Copper powder and method for producing copper powder
By covering the surface of the copper powder with chain organic matter in the polyol solvent, the problem of oxidation coating hindering the sintering of the copper powder during low-temperature sintering is solved, and excellent low-temperature sintering in an inactive atmosphere is achieved, making it suitable for large-scale production. .
Patent Information
- Application Number
- CN202380023999.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-18
AI Technical Summary
Existing copper powder easily forms an oxide film that hinders sintering during the low-temperature sintering process, resulting in deterioration of sintering properties. It also requires high vacuum or ultra-high vacuum conditions, making it difficult to apply in large-scale production.
By mixing chain organic matter with appropriate molecular weight and functional groups in a polyol solvent to cover the surface of the copper powder, a copper powder with excellent oxidation resistance and low-temperature sintering is formed, ensuring low-temperature sintering in an inactive atmosphere.
It achieves low-temperature sintering in an inactive atmosphere, avoids the formation of oxide films, improves the sintering properties of copper powder, and is suitable for large-scale production.
Smart Images

Figure CN118804807A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to copper powder obtained by heating copper oxide powder or copper powder in a polyol solvent and a method for producing the copper powder. Background Art
[0002] Copper powder is also used as a material for conductive pastes that form internal electrodes / external electrodes of multilayer ceramic capacitors (MLCCs) as electronic components, electrodes of multilayer ceramic substrates, etc. In recent years, the thinning of internal electrodes has been advancing with the miniaturization / larger capacity of multilayer ceramic capacitors, so in this application, the copper powder used in the above conductive paste (internal electrode paste) is also required to be fine. In particular, metal fine particles with an average particle size of less than 250nm are different from conventional particles of submicron level or above, and have a low sintering temperature, so they are considered to be used in low-temperature sintering pastes, etc.
[0003] In addition, metal powder sintered at low temperature has the characteristics of not only less heat load during sintering and residual stress during cooling, but also stable existence without melting until the melting point of bulk metal after sintering. Therefore, low-temperature sintered metal powder has attracted much attention in the field of chip mounting of printed electronics and power modules that operate at high temperatures, where thermal damage to the substrate is not desired.
[0004] Currently, nano-sized silver powder is widely used as a low-temperature sintered metal powder, but it is expensive and has the disadvantages of ion migration. Therefore, in recent years, low-temperature sintering of copper powder, which is cheap and has excellent ion migration resistance, has been actively developed.
[0005] In the low-temperature sintering of copper powder, it is effective to make the particles finer and increase the surface energy, as with other metal powders. However, if the particles are finer, the copper powder is easily oxidized, and if surface oxidation occurs, the sintering property will be deteriorated. Therefore, an oxidation-resistant film (antioxidation film) is required on the surface of the copper powder, and further, the oxidation-resistant film itself must be decomposed at low temperatures to avoid hindering sintering.
[0006] That is, the following two points are essential for low-temperature sintering of copper powder: fine particles and an oxidation-resistant film that does not hinder low-temperature sintering.
[0007] In contrast, Patent Document 1 discloses a copper powder that has both oxidation resistance and low-temperature sintering properties, with the particle size and particle size distribution adjusted to a certain range by physically adsorbing an aliphatic carboxylic acid having an aliphatic group with a carbon number of 5 or more on the surface of copper particles. As a result, even when the SEM primary particle size of the copper powder is 100 nm or less, oxidation after long-term standing in the atmosphere is not confirmed by XRD, and further, sintering at 300° C. in a nitrogen atmosphere is still possible.
[0008] In addition, Patent Document 2 discloses a copper powder that can be low-temperature calcined under a high vacuum condition of 0.01 Pa or less by having a cuprous oxide coating on the surface of the copper powder controlled to a certain ratio or average coating thickness. Thus, the copper powder that further protects the cuprous oxide layer covering the copper powder with caproic acid can achieve a vacuum degree of 3×10 -6 Sintering at 100°C under the condition of Pa.
[0009] In addition to the above-mentioned methods, Patent Document 3 discloses a method of heating and reducing copper oxide powder (raw material) in a polyol solvent (polyol method). The copper powder produced by this method is characterized by excellent oxidation resistance based on the organic film formed during reduction. Thus, by adding a silver salt for nucleation and adding polyvinyl pyrrolidone as a dispersant, copper fine particles with a particle size of 100 nm or less with silver as the core can be obtained.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2016-176146
[0013] Patent Document 2: International Publication No. 2019 / 106739
[0014] Patent Document 3: Japanese Patent Application Publication No. 2005-097677 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] However, it is known that the copper powder described in Patent Document 1 contains a large amount of organic components, and the aliphatic carboxylic acid is covered with a high density close to a liquid condensate film. Such organic components existing in large quantities on the copper surface will generate gas during pyrolysis and volatilization, and thus may cause failures caused by gas generation, such as expansion and short circuit in the formation of internal electrodes of MLCC.
[0017] In addition, the copper powder described in Patent Document 3 contains 40% by mass of polyvinyl pyrrolidone, a high molecular polymer, as a dispersant, relative to copper.
[0018] The oxide film formed on the surface of the copper powder can hinder sintering even if it is an extremely thin layer of about several nanometers. Therefore, for the copper powder described in the above-mentioned Patent Document 1, no XRD peak derived from the oxide was detected immediately after synthesis and after storage at 25°C in the atmosphere for 4 months. However, considering the detection sensitivity of XRD, it is difficult to use XRD to determine whether there is an oxide film that can hinder sintering.
[0019] Similarly, the copper powder described in the above-mentioned Patent Document 2 forms an oxide film, which may cause the generation of water vapor accompanying the reduction of the oxide film in a reducing atmosphere and hinder the sintering in an inert atmosphere. Furthermore, in order to perform the disclosed low-temperature sintering, high vacuum or ultra-high vacuum conditions are required, which is difficult to apply to heating furnaces for mass production such as conveyor-type continuous heating furnaces.
[0020] The present invention has been made in view of the above-mentioned conventional situation, and an object of the present invention is to provide a copper powder having an organic film for preventing the formation of an oxide film which may hinder sintering and having excellent low-temperature sintering properties.
[0021] Solutions for solving problems
[0022] The present inventors conducted intensive research to solve the above problems and found that when the surface of copper powder produced using polyol is covered with a mixture of an organic substance derived from a polyol solvent and a chain organic substance having an appropriate molecular weight and functional group, a copper powder having both excellent oxidation resistance and low-temperature sintering properties can be obtained, thereby completing the present invention. That is, the present invention provides the following solution.
