Diaphragm and preparation method thereof, battery and electric device
By using a double-layer structure of ceramics and flame retardants in the battery separator, the problems of low melting point and poor wettability of the separator material are solved, the ionic conductivity and high temperature resistance of the battery are improved, and the service life and safety of the battery are extended.
Patent Information
- Application Number
- CN202310383440.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
AI Technical Summary
Existing battery separator materials have low melting points, are prone to thermal runaway, and have poor wettability, which affects the ionic conductivity and service life of the battery.
It adopts a double-layer diaphragm structure, in which the coating between the first base film and the second base film contains ceramics and flame retardants. The ceramics are used to improve mechanical strength and heat resistance, and the flame retardants are used to improve ionic conductivity and high temperature resistance. performance.
The capacity retention rate and safety performance of the battery are significantly improved, the service life is extended, and the risk of powder removal and thermal runaway is reduced.
Smart Images

Figure CN118801037A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of battery materials, and specifically relates to a diaphragm and a preparation method thereof, a battery and an electrical device. Background Art
[0002] Battery separator film (BSF), also known as battery diaphragm, is one of the core materials in batteries. The diaphragm is located between the positive and negative electrodes of the battery. Its main function is to separate the positive and negative active materials of the battery to reduce the risk of short circuit caused by contact between the two electrodes. At the same time, it allows the current-carrying ions in the electrolyte to pass through to form a charge and discharge circuit, which has an important impact on battery safety and cost.
[0003] The commonly used diaphragm materials on the market have low melting points and are prone to thermal runaway, and their poor wettability can easily affect the ionic conductivity of the diaphragm, thereby affecting the performance and life of the battery. Summary of the invention
[0004] In view of the above problems, the present application provides a diaphragm and a preparation method thereof, a battery and an electrical device, aiming to solve the technical problem of how to improve the ionic conductivity and safety of use of the diaphragm.
[0005] In a first aspect, an embodiment of the present application provides a diaphragm, comprising a first base film, a second base film, and a coating located between the first base film and the second base film, wherein the coating contains ceramics and a flame retardant.
[0006] By applying ceramic and flame retardant materials to the coating between the first base film and the second base film, the composite effect of the first base film and the second base film can be used to improve the overall mechanical strength of the diaphragm, and the double-layer protection effect makes the ceramic and flame retardant not easy to fall off, thereby reducing the risk of powdering; based on the good wettability and heat resistance of the ceramic in the coating, it can not only improve the liquid absorption and liquid retention ability of the diaphragm, thereby improving the ionic conductivity, but also work together with the flame retardant to improve the high temperature resistance of the diaphragm. Therefore, the diaphragm provided in the embodiment of the present application can be used in a battery to significantly improve the capacity retention rate, safety performance and service life of the battery.
[0007] In some embodiments, the ceramic includes ceramic particles having an average particle size of 0.01 μm to 1 μm; and / or,
[0008] The flame retardant includes flame retardant particles with an average particle size of 0.02 μm to 2 μm.
[0009] Ceramic particles with an average particle size of 0.01 μm to 1 μm and flame retardant particles with an average particle size of 0.02 μm to 2 μm can be evenly dispersed in the coating to make the coating tightly and evenly coated, while also making the coating have good air permeability.
[0010] In some embodiments, the ceramic includes ceramic particles having an average particle size of 0.05 μm to 0.5 μm; and / or,
[0011] The flame retardant includes flame retardant particles with an average particle size of 0.05 μm to 1 μm.
[0012] The ceramic particles with an average particle size of 0.05 μm to 0.5 μm and the flame retardant particles with an average particle size of 0.05 μm to 1 μm have good comprehensive effects on the dispersibility and air permeability of the coating.
[0013] In some embodiments, the ceramic material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, yttrium oxide, cerium oxide, zirconium titanate, barium titanate and magnesium fluoride; and / or,
[0014] The flame retardant includes at least one of metaborate, orthoborate and polyborate.
[0015] On the one hand, the ceramic material can improve the heat resistance of the diaphragm; on the other hand, the borate flame retardant has a certain binding effect with the anions in the electrolyte, which can inhibit the migration of anions in the diaphragm; and the polar bonds in the flame retardant and the Lewis acid of the boron-containing anions can promote the desolvation of electrolyte ions. In this way, the combination of the ceramic material and the borate flame retardant in the coating can further significantly improve the ion migration rate and heat resistance safety performance of the diaphragm.
[0016] In some embodiments, the metaborate comprises at least one of calcium metaborate, barium metaborate, sodium metaborate, and ammonium metaborate; or
[0017] Orthoborates include zinc borate; or,
[0018] The polyborate includes at least one of ammonium pentaborate and sodium tetraborate.
[0019] The above-mentioned metaborates, orthoborates and polyborates can be selected and matched with ceramic materials to significantly improve the ion migration rate in the diaphragm.
[0020] In some embodiments, the mass ratio of the ceramic to the flame retardant is greater than or equal to 1.05.
[0021] Using ceramics and flame retardants in a coating between the first base film and the second base film in a mass ratio of ceramics to flame retardants greater than or equal to 1.05 can improve the overall wettability and heat resistance of the diaphragm.
[0022] In one embodiment, the mass ratio of ceramic to flame retardant is (1.05-9):1.
[0023] Using ceramics and flame retardants in a coating between the first base film and the second base film at a mass ratio of ceramics to flame retardants (1.05 to 9):1 can improve the overall wettability and heat resistance of the diaphragm.
[0024] In one embodiment, the base materials of the first base film and the second base film respectively and independently include at least one of a polyolefin-based material, a fluorine-containing polymer-based material, and a polyester-based material.
[0025] Using at least one of polyolefin materials, fluorine-containing polymer materials, and polyester materials as the main polymer material of the diaphragm substrate not only has good insulation properties, but also can form a microporous structure, so that the diaphragm can have the air permeability and porosity required by the industry, thereby providing a good migration channel for the ions of the electrolyte and allowing the battery to operate stably and efficiently.
[0026] In some embodiments, the porosity of the first base film is greater than the porosity of the second base film.
[0027] By utilizing the porosity difference between the first base membrane and the second base membrane, the ion migration rate can be improved while ensuring the mechanical strength of the diaphragm.
[0028] In some embodiments, the ratio of the porosity of the first base film to the porosity of the second base film is greater than or equal to 1.02; and / or,
[0029] The porosity of the first base film is 32% to 90%, and the porosity of the second base film is 30% to 85%.
