filler, lithium bis(fluorosulfonyl)imide (LiFSI) is a lithium salt, an appropriate amount of acetonitrile is used as a solvent, and a battery shell is formed in the form of an extremely thin soft-pack battery, and a batch of semi-finished batteries are prepared. The semi-finished batteries of this batch are placed in a conveyor pod and sent to the irradiation room for irradiation once. The magnetic induction intensity is 0.5T and the total irradiation dose is 45KGy to make in-situ batteries.
[0067] Comparative Example 4
[0068] The main difference between Comparative Example 4 and Example 3 is that the particle sizes of the inorganic nanoparticles used are different. The particle size of the inorganic nanoparticles used in Example 3 is 200 nm, and the particle size of the inorganic nanoparticles used in Comparative Example 4 is 400 nm.
[0069] The time the pod stays in the radiation chamber and the distance between the pod and the electron accelerator are controlled so that the magnetic induction intensity received by the semi-finished battery in each pod is 0.5T, and the radiation dose received is 45KGy for one entry and exit of the radiation chamber. The lithium iron phosphate material pole piece is used as the positive electrode, the silicon carbon negative electrode material pole piece is used as the negative electrode, the polypropylene (PP) porous membrane is used as the isolation device to isolate the positive electrode and the negative electrode to prevent short circuit, the small molecule polyethylene glycol (PEG) with a molecular weight of 499w is used as the cross-linking precursor, the acrylonitrile (AN) monomer is used as the comonomer, the magnetized silica nanoparticles with a particle size of 400nm are used as the inorganic filler, the lithium bis(fluorosulfonyl)imide (LiFSI) is used as the lithium salt, the appropriate amount of acetonitrile is used as the solvent, and the battery shell is formed of an extremely thin soft-pack battery to prepare a batch of semi-finished batteries. The batch of semi-finished batteries are placed in the conveying pod and sent to the irradiation chamber for irradiation once, and the magnetic induction intensity received is 0.5T, and the total radiation dose received is 45KGy, so as to make in-situ batteries.
[0070] Table 3 Capacity retention rate of in-situ batteries in Example 3 and Comparative Example 4
[0071]
[0072] It can be seen that the solid-state battery in Example 3 has a better capacity retention rate than that in Comparative Example 4, indicating that the solid-state polymer battery obtained after irradiation curing of inorganic nanoparticles with smaller particle sizes has better cycle stability.
[0073] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field, Features: The steps include: (1) Preparing a precursor liquid electrolyte: mixing electrolyte monomers, stirring at a speed of 400-600 r / min for 0.5-1 hour to obtain a precursor electrolyte solvent, and adding an electrolyte salt to the solvent to obtain a precursor liquid electrolyte; (2) preparing an organic-inorganic precursor: adding the magnetic inorganic nanoparticles to the electrolyte obtained in step (1), and ultrasonically treating for 5-24 hours to obtain an organic-inorganic precursor; (3) Assembly of semi-finished batteries: Assemble the positive and negative electrodes, separators, electrolytes, and tabs of the battery until the final sealing step; (4) Radiation curing: The semi-finished battery treated in step (3) is subjected to magnetization irradiation, the magnetic field strength is 0.1T-5T, and the irradiation dose is 5-100KGy; (5) Battery packaging: packaging the batteries processed in step (4).
2. The method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field according to claim 1, Features: Step (4) magnetization irradiation adopts pre-irradiation and full irradiation: ① Pre-irradiation: pre-irradiate the semi-finished battery under a magnetic field strength of 0.1T-5T, with an irradiation dose of 2.5-50KGy; ② Exhaust: Exhaust the semi-finished battery after pre-irradiation treatment, and the pressure in the cavity is -0.1 to -0.2MPa; ③ Full irradiation: The semi-finished batteries after degassing are pre-irradiated under a magnetic field strength of 0.1T-5T, and the irradiation dose is 2.5-50KGy.
3. The method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field according to claim 1, Features: The electrolyte monomers include one or more of ethylene oxide, propylene carbonate, ethylene carbonate, butylene carbonate, propylene carbonate, cyclohexene carbonate copolymer, and cyclohexene carbonate.
4. The method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field according to claim 1, Features: In step (1), the mass fraction of the electrolyte salt in the precursor liquid electrolyte is 5-15%.
5. The method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field according to claim 1, Features: The magnetic inorganic nanoparticles include Ti 2 O 3 、TiO 2 、ZrO 2 , VO, V 2 O 3 , VO 2 、V 2 O 5 、NbO、NbO 2 , Nb 2 O 5 ,CrO,Cr 2 O 3 CrO 2 、MoO 2 、MoO 3 , CoO, Co 3 O 4 、Co 2 O 3 、NiO、Ni 2 O 3 , Cu 2 O, CuO, Cu 2 O 3 , ZnO, Mn 2 O 3 , Fe 3 O 4 .
6. A composite solid electrolyte battery irradiated in situ under a magnetic field according to claim 5, Its characteristics are: The particle size of the magnetic inorganic nanoparticles is 100nm-200nm.
7. The method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field according to claim 1, Features: In step (2), the mass fraction of the magnetic inorganic nanoparticles in the organic-inorganic precursor is 1-20%.
8. The method for preparing a composite solid electrolyte battery by irradiation in-situ polymerization under a magnetic field according to claim 1, Features: In step (4), the magnetic field source is generated by one or more of an electromagnetic coil, a rubidium magnet, and a rubidium alloy magnet.
9. A composite solid electrolyte battery with in-situ polymerization by irradiation under a magnetic field, Features: The method is prepared according to any one of claims 1 to 8.
10. A composite solid electrolyte battery with in-situ polymerization by irradiation under a magnetic field according to claim 9, Features: Magnetic inorganic nanoparticles are arranged in a directional manner in the composite solid electrolyte.
Citation Information
Cited By
Polymer solid electrolyte and preparation method and application thereof
CN122436563A
Polymer solid electrolyte, preparation method and application thereof
CN122436563B