[0023] According to the present invention, there is provided a copper powder having an average particle size of 250 nm or less, having a surface covered with an organic substance, and satisfying all of the following conditions (1) to (4).
[0024] (1) When organic matter present on the surface of the copper powder is detected by gas chromatography-mass spectrometry (GC / MS),
[0025] Detected by
[0026] H(-O-CH2-CH2) n -OH (wherein n is an integer of 1 to 4),
[0027] HOOC-CH2(-O-CH2-CH2) m -OH (wherein m is an integer of 1 to 3),
[0028] HOOC-CH2(-O-CH2-CH2) l -O-CH2-COOH (wherein l is 1 or 2),
[0029] H(-C3H6O) s -OH (wherein s is an integer of 1 to 4),
[0030] HOOC-CH(CH3)(-C3H6O) t -OH (wherein t is an integer of 1 to 3),
[0031] HOOC-CH(CH3)(-C3H6O)u One or more members selected from the group consisting of -O-CH(CH3)-COOH (wherein u is 1 or 2).
[0032] (2) When organic matter present on the surface of the copper powder is detected by liquid chromatography-mass spectrometry (LC / MS),
[0033] A chain organic substance with a molecular weight of more than 200 and less than 1000 was detected, and the chain organic substance had at the end of the molecule one selected from the group consisting of a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), an aldehyde group (-CHO), a nitro group (-NO2), a thiol group (-SH), a sulfone group (-SO3HHH), a phosphate group (-PO4H2), a cyano group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodo group (-I), which are functional groups that can coordinate with copper ions.
[0034] (3) When a powder compact obtained by press-molding the copper powder is heated from 25°C in an inert atmosphere, the temperature at which the thermal shrinkage rate reaches 1% is 230°C or less in measurement of the thermal shrinkage rate based on the thickness of the powder compact at 25°C.
[0035] (4) When the powder compact obtained by press-forming the copper powder is heated from 25°C in an inert atmosphere and in a reducing atmosphere, in the measurement of thermal shrinkage based on the thickness of the powder compact at 25°C, the temperature difference between the temperature at which the thermal shrinkage reaches 3% in the inert atmosphere and the temperature at which the thermal shrinkage reaches 3% in the reducing atmosphere is less than 10°C.
[0036] In addition, the present invention provides a method for producing copper powder, characterized in that copper oxide powder slurry is heated at a temperature below 230° C., wherein the copper oxide powder slurry is obtained by mixing copper oxide powder with a polyol solvent having a boiling point below 230° C. to which the above-mentioned chain organic matter is added.
[0037] Furthermore, the amount of the chain organic substance added is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the copper oxide powder.
[0038] The polyol solvent having a boiling point of 230° C. or less is more preferably one or more selected from the group consisting of ethylene glycol (boiling point: 196° C.), propylene glycol (boiling point: 188° C.), 1,3-propanediol (boiling point: 214° C.), 1,2-butanediol (boiling point: 194° C.), 1,3-butanediol (boiling point: 207° C.), 1,4-butanediol (boiling point: 228° C.), 1,2-pentanediol (boiling point: 210° C.), and 1,2-hexanediol (boiling point: 223° C.).
[0039] In addition, through the method of the present invention, a method for manufacturing copper powder can be provided, characterized in that the copper powder slurry is heat-treated at above 230°C, and the copper powder slurry is made by dispersing copper powder having an average particle size of less than 250nm and at least not satisfying at least any one of the above conditions (3) and conditions (4) in a polyol solvent with a boiling point of more than 250°C added with the above-mentioned chain organic matter.
[0040] The polyol solvent having a boiling point of 250° C. or higher is more preferably at least one selected from the group consisting of triethylene glycol (boiling point: 287° C.), tetraethylene glycol (boiling point: 327° C.), and polyethylene glycol having an average molecular weight of 200 to 600 (boiling point: around 300° C.).
[0041] The heat treatment temperature is preferably 230° C. or higher, more preferably 250° C. or higher, and further preferably 270° C. or higher. The amount of the chain organic substance added is preferably 0.005 mass % or higher and 10 mass % or lower relative to the total amount of copper contained in the copper powder to be heat treated.
[0042] Effects of the Invention
[0043] The copper powder of the present embodiment has an organic film that prevents the formation of an oxide film that may hinder sintering and has excellent low-temperature sintering properties.
[0044] Furthermore, according to the method for producing copper powder of the present embodiment, it is possible to obtain copper powder having an organic film that prevents the formation of an oxide film that may inhibit sintering and having excellent low-temperature sintering properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 1 and 10 are thermomechanical analysis (TMA) profiles of the copper powder prepared in Example 10 under a nitrogen atmosphere and a 2% hydrogen-98% nitrogen atmosphere.
[0046] Figure 2 It is a figure which shows the results of the gas chromatography-mass spectrometry analysis of Example 17 and Conventional Example 3. DETAILED DESCRIPTION
[0047] Hereinafter, a specific embodiment of the present invention (hereinafter referred to as "the present embodiment") is described in detail. It should be noted that the present invention is not limited to the following embodiments, and various changes can be made within the scope of not changing the gist of the present invention. In addition, in this specification, the description of "X to Y" (X, Y are arbitrary values) means "more than X and less than Y".
[0048] In the polyol method, if copper oxide powder is suspended in a polyol solvent and heated, the polyol solvent acts as a reducing agent to reduce the copper powder. When copper oxide (CuO) is used as the copper oxide powder, reduction occurs from copper oxide (CuO) to copper (Cu) via cuprous oxide (Cu2O). When cuprous oxide (Cu2O) is used as the copper oxide, cuprous oxide (Cu2O) is reduced to copper (Cu). In either case, copper powder (hereinafter sometimes referred to as "polyol copper powder") is finally obtained. After the copper powder obtained is washed with pure water or the like and filtered, it is washed again and dried as needed. Specifically, as an example of washing, a method of stirring and washing the copper powder (polyol copper powder) obtained by reduction after precipitation and decantation is used, and pure water or the like is supplied. As an example of filtration, a method of dehydrating by centrifugation or the like is used.