[0030] The combination of the first base film with a porosity of 32% to 90% and the second base film with a porosity of 30% to 85% is not only beneficial to ion migration, but also makes the membrane as a whole have good air permeability and mechanical properties.
[0031] In some embodiments, the porosity of the first base film is 35% to 85%, and the porosity of the second base film is 34% to 45%.
[0032] The combination of the first base film with a porosity of 35% to 85% and the second base film with a porosity of 34% to 45% makes the overall mechanical properties, air permeability and ion mobility of the diaphragm good.
[0033] In some embodiments, a thickness of the first base film is greater than a thickness of the second base film.
[0034] By utilizing the thickness difference between the first base film and the second base film, the overall mechanical strength of the diaphragm can be well balanced, allowing it to be used for a long time in the battery.
[0035] In some embodiments, the ratio of the thickness of the first base film to the thickness of the second base film is (1.02-5.0):1; and / or,
[0036] The thickness of the first base film is 2 μm to 13 μm, and the thickness of the second base film is 1 μm to 12 μm.
[0037] The combination of the first base film with a thickness of 2μm to 13μm and the second base film with a thickness of 1μm to 12μm not only makes the diaphragm as a whole have good mechanical properties, but also has a good protective effect on the ceramics and flame retardants in the intermediate coating, making the ceramics and flame retardants not easy to fall off.
[0038] In some embodiments, the thickness of the first base film is 3 μm to 6 μm, and the thickness of the second base film is 2 μm to 5 μm.
[0039] The combination of the first base film with a thickness of 3μm to 6μm and the second base film with a thickness of 2μm to 5μm not only makes the overall mechanical properties of the diaphragm good, and the ceramic and flame retardant in the intermediate coating are not easy to fall off, but also can greatly improve the battery energy density in the battery.
[0040] In some embodiments, the coating has a thickness of 0.5 μm to 10 μm.
[0041] The coating thickness between the first base film and the second base film is 0.5 μm to 10 μm, which can improve the overall wettability and heat resistance of the diaphragm.
[0042] In some embodiments, the coating has a thickness of 1 μm to 5 μm.
[0043] The coating thickness between the first base film and the second base film is 1 μm to 5 μm, which can make the overall wettability and heat resistance of the diaphragm good, and at the same time make the diaphragm have good air permeability.
[0044] In some embodiments, the coating further comprises a binder.
[0045] By using a binder in the middle layer, the binder can bind and fix the ceramics and the flame retardant in the coating, so that the ceramics and the flame retardant are not easy to fall off.
[0046] In some embodiments, the binder comprises at least one of polyacrylate, acrylic acid and carboxymethyl cellulose; and / or,
[0047] The mass ratio of binder to ceramic is (0.01-0.3):1.
[0048] The above types of binders have very good adhesion. Under the above proportion conditions, they have good adhesion effect on the ceramics in the coating and have little effect on the coating thickness.
[0049] In a second aspect, an embodiment of the present application provides a method for preparing the above-mentioned diaphragm, comprising the following steps:
[0050] formulating a slurry containing ceramic and flame retardant;
[0051] The slurry is coated on the surface of the first base film to form a slurry coating layer, and then the second base film is covered on the slurry coating layer and subjected to a lamination process to obtain a diaphragm.
[0052] The diaphragm of the embodiment of the present application can be obtained by using a wet coating film-forming process, coating the slurry containing ceramics and flame retardants on the surface of the first base film to form a slurry coating, and then covering the second base film for lamination. Such a preparation method is not only simple in process and low in preparation cost, but also can obtain a diaphragm with good ionic conductivity and high temperature resistance.
[0053] In some embodiments, the step of preparing a slurry containing ceramics and a flame retardant includes: dissolving the ceramics and the flame retardant in water, and then adding a binder and stirring to obtain a slurry.
[0054] By adding a binder to the slurry, the slurry can have good viscosity, and at the same time, the ceramic and the flame retardant in the slurry can be better bonded to form a film between the first base film and the second base film.
[0055] In some embodiments, the binder comprises at least one of polyacrylate, acrylic acid and carboxymethyl cellulose; and / or,
[0056] The mass ratio of binder to ceramic is (0.01-0.3):1.
[0057] The above-mentioned adhesives have good viscosity, so that the ceramic and flame retardant in the middle of the final diaphragm are not easy to fall off. The above-mentioned proportion conditions have good adhesion effects and have little effect on the final coating thickness.
[0058] In some embodiments, the mass concentration of the ceramic in the slurry is 50% to 90%, and the mass concentration of the flame retardant is 10% to 50%.
[0059] In the slurry with the above mass concentration, the ceramic and the flame retardant are evenly dispersed, and the prepared slurry has good viscosity and is easy to coat and form a film.
[0060] In a third aspect, an embodiment of the present application provides a battery, comprising a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator provided in the first aspect of the embodiment of the present application and / or the separator prepared by the preparation method provided in the second aspect of the embodiment of the present application.
[0061] By using the diaphragm provided in the first aspect of the embodiment of the present application and / or the diaphragm prepared by the preparation method provided in the second aspect of the embodiment of the present application in a battery, the battery can have a good capacity retention rate based on the high ionic conductivity and significant high temperature resistance of the diaphragm, while having good safety performance and service life.
[0062] In some embodiments, the battery comprises a secondary battery.
[0063] The secondary battery has high energy density and good cycle stability. Based on the characteristics of the diaphragm, such a secondary battery can be well applied in the field of power batteries or energy storage system power supplies.
[0064] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising the battery provided in the third aspect of the present application.
[0065] By adopting the battery provided in the third aspect of the embodiment of the present application, such an electrical device has a high capacity retention rate and a long service life, and can work for a longer period of time.
[0066] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0068] Figure 1 is a schematic structural diagram of a diaphragm according to an embodiment of the present application;
[0069] Figure 2 1 is a schematic flow chart of a method for preparing a diaphragm according to an embodiment of the present application;
[0070] Figure 3 This is a schematic structural diagram of an implementation of a secondary battery in an embodiment of the present application;
[0071] Figure 4 for Figure 3 An exploded schematic diagram of a secondary battery is shown;
[0072] Figure 5 This is a schematic structural diagram of an implementation scheme of a battery module according to an embodiment of the present application;
[0073] Figure 6 This is a schematic structural diagram of an implementation scheme of a battery pack according to an embodiment of the present application;
[0074] Figure 7 for Figure 6 A schematic diagram of the exploded structure of the battery pack shown;
[0075] Figure 8It is a schematic diagram of an implementation of an electrical device including the battery of an embodiment of the present application as a power source.