[0049] The copper powder in this embodiment has an average particle size of 250 nm or less, and the surface is covered with organic matter, and the surface of the copper powder is covered with both specific organic matter detected by gas chromatography mass spectrometry (GC / MS) and specific organic matter detected by liquid chromatography mass spectrometry (LC / MS). By adopting such a structure, for a pressed powder body formed by pressing the copper powder, when the thickness of the pressed powder body at 25°C is used as a reference, the temperature at which the heat shrinkage rate in an inert atmosphere becomes 1% is 230°C or less when heated at a heating rate of 10°C / min, and the low-temperature sintering property is excellent. Similarly, for a pressed powder body formed by pressing the copper powder, when the thickness of the pressed powder body at 25°C is used as a reference, the temperature difference between the temperature at which the heat shrinkage rate in an inert atmosphere becomes 3% and the temperature at which the heat shrinkage rate in a reducing atmosphere becomes 3% is less than 10°C, and an oxide film that may hinder sintering is not formed on the surface of the copper powder, or even if formed, it is so thin that it does not hinder sintering. The copper powder of the present embodiment has an organic film that prevents the formation of an oxide film that may hinder sintering and has excellent low-temperature sintering properties.
[0050] The average particle size of the copper powder is preferably less than 250nm, more preferably less than 200nm, and further preferably less than 150nm. The average particle size of the copper powder can be set to, for example, less than 110nm, less than 100nm, less than 90nm, less than 70nm, or less than 60nm as described in the examples. Such fine copper powder can be suitably used in electronic components such as electrodes of stacked ceramic capacitors. The lower limit of the average particle size of the copper powder is not particularly limited, and the lower limit can be set to about 20nm by the manufacturing method described later. It should be noted that the average particle size of the copper powder in the present embodiment is a value measured by the method described in the examples. As described in the manufacturing method section later, the average particle size of the copper powder can be controlled by the manufacturing conditions.
[0051] [Gas chromatography-mass spectrometry]
[0052] In the copper powder of the present embodiment, as the specific organic substance detected by the gas chromatography-mass spectrometry (GC / MS), at least one selected from the group consisting of the following organic substances is preferred.
[0053] H(-O-CH2-CH2) n -OH (wherein n is an integer of 1 to 4),
[0054] HOOC-CH2(-O-CH2-CH2) m -OH (wherein m is an integer of 1 to 3),
[0055] HOOC-CH2(-O-CH2-CH2) l -O-CH2-COOH (wherein l is 1 or 2),
[0056] H(-C3H6O) s -OH (wherein s is an integer of 1 to 4),
[0057] HOOC-CH(CH3)(-C3H6O) t -OH (wherein t is an integer from 1 to 3), HOOC-CH(CH3)(-C3H6O) u -O-CH(CH3)-COOH (where u is 1 or 2)
[0058] Among them, more preferred is one or more selected from the group consisting of organic substances represented by the following (Chemical 1) to (Chemical 8). These organic substances are organic substances derived from a polyol solvent.
[0059] (Chemical 1) triethylene glycol (H(-O-CH2-CH2)3-OH) (molecular weight: 150),
[0060] (Chemical 2) Tetraethylene glycol (H(-O-CH2-CH2)4-OH) (molecular weight: 194),
[0061] (Chemical 3) 2-[2-(2-hydroxyethoxy)ethoxy]acetic acid (HOOC-CH2(-O-CH2-CH2)2-OH) (molecular weight: 164),
[0062] (Chemical 4) 2-[2-[2-(2-hydroxyethoxy)ethoxy]ethoxy]acetic acid (HOOC-CH2(-O-CH2-CH2)3-OH) (molecular weight: 208),
[0063] (Chemical 5) 3,6-dioxanoic acid (HOOC-CH2-O-CH2-CH2-O-CH2-COOH) (molecular weight: 178),
[0064] (Chemical 6) 2,5,8-trioxazelaic acid (HOOC-CH2(-O-CH2-CH2)2-O-CH2-COOH) (molecular weight: 222),
[0065] (Chemical 7) tripropylene glycol (H(-C3H6O)3-OH) (molecular weight: 192, any of atactic polymer, isotactic polymer, and syndiotactic polymer),
[0066] (Chemical 8) Tetrapropylene glycol (H(-C3H6O)4-OH) (molecular weight: 250, any one of atactic polymer, isotactic polymer, and syndiotactic polymer)
[0067] GC / MS is a method for measuring organic matter by vaporizing it for detection. Therefore, it is believed that the specific organic matter detected by the above GC / MS has a relatively small molecular weight and is an organic matter that is easily vaporized. It should be noted that the method for detecting the above organic matter by GC / MS in this embodiment is the method described in the examples. The structures of the above organic matter (Chemical 1) to (Chemical 8) are shown below.
[0068]
[0069]
[0070]
[0071] [Liquid chromatography mass spectrometry analysis]
[0072] As the specific organic substance detected by liquid chromatography-mass spectrometry (LC / MS), a chain organic substance having a molecular weight of 200 to 1000 is preferred, wherein the chain organic substance has at the end of the molecule one selected from the group consisting of a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), an aldehyde group (-CHO), a nitro group (-NO2), a thiol group (-SH), a sulfone group (-SO3HHH), a phosphate group (-PO4H2), a cyano group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodo group (-I) as a functional group that can coordinate with copper ions.
[0073] Among them, a chain organic substance having a molecular weight of 200 or more and 700 or less is more preferred. In addition, the chain organic substance more preferably has a carboxyl group or a hydroxyl group at the end of the molecule, and more preferably has a carboxyl group or a hydroxyl group at both ends. Examples of such chain organic substances include (Chemical 9) sebacic acid (molecular weight: 202), (Chemical 10) dodecanedioic acid (molecular weight: 230), (Chemical 11) tetradecanedioic acid (molecular weight: 258), (Chemical 12) hexadecanedioic acid (molecular weight: 286), (Chemical 13) octadecanediic acid (molecular weight: 314), (Chemical 14) eicosanedioic acid (molecular weight: 342), (Chemical 15) poly (ethylene glycol) bis (carboxymethyl) ether (average molecular weight 250), (Chemical 16) poly (ethylene glycol) bis (carboxymethyl) ether (average molecular weight 600). If these are used, it is preferred from the perspective of being easy to purchase. The structures of the above organic substances (Chemical 9) to (Chemical 16) are shown below.
[0074]
[0075]
[0076]
[0077] The mechanism by which the copper powder in this embodiment has the low-temperature sintering property as mentioned above has not yet been clarified in detail, but it may be because: in the specific organic matter detected by the above-mentioned GC / MS and the specific organic matter detected by the above-mentioned LC / MS, the proportion of functional groups that can coordinate with copper ions in the long chain molecules is small, so even if the copper powder surface is unevenly covered with organic matter, the density of bonding on the copper powder surface through functional groups is low, and heat-induced detachment from the copper powder surface becomes easy.
[0078] It should be noted that the organic matter detected by the above GC / MS can also be detected by the above LC / MS, and the organic matter detected by the above LC / MS can also be detected by the above GC / MS.
[0079] For the copper powder in the present embodiment, when a pressed powder body is formed by press molding at 100 MPa and the heat shrinkage rate is measured based on the thickness of the pressed powder body at 25°C when heated at a heating rate of 10°C / min from 25°C in an inert atmosphere, the temperature at which the heat shrinkage rate becomes 1% is 230°C or less. The temperature at which the heat shrinkage rate of the pressed powder body becomes 1% refers to the temperature at which the copper powder begins to shrink in volume due to the sintering phenomenon, and can also be expressed as the temperature at which sintering begins. For example, as described in the examples, the temperature at which the heat shrinkage rate of the copper powder in the present embodiment becomes 1% can be 220°C or less, 215°C or less, 210°C or less, 205°C or less, 200°C or less, 195°C or less, etc.
[0080] In addition, when the copper powder in the present embodiment is pressed at 100 MPa to form a powder compact, and the heat shrinkage rate is measured based on the thickness of the above powder compact at 25°C when heated at a temperature increase rate of 10°C / min from 25°C in an inert atmosphere and a reducing atmosphere, the temperature difference between the temperature at which the heat shrinkage rate in the inert atmosphere becomes 3% and the temperature at which the heat shrinkage rate in the reducing atmosphere becomes 3% is less than 10°C. At this time, the sintering state of the roasting (heating) atmosphere does not change much between the case of the inert atmosphere and the case of the reducing atmosphere, so the restriction caused by the difficulty of sintering the copper powder in the selection of the roasting atmosphere is relaxed. In addition, the temperature at which the heat shrinkage rate of the powder compact becomes 3% refers to the temperature at which the volume shrinkage caused by the sintering phenomenon of the copper powder has progressed to a certain extent, and can be used as an indicator of the sinterability of the copper powder. By comparing the inert atmosphere and the reducing atmosphere, it is possible to infer whether there is an oxide film that hinders sintering. That is, if the temperature difference between the temperature at which the thermal shrinkage rate of the powder compact in the inert atmosphere and the temperature at which the thermal shrinkage rate of the powder compact in the reducing atmosphere reaches 3% is less than 10°C, it means that no oxide film that may hinder sintering is formed on the surface of the copper powder. For example, in the copper powder of the present embodiment, as described in the examples, the temperature difference between the temperature at which the thermal shrinkage rate in the inert atmosphere reaches 3% and the temperature at which the thermal shrinkage rate in the reducing atmosphere reaches 3% can be set to 8°C or less, 6°C or less, 5°C or less, etc.
[0081] Specifically, when the temperature at which the thermal shrinkage of the powder compact in a reducing atmosphere becomes 3% is lower by 10°C or more than the temperature at which the thermal shrinkage of the powder compact in an inert atmosphere becomes 3%, it can be considered that the surface of the copper powder subjected to the thermal shrinkage measurement is covered with a thin oxide film, and therefore the oxide film is reduced by the reducing gas and becomes easy to sinter (sintering is hindered by the oxide film in the inert atmosphere). On the other hand, when the thermal shrinkage in a reducing atmosphere is measured under the condition that there are more oxides on the surface of the copper powder subjected to the thermomechanical analysis, the amount of raw water vapor generated by the reduction becomes more, and the amount of shrinkage caused by the sintering of the copper powder also causes the amount of expansion of the powder compact based on water vapor to increase, confirming the tendency of the thermal shrinkage behavior in the thermomechanical analysis distribution diagram to shift to the high temperature side. This is equivalent to the case where the temperature at which the thermal shrinkage of the powder compact in a reducing atmosphere becomes 3% higher by 10°C or more than the temperature at which the thermal shrinkage of the powder compact in an inert atmosphere becomes 3%.
[0082] The mechanism by which the copper powder in the present embodiment has the effect of preventing the formation of an oxide film as described above has not yet been clarified in detail, but it is likely that the specific organic matter detected by the above-mentioned GC / MS and the specific organic matter detected by the above-mentioned LC / MS are a combination of organic matter with different molecular lengths, which can efficiently and unevenly cover the surface of the copper powder, and thus have a strong function as an antioxidant film.
[0083] It should be noted that the organic matter present on the surface of the copper powder of this embodiment, the organic matter detected by the GC / MS, and the organic matter detected by the LC / MS may include other organic matter, compounds, and other substances without departing from the scope of the present invention.
[0084] As described above, the copper powder of the present embodiment has an average particle size of 250 nm or less, has a surface covered with an organic substance, and satisfies all of the following conditions (1) to (4).
[0085] (1) When the organic matter present on the surface of the copper powder is detected by gas chromatography-mass spectrometry, the detection is selected from
[0086] H(-O-CH2-CH2) n -OH (wherein n is an integer of 1 to 4),
[0087] HOOC-CH2(-O-CH2-CH2) m -OH (wherein m is an integer of 1 to 3),
[0088] HOOC-CH2(-O-CH2-CH2) l -O-CH2-COOH (wherein l is 1 or 2),
[0089] H(-C3H6O) s -OH (wherein s is an integer of 1 to 4),
[0090] HOOC-CH(CH3)(-C3H6O) t -OH (wherein t is an integer of 1 to 3),
[0091] HOOC-CH(CH3)(-C3H6O) u One or more members selected from the group consisting of -O-CH(CH3)-COOH (wherein u is 1 or 2).
[0092] (2) When organic matter present on the surface of the copper powder is detected by liquid chromatography-mass spectrometry,
[0093] A chain organic substance having a molecular weight of 200 or more and 1000 or less was detected, and the chain organic substance had at the end of the molecule one selected from the group consisting of a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), an aldehyde group (-CHO), a nitro group (-NO2), a thiol group (-SH), a sulfone group (-SO3HHH), a phosphate group (-PO4H2), a cyano group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodo group (-I) as a functional group that can coordinate with copper ions.
[0094] (3) When a powder compact obtained by press-molding the copper powder is heated from 25°C in an inert atmosphere, the temperature at which the thermal shrinkage rate reaches 1% is 230°C or less in measurement of the thermal shrinkage rate based on the thickness of the powder compact at 25°C.