[0076] Description of reference numerals:
[0077] 11-first base film; 12-second base film; 13-coating; 20-battery cell; 21-housing; 22-top cover assembly; 23-electrode assembly; 30-battery module; 40-battery pack; 41-upper box; 42-lower box. DETAILED DESCRIPTION
[0078] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0079] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0080] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0081] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0082] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0083] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two), and similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces). "At least one" refers to more than one (including one, two, three, etc.).
[0084] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0085] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0086] In the context of energy conservation and emission reduction, new energy technologies are developing rapidly, among which the research breakthroughs and applications of battery technology are the most significant. In ion batteries such as lithium-ion batteries, battery separators are one of the important components.
[0087] The separator is a microporous membrane used to separate the positive electrode and the negative electrode. It is a polymer functional material with a nano-scale microporous structure. Its main function is to separate the positive and negative active materials of the battery to reduce the risk of short circuit between the two electrodes, while allowing electrolyte ions to pass through. The performance of the separator determines the interface structure and internal resistance of the battery, and directly affects the capacity, cycle and safety performance of the battery.
[0088] Although the commonly used diaphragms on the market have good mechanical properties, the surface polarity of the commonly used diaphragms is low, resulting in poor liquid absorption and retention capabilities, which affects the ionic conductivity of the diaphragm. Such diaphragms are used in batteries, which affects the ion migration of the battery during the charging and discharging process, thereby increasing the internal resistance of the battery and seriously affecting the service life of the battery. At the same time, the commonly used diaphragm materials have a low melting point, and the battery will release heat during the charging and discharging process, especially when short-circuited or overcharged, a large amount of heat will be released. Therefore, when the temperature rises, the low-melting-point diaphragm material is prone to thermal runaway.
[0089] In practical applications, technicians generally modify and modify the diaphragm. For example, a ceramic coating is applied to the surface of the diaphragm. Although the ceramic coating can improve the wettability of the diaphragm to the electrolyte to a certain extent, the ceramic is prone to powdering, which affects its stability. Although flame retardants are currently used in diaphragms, they are generally used in the diaphragm base film, that is, the flame retardant and the base material are mixed to form the base film, which has limited effect on improving the wettability of the base film.
[0090] Based on the above considerations, in order to overcome the defects of the diaphragm, the embodiment of the present application designs a diaphragm using ceramics and flame retardants in the coating between the first base film and the second base film. By utilizing the protective effect of the first base film and the second base film on the ceramics and the flame retardant, and the effect of the combination of ceramics and flame retardants on improving ionic conductivity and high temperature resistance, the diaphragm provided in the embodiment of the present application can be used in a battery to significantly improve the capacity retention rate of the battery, as well as the safety performance and service life of the battery.
[0091] Therefore, the following technical solution is proposed.
[0092] Diaphragm
[0093] In the first aspect, the present application embodiment provides a diaphragm, please refer to Figure 1 The diaphragm includes a first base film 11, a second base film 12, and a coating 13. The coating 13 is located between the first base film 11 and the second base film 12, and the coating 13 contains ceramic and a flame retardant.
[0094] The first base film 11 and the second base film 12 refer to base films made of a diaphragm substrate. The diaphragm substrate is generally a polymer material. The diaphragm substrate as a main material can be made into a base film with a microporous structure, which can meet the mechanical properties and electrochemical properties required by the battery diaphragm.
[0095] The coating 13 refers to a functional layer formed by coating the surface of the first base film 11 relative to the second base film 12, or the surface of the second base film 12 relative to the first base film 11. The coating 13 is located between the first base film 11 and the second base film 12, and the first base film 11, the coating 13 and the second base film 12 are bonded together to form a diaphragm. Ceramic and flame retardant functional materials are used in the coating 13. The ceramic has good thermal stability, which can improve the heat resistance of the diaphragm, while enhancing the mechanical strength and reducing the shrinkage of the diaphragm, and increasing the wettability and liquid retention of the diaphragm. The flame retardant has flame retardancy, and the combination with thermally stable ceramics used in the coating 13 can further improve the heat resistance of the diaphragm.
[0096] The embodiment of the present application applies ceramic and flame retardant materials to the coating 13 between the first base film 11 and the second base film 12, and utilizes the double-layer superposition composite effect of the first base film 11 and the second base film 12 to improve the overall mechanical strength of the diaphragm, and at the same time, the ceramic and flame retardant in the coating 12 are not easy to fall off, thereby reducing the risk of diaphragm powdering. At the same time, based on the good wettability and heat resistance of the ceramic in the coating 13, it can not only improve the liquid absorption and liquid retention ability of the diaphragm, thereby improving the ionic conductivity, but also work together with the flame retardant to improve the high temperature resistance of the diaphragm. Therefore, the diaphragm provided in the embodiment of the present application can be used in a battery to significantly improve the capacity retention rate, safety performance and service life of the battery.
[0097] The ceramic in the coating 13 may be ceramic powder, which may be an aggregate of many small ceramic particles; the flame retardant may be flame retardant powder, which may be an aggregate of many small flame retardant particles.
[0098] In some embodiments, the average particle size represents a scale of the geometric size of the dispersed solid particle group. In this application, the average particle size is represented by D50, that is, the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%. Ceramics include ceramic particles with an average particle size of 0.01 μm to 1 μm; in the exemplary embodiment, the average particle size of the ceramic can be 0.01 μm, 0.05 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, etc., which are typical but non-limiting average particle sizes. The flame retardant includes flame retardant particles having an average particle size of 0.02μm to 2μm; in the exemplary embodiment, the average particle size of the flame retardant particles can be 0.02μm, 0.05μm, 0.1μm, 0.2μm, 0.3μm, 0.5μm, 0.6μm, 0.8μm, 1μm, 1.2μm, 1.5μm, 1.8μm, 2μm and other typical but non-limiting average particle sizes.
[0099] In the coating 13, ceramic particles with an average particle size of 0.01μm to 1μm and flame retardant particles with an average particle size of 0.02μm to 2μm have good dispersibility and can be evenly dispersed in the coating 13, so that the coating 13 has good flatness and good air permeability.
[0100] In some embodiments, the ceramic includes ceramic particles with an average particle size of 0.05 μm to 0.5 μm; the flame retardant includes flame retardant particles with an average particle size of 0.05 μm to 1 μm. The coating 13 uses ceramic particles with an average particle size of 0.05 μm to 0.5 μm and an average particle size of 0.05 μm to 1 μm, so that the overall dispersion and air permeability of the coating 13 are good.
[0101] In some embodiments, the ceramic material includes at least one of (γ-AlOOH), aluminum oxide (Al2O3), barium sulfate (BaSO4), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), silicon dioxide (SiO2), tin dioxide (SnO2), titanium oxide (TiO2), calcium oxide (CaO), zinc oxide (ZnO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), cerium oxide (CeO2), zirconium titanate (ZrTiO3), barium titanate (BaTiO3), and magnesium fluoride (MgF2); and the flame retardant includes at least one of metaborate, orthoborate, and polyborate.
[0102] Metaborates, orthoborates and polyborates can be classified as borate flame retardants. Borate flame retardants have a certain binding effect with anions, which can inhibit the migration of anions in the diaphragm. At the same time, the boron-containing anions (i.e., metaborate ions, orthoborate ions and polyborate ions) in the above-mentioned borate flame retardants have Lewis acid properties and can bind to polar bonds (XO represents, X is a cation such as Ca 2+ , Ba 2+ NH 4+ Mg 2+ 、Na + 、Zn 2+ In this way, the ion migration rate in the diaphragm can be further significantly improved by combining the ceramic material and the borate flame retardant in the coating 13.
[0103] In some embodiments, the metaborate includes at least one of calcium metaborate (CaB2O4), barium metaborate (BaB2O4), sodium metaborate (NaBO2), and ammonium metaborate (NH4BO2); the orthoborate includes zinc borate (B2O6Zn3); and the polyborate includes at least one of ammonium pentaborate (NH4B5O8) and sodium tetraborate (Na2B4O7). The selection of the types of these metaborates, orthoborates, and polyborates can significantly improve the ion migration rate and heat resistance safety performance of the diaphragm when combined with ceramic materials.
[0104] In some embodiments, the mass ratio of ceramic to flame retardant is greater than or equal to 1.05. The ceramic and flame retardant are used in the coating 13 in a certain mass ratio, and the performance of the ceramic and flame retardant can be comprehensively utilized. The ceramic and flame retardant are used in the coating 13 between the first base film 11 and the second base film 12 in a mass ratio of ceramic to flame retardant greater than or equal to 1.05, so that the overall wettability and heat resistance of the diaphragm are improved.
[0105] In some embodiments, the mass ratio of ceramic to flame retardant is (1.05-9): 1. In exemplary embodiments, the mass ratio of ceramic to flame retardant can be 1.05: 1, 1.5: 1, 2.0: 1, 2.5: 1, 3.0: 1, 3.5: 1, 3.8: 1, 4.0: 1, 5.0: 1, 7.0: 1, 9.0: 1, etc. Using ceramic and flame retardant in coating 13 according to the mass ratio of ceramic to flame retardant (1.05-9): 1 can make the overall wettability and heat resistance of the diaphragm better.
[0106] In some embodiments, the substrates of the first base film 11 and the second base film 12 may be the same or different, specifically including: at least one of polyolefin materials, fluorinated polymer materials and polyester materials. Among them, (1) polyolefin materials may include at least one of polyethylene (PE) and polypropylene (PP); polyethylene and polypropylene have the characteristics of low price, excellent mechanical properties and high electrochemical stability. Most commercial lithium-ion battery separator products are microporous membranes made of polyolefin materials, and the main raw materials are high molecular weight polyethylene and polypropylene. Such polyolefin materials have the advantages of high strength, good acid and alkali corrosion resistance, and waterproofness. Their industrial preparation is mature and their commercial applications are extensive. (2) Fluorinated polymer materials may include at least one of polytetrafluoroethylene, polyvinyl fluoride and polyvinylidene fluoride; fluorinated polymer materials have good polarity and dielectric constant. The above-mentioned fluorinated polymer materials can be used in batteries to improve the lyophilicity of the separator, and polyvinylidene fluoride is the most widely used. (3) Polyester materials may include polyethylene terephthalate. Polyethylene terephthalate, a polyester material, has good resistance to electrolyte corrosion. Therefore, the type of the base material of the polymer base film can be selected according to actual needs.
[0107] In some embodiments, the porosity of the first base film 11 is greater than the porosity of the second base film 12. Porosity affects the mechanical properties and air permeability of the material, and also affects the ion mobility. The embodiment of the present application utilizes the porosity difference between the first base film 11 and the second base film 12, so that the diaphragm after the first base film 11 and the second base film 12 are double-layered, while ensuring the mechanical strength of the diaphragm, it is also more conducive to improving the ion migration rate.
[0108] In some embodiments, the ratio of the porosity of the first base film 11 to the porosity of the second base film 12 is greater than or equal to 1.02. In an exemplary embodiment, the ratio of the porosity of the first base film 11 to the porosity of the second base film 12 can be 1.02 to 3.0, and the diaphragm formed by the combination of the first base film 11 and the second base film 12 with this porosity ratio is more conducive to ion migration.
[0109] Further, the porosity of the first base film 11 is greater than the porosity of the second base film 12, and the porosity of the first base film 11 is 32%-90%, and the porosity of the second base film 12 is 30%-85%. In the exemplary embodiment, the porosity of the first base film 11 can be 32%, 35%, 36%, 40%, 45%, 48%, 50%, 52%, 54%, 58%, 60%, 65%, 68%, 70%, 72%, 78%, 80%, etc., which are typical but non-limiting porosities. In the exemplary embodiment, the porosity of the second base film 12 can be 30%, 32%, 35%, 36%, 40%, 45%, 48%, 50%, 52%, 54%, 58%, 60%, 65%, 68%, 70%, 72%, 75%, etc., which are typical but non-limiting porosities. Under the above-mentioned porosity ratio conditions, selecting a first base membrane 11 with a porosity of 32%-90% and a second base membrane 12 with a porosity of 30%-85% can enrich the pore structure, which is not only beneficial to ion migration, but also makes the diaphragm as a whole have good air permeability and mechanical properties.
[0110] In some embodiments, the porosity of the first base film 11 is greater than the porosity of the second base film 12, and the porosity of the first base film 11 is 35%-85%, and the porosity of the second base film 12 is 34%-45%. The combination of the first base film 11 with a porosity of 35%-85% and the second base film 12 with a porosity of 34%-45% makes the overall mechanical properties, air permeability and ion mobility of the diaphragm good.
[0111] In some embodiments, the thickness of the first base film 11 is greater than the thickness of the second base film 12. By utilizing the thickness difference between the first base film 11 and the second base film 12, the mechanical strength of the entire separator can be well balanced, and the separator can be used for a long time in the battery.