[0095] (4) When the powder compact obtained by press-forming the copper powder is heated from 25°C in an inert atmosphere and in a reducing atmosphere, in the measurement of thermal shrinkage based on the thickness of the powder compact at 25°C, the temperature difference between the temperature at which the thermal shrinkage reaches 3% in the inert atmosphere and the temperature at which the thermal shrinkage reaches 3% in the reducing atmosphere is less than 10°C.
[0096] The copper powder of the present embodiment may have any configuration other than the above configuration. The copper powder of the present embodiment has an organic film that prevents the formation of an oxide film that may hinder sintering and has excellent low-temperature sinterability.
[0097] Next, the method for manufacturing copper powder of the present embodiment (method for manufacturing copper powder 1, method for manufacturing copper powder 2) is described. It should be noted that in the following description, matters that have been described may sometimes be omitted or simplified. In addition, the method for manufacturing copper powder of the present embodiment may be appropriately applied to the matters described in the copper powder of the present embodiment described above. In addition, the matters described in the method for manufacturing copper powder of the present embodiment may also be appropriately applied to the copper powder of the present embodiment described above.
[0098] (Method 1 for producing copper powder)
[0099] In the method for producing copper powder in the present embodiment, copper powder is obtained by reducing copper oxide powder (raw material) in a polyol solvent having a boiling point of 230° C. or less (hereinafter, the polyol solvent having a boiling point of 230° C. or less is sometimes referred to as polyol solvent A). In the reduction step, the specific chain organic matter described above is added to the polyol solvent A in which the copper oxide powder is suspended (hereinafter, the suspension liquid formed by mixing the polyol solvent A and the copper oxide powder is sometimes referred to as reaction liquid), and the target copper powder is obtained by heating and reducing. Through the above-mentioned reduction step, the organic matter containing the above-mentioned chain organic matter can be imparted to the surface of the copper powder, thereby obtaining the copper powder of the present embodiment described above.
[0100] It should be noted that the chain-like organic substance to be added only needs to be in the form of the chain-like organic substance in the reaction solution, and the organic substance to be added may be in the form of a salt or the like.
[0101] The copper oxide powder used as a raw material in the reduction step may be either copper oxide (CuO) or cuprous oxide (Cu2O). Alternatively, the copper oxide powder may be pulverized in advance and then used in the reduction reaction.
[0102] The polyol solvent A used in the reduction step is a polyol solvent having a boiling point of 230° C. or less, and more preferably is one or more selected from the group consisting of ethylene glycol (boiling point: 196° C.), propylene glycol (boiling point: 188° C.), 1,3-propanediol (boiling point: 214° C.), 1,2-butanediol (boiling point: 194° C.), 1,3-butanediol (boiling point: 207° C.), 1,4-butanediol (boiling point: 228° C.), 1,2-pentanediol (boiling point: 210° C.), and 1,2-hexanediol (boiling point: 223° C.). In addition, the amount of the chain organic substance added to the polyol solvent A is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the copper oxide powder.
[0103] The reaction temperature of the reduction step is preferably set to be -50°C or higher relative to the boiling point of the polyol solvent A, and more preferably -40°C or higher relative to the boiling point of the polyol solvent A. In addition, the reaction temperature is preferably set to be ±0°C or lower relative to the boiling point of the polyol solvent A, and more preferably -5°C or lower relative to the boiling point of the polyol solvent A. In addition, the reaction temperature is set to be -50°C or higher relative to the boiling point of the polyol solvent A, and preferably set to be ±0°C or lower relative to the boiling point of the polyol solvent A, set to be -40°C or higher relative to the boiling point of the polyol solvent A, and more preferably set to be -5°C or lower relative to the boiling point of the polyol solvent A. When the above reaction temperature is set to a temperature lower than -50°C relative to the boiling point of the polyol solvent A, the reduction reaction will not proceed sufficiently, the copper oxide powder (raw material) will remain, and the oxygen content in the obtained copper powder (polyol copper powder) will also increase, and the reaction time will be greatly delayed, and the productivity will also deteriorate. In addition, when the above heating temperature is set to be higher than the boiling point of the polyol solvent A, there is a concern that the reduction (consumption) due to the decomposition and volatilization of the polyol solvent will become significant, and sufficient reduction may not be achieved.
[0104] In the reduction step, the copper oxide powder is heated and reduced with the polyol solvent A to which the chain organic substance is added to obtain the copper powder of the present embodiment. In the reduction reaction, heating is started after the chain organic substance is added to the reaction solution. The chain organic substance can be added to the reaction solution during the heating or after the heating.
[0105] When the aqueous solution is prepared, when the above-mentioned chain organic matter that does not become neutral (pH is about 6.5 to 7.5) is used, in order to neutralize the above-mentioned chain organic matter added to the reaction solution, it is preferred to add a base or an acid in combination as a neutralizing agent. When a base is used as the neutralizing agent, an alkali metal hydroxide is preferred, and specifically, sodium hydroxide and potassium hydroxide can be used. When an acid is used as the neutralizing agent, an inorganic acid is preferred, and specifically, sulfuric acid and hydrochloric acid can be used. When the neutralizing agent is added to the reaction solution, it can also be added to the aqueous solution in advance.
[0106] As the amount of the above-mentioned chain organic matter in the reaction solution increases, the particle size (average particle size) of the obtained copper powder also becomes finer. That is, the average particle size of the copper powder can be controlled by the amount of the chain organic matter. Furthermore, by introducing the above-mentioned chain organic matter into the organic film formed on the surface of the copper powder, the sintering property can be improved. The amount of the above-mentioned chain organic matter in the reaction solution is set according to conditions such as the particle size of the copper powder obtained after the reduction reaction. The amount of the above-mentioned chain organic matter in the reaction solution can be set by preliminary experiments. The amount of the above-mentioned chain organic matter in the reaction solution is preferably 10% by mass or less relative to the total amount of copper contained in the copper oxide of the raw material. In addition, the amount of the above-mentioned chain organic matter in the reaction solution (the amount of the above-mentioned chain organic matter added in the polyol solvent A) is preferably 0.005% by mass or more relative to the total amount of copper contained in the copper oxide of the raw material. In addition, the amount of the above-mentioned chain organic matter in the reaction solution is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the copper oxide of the raw material. The addition of the above-mentioned chain organic matter in an amount of less than 0.005 mass % relative to the total amount of copper contained in the copper oxide of the raw material may not be conducive to fully exerting the particle size control effect and the sinterability improvement effect. In addition, the effect of the addition of the above-mentioned chain organic matter decreases with the increase of the addition amount, so the addition of the above-mentioned chain organic matter in an amount of more than 10 mass % relative to the total amount of copper contained in the copper oxide of the raw material will increase the production cost, and is therefore uneconomical. In addition, the amount of the above-mentioned chain organic matter in the reaction liquid (relative to the total amount of copper contained in the copper oxide of the raw material, the amount of the above-mentioned chain organic matter added in the polyol solvent A is preferably 0.001 mol% or more, for example, it can be 0.01 mol% or more, and it can be 0.1 mol% or more. In addition, relative to the total amount of copper contained in the copper oxide of the raw material, the amount of the above-mentioned chain organic matter in the reaction liquid is preferably 1 mol% or less. In addition, relative to the total amount of copper contained in the copper oxide of the raw material, the amount of the above-mentioned chain organic matter in the reaction liquid is preferably 0.001 mol% or more and 1 mol or less, it can be 0.01 mol% or more and 1 mol% or more, and it can be 0.1 mol% or more and 1 mol% or less.