[0112] In some embodiments, the ratio of the thickness of the first base film 11 to the thickness of the second base film 12 is 1.02 to 5.0. In an exemplary embodiment, the ratio of the thickness of the first base film 11 to the thickness of the second base film 12 can be 1.02, 1.5, 2.0, 2.2, 2.6, 2.8, 3.0, 3.2, 3.5, 3.8, 3.9, 4.0, 4.2, 4.6, 4.8, 5.0, etc.
[0113] In some embodiments, the thickness of the first base film 11 is greater than the thickness of the second base film 12, and the thickness of the first base film 11 is 2 μm to 13 μm, and the thickness of the second base film 12 is 1 μm to 12 μm. In the exemplary embodiment, the thickness of the first base film 11 can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, etc., which are typical but non-limiting thicknesses. In the exemplary embodiment, the thickness of the second base film 12 can be 1 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, etc., which are typical but non-limiting thicknesses. The combination of the first base film 11 with a thickness of 2μm to 13μm and the second base film 12 with a thickness of 1μm to 12μm not only makes the diaphragm as a whole have good mechanical properties, but also has a good protective effect on the ceramics and flame retardants in the middle coating 13, making it difficult for the ceramics and flame retardants to fall off.
[0114] In some embodiments, the thickness of the first base film 11 is greater than the thickness of the second base film 12, and the thickness of the first base film 11 is 3 μm to 6 μm, and the thickness of the second base film 12 is 2 μm to 5 μm. The combination of the first base film 11 with a thickness of 3 μm to 6 μm and the second base film 12 with a thickness of 2 μm to 5 μm not only makes the overall mechanical properties of the diaphragm good, the ceramic and flame retardant in the intermediate coating 13 are not easy to fall off, and the battery energy density can be well improved in the battery.
[0115] In some embodiments, the thickness of the coating 13 is 0.5 μm to 10 μm. In the exemplary embodiment, the thickness of the coating 13 can be 0.5 μm, 1 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc. Typical but non-limiting thicknesses. The coating 13 between the first base film 11 and the second base film 12 is coated with a thickness of 0.3 μm to 10 μm, so that the overall wettability and heat resistance of the diaphragm are well combined.
[0116] In some embodiments, the thickness of the coating 13 is 1 μm to 5 μm. The thickness of the coating 13 between the first base film 11 and the second base film 12 is 1 μm to 5 μm, which can improve the overall wettability and heat resistance of the diaphragm and make the diaphragm have good air permeability.
[0117] In some embodiments, the coating 13 further contains a binder, specifically, the coating 13 includes ceramics, a flame retardant and a binder. By using a binder in the middle coating 13, the binder can bind and fix the ceramics and the flame retardant in the coating 13, so that the ceramics and the flame retardant are not easy to fall off.
[0118] In some embodiments, the coating 13 includes ceramics, flame retardants and binders, and the binder includes at least one of polyacrylate, acrylic acid and carboxymethyl cellulose. The above binders have good adhesion and can play a good role in the adhesion of ceramics and flame retardants in the coating 13.
[0119] In some embodiments, the coating 13 includes ceramic, flame retardant and binder, and the mass ratio of binder to ceramic is (0.01-0.3): 1. In an exemplary embodiment, the mass ratio of binder to ceramic can be 0.05: 1, 0.15: 1, 0.2: 1, 0.25: 1, 0.3: 1, etc. Under the above ratio conditions, the ceramic adhesion effect in the coating 13 is good, and the thickness of the coating 13 is slightly affected.
[0120] In some embodiments, the diaphragm includes a first base film 11, a second base film 12, and a coating 13. The ratio of the porosity of the first base film 11 to the porosity of the second base film 12 can be 1.02-3.0, and the porosity of the first base film 11 is 35%-85%, and the porosity of the second base film 12 is 34%-45%. The ratio of the thickness of the first base film 11 to the thickness of the second base film 12 is 1.02-5.0, the thickness of the first base film 11 is 3μm-6μm, and the thickness of the second base film 12 is 2μm-5μm. The coating 13 has a thickness of 1-5μm and contains ceramics, flame retardants and binders. The ceramics are ceramic particles with an average particle size of 0.05μm-0.5μm, and the flame retardants are flame retardant particles with an average particle size of 0.05μm-1μm. The mass ratio of ceramics, flame retardants and binders is 8:2:1. Such a diaphragm has better comprehensive effects in mechanical properties, air permeability, thermal stability and ion mobility.
[0121] Preparation method of diaphragm
[0122] In a second aspect, the present application provides a method for preparing a diaphragm. Figure 2 As shown, the method for preparing the diaphragm comprises the following steps:
[0123] S01: Prepare slurry containing ceramic and flame retardant;
[0124] S02: coating the slurry on the surface of the first base film 11 to form a slurry coating layer, and then covering the second base film 12 on the slurry coating layer, performing a lamination process, and obtaining a diaphragm.
[0125] The embodiment of the present application adopts a wet coating film-forming process, and a slurry containing ceramics and flame retardants is coated on the surface of the first base film 11 to form a slurry coating, and then the second base film 12 is covered and laminated to obtain the diaphragm of the embodiment of the present application. Such a preparation method is not only simple in process and low in preparation cost, but also can obtain a diaphragm with good ionic conductivity and high temperature resistance.
[0126] In some embodiments, the material type, porosity, thickness of the first base film 11 and the second base film 12 , and the material type and ratio of the ceramic and the flame retardant have been described in detail above.
[0127] In some embodiments, the step of preparing the slurry containing ceramics and flame retardants includes: dissolving the ceramics and flame retardants in water, and then adding a binder and stirring to obtain the slurry. By adding the binder to the slurry, the slurry can have good viscosity, and the ceramics and flame retardants in the slurry can be better bonded to form a film between the first base film 11 and the second base film 12.
[0128] In some embodiments, the mass concentration of ceramic in the slurry is 50% to 90%. In the exemplary examples, the mass concentration of ceramic can be 50%, 52%, 54%, 58%, 60%, 65%, 68%, 70%, 72%, 78%, 80%, 85%, 90% and other typical but non-limiting mass concentrations. The mass concentration of flame retardant is 10% to 50%. In the exemplary examples, the mass concentration of flame retardant can be 10%, 12%, 14%, 18%, 20%, 25%, 28%, 30%, 32%, 38%, 40%, 45%, 50% and other typical but non-limiting mass concentrations. In the slurry of the above mass concentration, ceramic and flame retardant are evenly dispersed, and the prepared slurry is easy to coat into a film.