[0107] The average particle size of the copper powder obtained by the method 1 for manufacturing copper powder of the present embodiment is preferably less than 250nm. By using the above-mentioned chain organic matter during the reduction reaction, the copper powder (polyol copper powder) obtained by the manufacturing method described above can be controlled to be less than the above-mentioned average particle size. Since it is a fine copper powder, it can be used for electronic components such as electrodes of stacked ceramic capacitors. For example, by the method 1 for manufacturing copper powder, copper powders with an average particle size of less than 200nm, less than 150nm, less than 110nm, less than 100nm, less than 90nm, less than 70nm, and less than 60nm as described in the embodiments can be obtained.
[0108] As described above, the method 1 for manufacturing copper powder of the present embodiment is characterized in that the copper oxide powder slurry is heated at a temperature below 230°C, wherein the copper oxide powder slurry is obtained by mixing copper oxide powder with a polyol solvent having a boiling point below 230°C to which the above-mentioned chain organic matter is added. The method 1 for manufacturing copper powder of the present embodiment is a method for manufacturing the copper powder of the present embodiment. It should be noted that in the method 1 for manufacturing copper powder of the present embodiment, the configuration other than the above-mentioned configuration may be any configuration. By the method 1 for manufacturing copper powder of the present embodiment, a copper powder having an organic coating that prevents the formation of an oxide coating that may hinder sintering and having excellent low-temperature sintering properties can be obtained. It should be noted that in the method 1 for manufacturing copper powder of the present embodiment, substances other than the above-mentioned configuration may be added to the reaction solution without departing from the main purpose of the present invention.
[0109] (Method 2 for producing copper powder)
[0110] The method for producing copper powder of another embodiment of the present invention comprises: a copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) of the copper powder of the present embodiment described above is dispersed in a polyol solvent having a boiling point of 250° C. or more (hereinafter, the polyol solvent having a boiling point of 250° C. or more is also referred to as polyol solvent B) to which the chain organic matter is added (hereinafter, the suspension liquid formed by mixing the polyol solvent B and the copper powder is also collectively referred to as "treatment liquid"), and heated to obtain the target copper powder. The heat treatment step can modify the organic matter on the surface of the copper powder, and the modification includes imparting the added chain organic matter to the surface of the copper powder. Thus, the copper powder of the present embodiment described above can be obtained. For example, by the method for producing copper powder 2, copper powder having an average particle size of 200 nm or less, 150 nm or less, 110 nm or less, 100 nm or less, 90 nm or less, 70 nm or less, or 60 nm or less can be obtained as described in the examples.
[0111] It should be noted that the copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) of the copper powder in the present embodiment mentioned above refers to, for example, copper powder produced by the method for producing copper powder described in Japanese Patent Application Laid-Open No. 2022-128445. Obviously, it is not limited to this, and as long as it is a copper powder that does not satisfy at least one of the conditions (3) and (4) of the copper powder in the present embodiment mentioned above, it may also be a copper powder produced by other wet methods or gas phases.
[0112] The polyol solvent B used in the heat treatment step is more preferably selected from the group consisting of polyols having a boiling point of 250°C or more, triethylene glycol (boiling point: 287°C), tetraethylene glycol (boiling point: 327°C) and polyethylene glycol having an average molecular weight of 200 or more and 600 or less (boiling point: around 300°C). In addition, the amount of the chain organic matter added is preferably 10% by mass or less relative to the total amount of copper contained in the treated copper powder. In addition, the amount of the chain organic matter added is preferably 0.005% by mass or more relative to the total amount of copper contained in the treated copper powder. In addition, the amount of the chain organic matter added is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the treated copper powder.
[0113] The heat treatment temperature of the heat treatment step is preferably 230°C or higher. The heat treatment temperature can be set, for example, to the conditions described in the examples, and can be set to 240°C or higher, 250°C or higher, 260°C or higher, or 270°C or higher. In addition, the heat treatment temperature is preferably ±0°C or lower relative to the boiling point of the polyol solvent B, and more preferably -5°C or lower relative to the boiling point of the polyol solvent B. In addition, the heat treatment temperature is preferably 230°C or higher and ±0°C or lower relative to the boiling point of the polyol solvent B, more preferably 250°C or higher and -5°C or lower relative to the boiling point of the polyol solvent B, and further preferably 270°C or higher and -5°C or lower relative to the boiling point of the polyol solvent B. When the heat treatment temperature is set to less than 230°C, the replacement of organic matter on the surface of the copper powder cannot be fully carried out, and the intended organic film cannot be formed, so that excellent oxidation resistance and low temperature sintering properties cannot be imparted to the copper powder. If the heat treatment temperature is set higher than the boiling point of the polyol solvent B, the polyol solvent may be significantly reduced (consumed) by decomposition and volatilization, and the heat treatment may not be performed sufficiently. The heat treatment time is preferably within 1 hour, more preferably within 30 minutes, and further preferably within 15 minutes.
[0114] In the heating treatment step, the copper powder that does not satisfy at least one of the conditions (3) and (4) of the copper powder in the present embodiment is heated in the polyol solvent B to which the chain organic substance is added, thereby obtaining the copper powder in the present embodiment. In the heating treatment step, the heating is started after the chain organic substance is added to the treatment liquid. The chain organic substance may be added to the reaction liquid during the heating.
[0115] When the above-mentioned chain organic matter that does not become neutral (about pH 6.5 to 7.5) when made into an aqueous solution is used, in order to neutralize the above-mentioned chain organic matter added to the treatment solution, it is preferred to add a base or an acid in combination as a neutralizing agent. When a base is used as a neutralizing agent, an alkali metal hydroxide is preferred, and specifically, sodium hydroxide and potassium hydroxide can be used. When an acid is used as a neutralizing agent, an inorganic acid is preferred, and specifically, sulfuric acid and hydrochloric acid can be used. When adding a neutralizing agent to the reaction solution, it can also be added to the aqueous solution in advance.
[0116] The above-mentioned chain organic matter in the treatment liquid also acts as an anti-connection agent for the copper powder. The amount of the above-mentioned chain organic matter in the treatment liquid can be set according to conditions such as the particle size of the copper powder to be treated. The amount of the above-mentioned chain organic matter in the treatment liquid can be set by preliminary experiments. The amount of the above-mentioned chain organic matter in the treatment liquid is preferably 10% by mass or less relative to the total amount of copper contained in the treated copper powder. In addition. The amount of the above-mentioned chain organic matter in the treatment liquid (the amount of the above-mentioned chain organic matter added in the polyol solvent B) is preferably 0.005% by mass or more relative to the total amount of copper contained in the treated copper powder. In addition, the amount of the above-mentioned chain organic matter in the treatment liquid is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the treated copper powder. When the above-mentioned chain organic matter is added in an amount less than 0.005% by mass relative to the total amount of copper contained in the treated copper powder, the effect of the copper powder as an anti-connection agent cannot be fully exerted. In addition, the effect of adding the above-mentioned chain organic matter decreases as the amount of addition increases. Therefore, when more than 10% by mass of the above-mentioned chain organic matter is added relative to the total amount of copper contained in the treated copper powder, the production cost will increase, so it is not economical. In addition, relative to the total amount of copper contained in the treated copper powder, the amount of the above-mentioned chain organic matter in the treatment solution (the amount of the above-mentioned chain organic matter added in the polyol solvent B) is preferably 0.001 mol% or more, for example, it can be 0.01 mol% or more, or it can be 0.1 mol% or more. In addition, relative to the total amount of copper contained in the treated copper powder, the amount of the above-mentioned chain organic matter in the treatment solution is preferably 1 mol% or less. In addition, relative to the total amount of copper contained in the treated copper powder, the amount of the above-mentioned chain organic matter in the treatment solution is preferably 0.001 mol% or more and 1 mol or less, it can be 0.01 mol% or more and 1 mol% or more.
[0117] As described above, the copper powder manufacturing method 2 of the present embodiment is the following copper powder manufacturing method:
[0118] It is characterized in that the copper powder slurry is heated at a temperature above 230°C, wherein the copper powder slurry is obtained by mixing a copper powder having an average particle size of less than 250nm and not satisfying at least one of the conditions (3) and (4) described in the copper powder of the present embodiment, with a polyol solvent having a boiling point of more than 250°C to which the above-mentioned chain organic matter is added. The method 2 for manufacturing the copper powder of the present embodiment is a method for manufacturing the copper powder of the present embodiment. It should be noted that in the method 2 for manufacturing the copper powder of the present embodiment, in addition to the above-mentioned structure, any structure may be used. By the method 2 for manufacturing the copper powder of the present embodiment, a copper powder having an organic film that prevents the formation of an oxide film that may hinder sintering and having excellent low-temperature sintering properties can be obtained. It should be noted that in the method 2 for manufacturing the copper powder of the present embodiment, substances other than the above-mentioned substances may be added to the reaction solution without departing from the scope of the present invention.
[0119] Example
[0120] Hereinafter, the embodiments and comparative examples of the present invention are shown together and further described in detail, but the present invention is not limited to the following embodiments. Here, in the following description, the polyol solvent used in the reduction process is the first polyol solvent, and the polyol solvent used in the heat treatment process is the second polyol solvent. It should be noted that the determination method of the physical property values is as follows.
[0121] (1) Average particle size
[0122] The average particle size of the obtained copper powder (polyol copper powder) was determined by analyzing an image of 200 or more particles observed with a SEM (scanning electron microscope) to obtain a number average particle size.
[0123] (2) Analysis of organic matter on the surface of copper powder
[0124] Regarding the organic components on the surface of the copper powder, 10 mg of the copper powder was immersed in 70 μl of a 1 wt% tetramethylammonium hydroxide-methanol solution to extract the organic matter on the surface. The powder was dried at 50°C for 10 minutes, and then the organic components were vaporized at 300°C for 30 seconds in a pyrolysis furnace (PY-3030D manufactured by Frontier Laboratories). The organic components were detected in the range of m / z=33 to 550 using GC / MS (GC unit: GC-2010PLus, MS unit: QP-2010ULtra manufactured by Shimadzu Corporation).
[0125] <Gas chromatography conditions>
[0126] Column: UltraALLOY+-5 made by Frontier Laboratories 30M × inner diameter 0.25mm
[0127] Carrier gas: Helium
[0128] Temperature program: 50~350℃, 10℃ / min
[0129] Injection method: split (split ratio 20:1)
[0130] Inlet temperature: 300℃
[0131] At the same time, 0.5 g of copper powder was immersed in 10 ml of 0.5 N sodium hydroxide aqueous solution, and the organic matter on the surface was extracted and centrifuged to obtain the supernatant as an evaluation sample, which was detected by LC / MS (LC part: AGILEnt 1290 Infinity 2, MS part: Agilent 6530, manufactured by Agilent Technologies, Inc.). Based on the data obtained above, qualitative analysis of the organic components was performed.