[0129] In some embodiments, the binder added to the slurry includes at least one of polyacrylate, acrylic acid and carboxymethyl cellulose. The ratio of the binder in the slurry is calculated based on the mass ratio of the binder to the ceramic in the coating 13 after film formation (0.01-0.3):1. The above-mentioned binder types have good viscosity, so that the ceramic and flame retardant in the middle of the final diaphragm are not easy to fall off. The above-mentioned ratio conditions have good adhesion effects and have little effect on the final coating thickness.
[0130] In some embodiments, the lamination process includes a roller lamination process. After roller lamination, the first base film, the second base film and the intermediate coating layer can be better laminated. The slurry coating formed by coating the slurry on the surface of the first base film 11 contains water-soluble substances, so the slurry coating is subsequently dried to remove the solvent to form a solvent-free coating layer 13, so that the two film layers and the intermediate coating layer 13 are fully laminated.
[0131] Battery
[0132] In a third aspect, an embodiment of the present application provides a battery, comprising a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator provided in the first aspect of the embodiment of the present application and / or the separator prepared by the preparation method provided in the second aspect of the embodiment of the present application.
[0133] By using the diaphragm provided by the first aspect of the embodiment of the present application and / or the diaphragm prepared by the preparation method provided by the second aspect of the embodiment of the present application in a battery, the battery can have a good capacity retention rate based on the high ionic conductivity and significant high temperature resistance of the diaphragm, thereby having charge and discharge cycle stability, as well as good safety performance and service life.
[0134] The first base film 11 of the separator may be adjacent to the positive electrode, and the second base film 12 may be adjacent to the negative electrode. Alternatively, the first base film 11 of the separator may be adjacent to the negative electrode, and the second base film 12 may be adjacent to the positive electrode.
[0135] In some embodiments, the battery is a secondary battery. In the exemplary embodiment, the secondary battery can be an ion battery or a sodium ion battery, etc. Such a secondary battery in the embodiment of the present application has high energy density and good cycle stability, and based on the advantages of the diaphragm in the embodiment of the present application, such a secondary battery is well used as a power battery or a power source for an energy storage system.
[0136] In some embodiments, the secondary battery of the present application may include any one of a battery cell, a battery module, and a battery pack.
[0137] The battery cell refers to a battery housing and a battery cell encapsulated in the battery housing. The shape of the battery cell is not particularly limited and can be cylindrical, square or any other shape. Figure 3 The battery cell 20 shown has a square structure.
[0138] In some embodiments, Figure 4As shown, the outer packaging of the battery cell 20 may include a shell 21 and a top cover assembly 22. The shell 21 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 21 has an opening connected to the receiving cavity, and the top cover assembly 22 is used to cover the opening to close the receiving cavity. The positive electrode, diaphragm and negative electrode sheet contained in the secondary battery of the embodiment of the present application can form an electrode assembly 23 through a winding process and / or a lamination process. The electrode assembly 23 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 23. The number of electrode assemblies 23 contained in the battery cell 20 may be one or more, which can be adjusted according to actual needs.
[0139] The preparation method of the battery cell 20 is well known. In some embodiments, the positive electrode, the separator, the negative electrode sheet and the electrolyte can be assembled to form the battery cell 20. As an example, the positive electrode, the separator and the negative electrode sheet can be formed into an electrode assembly 23 through a winding process or a lamination process, and the electrode assembly 23 is placed in an outer package, dried and then injected with electrolyte, and the battery cell 20 is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0140] The battery module is assembled from the battery cells 20 , that is, it may contain a plurality of the battery cells 20 , and the specific number can be adjusted according to the application and capacity of the battery module.
[0141] In some embodiments, Figure 5 FIG. 3 is a schematic diagram of a battery module 30 as an example. Figure 5 As shown, in the battery module 30, the plurality of battery cells 20 may be arranged in sequence along the length direction of the battery module 30. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 20 may be fixed by fasteners.
[0142] Optionally, the battery module 30 may further include a housing having an accommodation space, and the plurality of battery cells 20 may be accommodated in the accommodation space.
[0143] A battery pack is composed of the above-mentioned battery cells 20, that is, it may contain multiple battery cells 20, wherein multiple battery cells 20 may be assembled into the above-mentioned battery module 30. The specific number of battery cells 20 or battery modules 30 contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0144] As in the embodiment, Figure 6 and Figure 7 4 is a schematic diagram of an exemplary battery pack 40. The battery pack 40 may include a battery box and a plurality of battery modules 30 disposed in the battery box. The battery box includes an upper box body 41 and a lower box body 42, wherein the upper box body 41 is used to cover the lower box body 42 and form a closed space for accommodating the battery modules 30. The plurality of battery modules 30 may be arranged in the battery box in any manner.
[0145] Electrical devices
[0146] In a fourth aspect, the present application also provides an electric device, which includes the battery of the above-mentioned application. The battery can be used as a power source for the electric device, or as an energy storage unit for the electric device. Therefore, the electric device of the present application has a high capacity retention rate, good stability and safety in use.
[0147] The electrical device may be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc. The electrical device may select a secondary battery, a battery module or a battery pack according to its use requirements.
[0148] Figure 8 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.
[0149] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.
[0150] Example
[0151] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0152] 1. Diaphragm and its preparation method embodiment
[0153] Example A1
[0154] A diaphragm includes a first base film 11, a second base film 12, and a coating 13 located between the first base film 11 and the second base film 12. The first base film 11 is made of polypropylene (PP), with a thickness of 5 μm and a porosity of 48%; the second base film 11 is made of polyethylene (PE), with a thickness of 3 μm and a porosity of 50%; the coating 13 is 0.5 μm thick and contains ceramics, flame retardants and binders, the ceramics are aluminum oxide particles with an average particle size of 0.01 μm, the flame retardant is calcium metaborate with an average particle size of 0.02 μm, the binder is carboxymethyl cellulose, and the mass ratio of ceramics, flame retardants and binders is 8:2:1. See Table 1 for details.
[0155] The preparation method of the diaphragm comprises the following steps:
[0156] S11: adding ceramics, flame retardant and binder into water according to proportion and stirring to obtain slurry.
[0157] S12: The slurry obtained in the above step is coated on the first base film 11 to form a slurry coating layer, and then the second base film 12 is covered on the slurry coating layer, and the slurry coating layer is rolled and laminated, and then dried to obtain a finished diaphragm.
[0158] Example A2
[0159] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0160] Example A3
[0161] A diaphragm includes a first base film 11, a second base film 12, and a coating 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0162] Example A4
[0163] A diaphragm includes a first base film 11, a second base film 12, and a coating 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0164] Example A5
[0165] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0166] Example A6
[0167] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0168] Example A7
[0169] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0170] Example A8
[0171] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1. The preparation method of the diaphragm is similar to that of Example A1.
[0172] Comparative Example A1
[0173] A diaphragm includes a first base film 11 and a coating 13 located on the surface of the first base film 11. The materials of each layer are shown in Table 1.
[0174] Comparative Example A2
[0175] A diaphragm includes a second base film 12 and a coating 13 located on the surface of the second base film 12. The materials of each layer are shown in Table 1.
[0176] Comparative Example A3
[0177] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1.
[0178] Comparative Example A4
[0179] A diaphragm includes a first base film 11, a second base film 12, and a coating layer 13 located between the first base film 11 and the second base film 12. The materials of each layer are shown in Table 1.
[0180] 2. Secondary battery cell example
[0181] Example B1
[0182] A secondary battery cell includes a battery core formed by a positive electrode sheet, a separator and a negative electrode sheet, and also includes an electrolyte.
[0183] The diaphragm is the diaphragm provided in Example A1. The preparation method of the secondary battery comprises:
[0184] Preparation of positive electrode: Using methyl pyrrolidone (NMP) as solvent, LiNi 0.8 Co 0.1Mn 0.1 O2, carbon nanotubes (CNT), and binder (PVDF) are mixed in a mass ratio of 97:2:1 to prepare a positive electrode slurry with a solid content of 80%; the positive electrode slurry is evenly coated on an aluminum foil for double-sided coating, wherein the surface density of each single side is 0.112 mg / mm 2 After being fully dried, cold pressed and cut, the positive electrode sheet is obtained as the positive electrode.
[0185] Preparation of negative electrode sheet: Using water as solvent, artificial graphite, conductive agent SP, dispersant (CMC), and binder (SBR) are mixed in a mass ratio of 96:1:1:2 to prepare a negative electrode slurry with a solid content of 58%; the positive electrode slurry is evenly coated on the aluminum foil for double-sided coating, where the surface density of each single side is 0.170 mg / mm 2 After being fully dried, cold pressed and cut, the negative electrode sheet is obtained as the negative electrode.
[0186] Electrolyte: At room temperature, ethylene carbonate (EC) / diethyl carbonate (DEC) were mixed in a volume ratio of 1:1, and LiPF6 was added to the mixed solution to obtain a solution with a concentration of 1 mol / L as the electrolyte;
[0187] Secondary battery assembly: In a low-humidity constant temperature room, the positive and negative electrode plates prepared as above are stacked and wound in the order of "positive electrode-diaphragm-negative electrode" to form a bare cell, and then filled with electrolyte to assemble into a lithium-ion secondary battery.
[0188] Example B1 to Example B8 and Comparative Example B1 to Comparative Example B4;
[0189] The present embodiment B1 to embodiment B8 and comparative examples B1 to comparative examples B4 respectively provide a secondary battery cell, each of which includes a battery cell formed by a positive electrode sheet, a separator and a negative electrode sheet, and also includes an electrolyte. Among them, the separators of embodiments B1 to embodiments B8 and comparative examples B1 to comparative examples B4 correspond to the separators provided by embodiments A1 to embodiments A8 and comparative examples A1 to comparative examples A4 respectively. Among them, the separator in the above embodiment A1 is used as the separator in the battery cell of the secondary battery embodiment B1, the separator in the embodiment A2 is used as the separator in the battery cell of the secondary battery embodiment B2, and so on, the separator in comparative example A4 is used as the separator in the battery cell of the battery comparative example B4.
[0190] Performance Testing
[0191] The separators and secondary battery cells of the above-mentioned embodiments and comparative examples were tested respectively.
[0192] (1) Ion mobility test of the diaphragm:
[0193] The prepared diaphragm is cut into circular diaphragms, and a stainless steel sheet is used as a counter electrode to assemble a button cell. The electrochemical AC impedance of the button cell is tested to obtain the resistance value. The ionic conductivity of the diaphragm is calculated according to the formula: σ = L / (R×S), where: σ is the ionic conductivity, L is the thickness of the diaphragm, R is the resistance value, and S is the area of the diaphragm.
[0194] (2) Diaphragm heat resistance test:
[0195] Sample preparation: Punch the prepared isolation film into samples with a width of 50 mm and a length of 100 mm along the TD and MD directions using a punching machine. Place 5 parallel samples on A4 paper, and then place the A4 paper with the samples on corrugated paper with a thickness of 1 mm to 5 mm.
[0196] Sample test: Set the temperature of the blast oven to 150°C. After the temperature reaches the set temperature and stabilizes for 30 minutes, put the A4 paper placed on the corrugated paper into the blast oven and start timing. After the set time (1 hour in this application) is reached, measure the length and width of the isolation film, and mark the values as a and b respectively.
[0197] Calculation of thermal shrinkage: longitudinal (MD) thermal shrinkage = [(100-a) / 100] × 100%, transverse (TD) thermal shrinkage = [(50-b) / 50] × 100%, and the average value of 5 parallel samples is taken as the test result.
[0198] (3) Diaphragm air permeability test:
[0199] Cut the membrane of appropriate size and fix it on the membrane permeability instrument. The test instrument is applied under 1.21kPa pressure. The area through which 100mL (1ml = 1cc) of air passes is 642mm. 2 The time required for gas to pass through the membrane is the membrane's air permeability value (sec / 100cc).
[0200] The test results of the diaphragm are shown in Table 1.
[0201] Table 1
[0202]
[0203] From the test results in Table 1, we can see that:
[0204] The diaphragm of the embodiment of the present application has better ion mobility, lower heat shrinkage and air permeability than the comparative example. The embodiment of the present application compounds two base films with suitable porosity to ensure a certain porosity while having high mechanical strength as a whole. The ceramic particles and the flame retardant are present in the coating between the two base films. The ceramic makes the diaphragm have good heat resistance. The flame retardant and the ceramic can further improve the ionic conductivity of the diaphragm. The two complement each other to improve the heat resistance stability and ion mobility of the diaphragm.
[0205] (4) Battery room temperature cycle performance test:
[0206] The secondary battery cells of Examples B1 to B8 and Comparative Examples B1 to B4 were discharged at a constant current of 1C to a termination voltage and left to stand for 10 min; then they were charged at a constant current and constant voltage of 1C, and the charging was stopped at a cutoff current of 0.02C. This cycle was repeated 500 times. The first discharge capacity was recorded as C1, and the 500th discharge capacity was recorded as C2. The discharge capacity retention rate was calculated according to the formula = C2 / C1, thereby obtaining the discharge capacity retention rate.
[0207] (5) High temperature heat resistance test of the battery:
[0208] Place the fully charged battery in an oven at 150°C and heat it for 1 hour. During the heating process, if the battery short-circuit, catch fire or explode, it means that the diaphragm has poor heat resistance. If the battery does not catch fire or explode, it means that the diaphragm has good heat resistance.
[0209] The test results of the battery are shown in Table 2.
[0210] Table 2
[0211] Implementation Capacity retention rate 150℃ battery heating Example B1 97% No fire Example B2 92% No fire Example B3 93% No fire Example B4 96% No fire Example B5 94% No fire Example B6 93% No fire Comparative Example B1 91% Fire breaks out, fire quickly subsides Comparative Example B2 90% Fire breaks out, fire quickly subsides Comparative Example B3 92% Fire breaks out, fire quickly subsides Comparative Example B4 85% No fire
[0212] From the test results in Table 2, we can see that:
[0213] The battery of the embodiment of the present application has better capacity retention and safety performance than the comparative example. Because the ceramic particles and flame retardant in the battery's diaphragm coating are present in the two base films, on the one hand, the ceramic particles make the diaphragm have good heat resistance, improve the heat resistance and safety performance of the battery, and also have good liquid absorption and retention capabilities; on the other hand, the flame retardant has flame retardant properties, and can be mixed with ceramics to further improve the ionic conductivity of the diaphragm, thereby improving the capacity retention of the battery. Therefore, the comprehensive use of ceramic particles and flame retardant particles can make the battery have both high capacity retention rate and safety performance and service life.
[0214] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A diaphragm, characterized in that: The invention comprises a first base film, a second base film and a coating layer located between the first base film and the second base film, wherein the coating layer contains ceramics and a flame retardant.
2. The diaphragm according to claim 1, wherein The ceramic comprises ceramic particles having an average particle size of 0.01 μm to 1 μm; and / or, The flame retardant comprises flame retardant particles with an average particle size of 0.02 μm to 2 μm.
3. The diaphragm according to claim 2, wherein The ceramic comprises ceramic particles having an average particle size of 0.05 μm to 0.5 μm; and / or, The flame retardant comprises flame retardant particles with an average particle size of 0.05 μm to 1 μm.
4. The diaphragm according to any one of claims 1 to 3, characterized in that The ceramic material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, yttrium oxide, cerium oxide, zirconium titanate, barium titanate and magnesium fluoride; and / or, The flame retardant includes at least one of metaborate, orthoborate and polyborate.
5. The diaphragm according to claim 4, wherein The metaborate includes at least one of calcium metaborate, barium metaborate, sodium metaborate, and ammonium metaborate; or The orthoborate comprises zinc borate; or The polyborate includes at least one of ammonium pentaborate and sodium tetraborate.
6. The diaphragm according to any one of claims 1 to 5, characterized in that The mass ratio of the ceramic to the flame retardant is greater than or equal to 1.
05.
7. The diaphragm according to claim 6, wherein The mass ratio of the ceramic to the flame retardant is (1.05-9):
1.
8. The diaphragm according to any one of claims 1 to 7, characterized in that The base materials of the first base film and the second base film independently include at least one of a polyolefin material, a fluorine-containing polymer material and a polyester material.
9. The diaphragm according to any one of claims 1 to 8, characterized in that The porosity of the first base film is greater than the porosity of the second base film.
10. The diaphragm according to claim 9, wherein The ratio of the porosity of the first base film to the porosity of the second base film is greater than or equal to 1.02; and / or The porosity of the first base film is 32% to 90%, and the porosity of the second base film is 30% to 85%.
11. The diaphragm according to claim 10, wherein The porosity of the first base film is 35% to 85%, and the porosity of the second base film is 34% to 45%.
12. The diaphragm according to any one of claims 1 to 11, characterized in that The thickness of the first base film is greater than the thickness of the second base film.
13. The diaphragm according to claim 12, wherein The ratio of the thickness of the first base film to the thickness of the second base film is (1.02-5.0):1; and / or The thickness of the first base film is 2 μm to 13 μm, and the thickness of the second base film is 1 μm to 12 μm.
14. The diaphragm according to claim 13, wherein The thickness of the first base film is 3 μm to 6 μm, and the thickness of the second base film is 2 μm to 5 μm.
15. The diaphragm according to any one of claims 1 to 14, characterized in that The thickness of the coating is 0.5 μm to 10 μm.
16. The diaphragm according to claim 15, wherein The thickness of the coating is 1 μm to 5 μm.
17. The diaphragm according to any one of claims 1 to 16, characterized in that The coating also contains a binder.
18. The diaphragm according to claim 17, wherein The binder comprises at least one of polyacrylate, acrylic acid and carboxymethyl cellulose; and / or, The mass ratio of the binder to the ceramic is (0.01-0.3):
1.
19. A method for preparing a diaphragm according to any one of claims 1 to 16, characterized in that: The following steps are involved: preparing a slurry containing the ceramic and the flame retardant; The slurry is coated on the surface of the first base film to form a slurry coating layer, and then the second base film is covered on the slurry coating layer and subjected to a lamination process to obtain the diaphragm.
20. The preparation method according to claim 19, wherein The step of preparing the slurry containing the ceramic and the flame retardant comprises: dissolving the ceramic and the flame retardant in water, then adding a binder and stirring to obtain the slurry.
21. The preparation method according to claim 20, characterized in that The binder comprises at least one of polyacrylate, acrylic acid and carboxymethyl cellulose; and / or, The mass ratio of the binder to the ceramic is (0.01-0.3):
1.
22. The preparation method according to any one of claims 19 to 21, characterized in that: In the slurry, the mass concentration of the ceramic is 50% to 90%, and the mass concentration of the flame retardant is 10% to 50%.
23. A battery, characterized in that: The invention comprises a positive electrode, a negative electrode and a separator placed between the positive electrode and the negative electrode, wherein the separator is the separator according to any one of claims 1 to 18 or the separator prepared by the preparation method according to any one of claims 19 to 22.
24. The battery according to claim 23, wherein The battery includes a secondary battery.
25. An electrical device, characterized in that: The electrical device comprises the battery according to claim 23 or 24.
Citation Information
Cited By
Composite diaphragm, preparation method thereof and lithium ion battery
CN121642426A
Separator film and preparation method therefor, and battery and electric device
EP4632929A1
Separator film and preparation method therefor, and battery and electric device
WO2024212527A1