[0132] <Liquid chromatography conditions>
[0133] Column: Waters ACQUITY UPLC BEH C18 1.7 μM × 150 mm
[0134] Column temperature: 40°C
[0135] Flow rate: 0.2ml / min
[0136] Injection volume: 5μl
[0137] Eluent: Pure water / acetonitrile mixture: 0 to 22.5 minutes...99.5 / 0.5, 22.51 to 30 minutes...0 / 100, 30.01 to 35 minutes...99.5 / 0.5
[0138] <Mass spectrometry analysis conditions (for LC)>
[0139] Polarity: Positive
[0140] Determination mass range: m / z = 70 ~ 1700
[0141] Ionization method: ESI
[0142] Gas temperature, flow rate: 280℃, 12L / min
[0143] Atomizer pressure: 55psi
[0144] Sheath gas temperature and flow rate: 350℃, 12L / min
[0145] Fragmentation voltage: 100V
[0146] Scanning speed: 3spec / sec
[0147] (3) Determination of thermal shrinkage behavior (TMA)
[0148] The thermal shrinkage behavior of the obtained copper powder was measured using a thermomechanical analysis (TMA) (TMA4000SA, manufactured by BRUKER Corporation). About 0.3 g of copper powder was weighed and filled into a mold with a cylindrical hole with an inner diameter of 5 mm. A load of 100 MPa was applied for 1 minute using a pressing machine to form a powder compact with a diameter of 5 mm and a height of 2 mm to 4 mm. The shrinkage rate of the powder compact in the thickness (height) direction when heated from 25°C was measured under the following conditions, and the temperature at which the thermal shrinkage rate became 1% and the temperature at which it became 3% based on the thickness of the powder compact at 25°C were determined.
[0149] Heating rate: 10℃ / min
[0150] Temperature range: room temperature ~ 800℃
[0151] Applied load: 98mN
[0152] Atmosphere: pure nitrogen (inactive atmosphere) or 2 volume %-H2 + 98 volume %-N2 (reducing atmosphere)
[0153] (Example 1)
[0154] [Reduction process]
[0155] 3.6 g of cuprous oxide (Cu2O) powder (manufactured by Chemet Co., Ltd., product number: Ultrafine) as copper oxide powder was placed in a 50 ml tall beaker, 13.5 g of propylene glycol (abbreviated as PG, boiling point: 188°C, molecular weight 76) as the first polyol solvent was added, 0.302 g of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (abbreviated as PEG600 dibasic acid, manufactured by Sigma-Aldrich Co., Ltd.) (9.44 mass % (1 mol %) relative to the total amount of copper in the cuprous oxide) and 162 μl of a 25 mass volume % sodium hydroxide aqueous solution for neutralization were added, and mixed to form a uniform slurry. The slurry was heated to 185°C and maintained at the temperature while stirring for 45 minutes to perform a reduction reaction. After the reaction solution was cooled, the generated polyol copper powder was centrifuged, washed, and dried.
[0156] (Example 2)
[0157] A polyol copper powder was obtained in the same manner as in Example 1 except that the first polyol solvent was replaced with 1,3-propylene glycol (abbreviation: 1,3-PDO, boiling point: 214° C., molecular weight 76).
[0158] (Example 3)
[0159] A polyol copper powder was obtained in the same manner as in Example 1 except that the first polyol solvent was replaced with 1,2-butanediol (abbreviation: 1,2-BDO, boiling point: 194° C., molecular weight 90).
[0160] (Example 4)
[0161] A polyol copper powder was obtained in the same manner as in Example 1 except that the first polyol solvent was replaced with 1,3-butanediol (abbreviation: 1,3-BDO, boiling point: 207° C., molecular weight 90).
[0162] (Example 5)
[0163] Polyol copper powder was obtained in the same manner as in Example 3 except that the amount of PEG600 dibasic acid added was 0.0302 g (0.94 mass % (0.1 mol %) relative to the total amount of copper in cuprous oxide) and 16 μl of a 25 mass volume % sodium hydroxide aqueous solution was added for neutralization.
[0164] (Example 6)
[0165] Polyol copper powder was obtained in the same manner as in Example 3 except that the amount of PEG600 dibasic acid added was 0.0030 g (the amount of oxygen relative to the total amount of copper in cuprous oxide was 0.094 mass % (0.01 mol %)) and 16 μl of a 25 mass volume % sodium hydroxide aqueous solution was added for neutralization.
[0166] (Example 7)
[0167] Polyol copper powder was obtained in the same manner as in Example 3 except that the amount of PEG600 dibasic acid added was 0.0003 g (0.0094 mass % (0.001 mol %) relative to the total amount of copper in cuprous oxide) and 16 μl of a 25 mass volume % sodium hydroxide aqueous solution was added for neutralization.
[0168] (Example 8)
[0169] [Reduction process]
[0170] Copper powder was prepared according to the method of Example 5 described in Japanese Patent Application Laid-Open No. 2022-128445. Specifically, 27 g of cuprous oxide powder as copper oxide powder was placed in a 200 ml detachable flask, and 100 g of ethylene glycol (abbreviated as: EG, boiling point: 197°C, molecular weight 62) as the first polyol solvent was added, followed by 0.65 g of cis-1,2-cyclohexanedicarboxylic acid (2.71 mass % (1 mol %) relative to the total amount of copper in cuprous oxide) and 1.21 ml of a 25 mass volume % sodium hydroxide aqueous solution for neutralization, and mixed in a uniform slurry. The slurry was heated to 190°C and maintained at the temperature while stirring for 45 minutes to perform a reduction reaction. After cooling the reaction solution, the generated polyol copper powder was centrifuged, washed, and dried.
[0171] [Heat treatment process]
[0172] 3.2 g of copper powder was classified from the product obtained by centrifuging the generated polyol copper powder and redispersed in 13.5 g of tetraethylene glycol (abbreviated as TeEG, boiling point: 327° C., molecular weight 194) as the second polyol solvent. Then, 0.302 g of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) (9.44 mass % (1 mol %) relative to the total amount of copper in the treated copper) and 162 μl of a 25 mass volume % sodium hydroxide aqueous solution for neutralization were added and mixed in a uniform slurry. The slurry was heated to 280° C. and maintained at the temperature while stirring for 10 minutes to perform a heat treatment. After the reaction solution was cooled, the generated heat-treated polyol copper powder was centrifuged, washed, and dried.
[0173] (Example 9)
[0174] A heat-treated polyol copper powder was obtained in the same manner as in Example 8 except that the temperature of the reduction reaction was changed to 180°C.
[0175] (Example 10)
[0176] [Reduction process]
[0177] Copper powder was prepared according to the method of Example 24 described in Japanese Patent Application Laid-Open No. 2022-128445. Specifically, 27 g of cuprous oxide powder as copper oxide powder was placed in a 200 ml detachable flask, 100 g of propylene glycol (abbreviated as: PG, boiling point: 188°C, molecular weight 76) as the first polyol solvent was added, and 0.65 g of cis-1,2-cyclohexanedicarboxylic acid (2.71 mass % (1 mol %) relative to the total amount of copper in cuprous oxide) and 1.21 ml of 25 mass volume % sodium hydroxide aqueous solution for neutralization were added and mixed in a uniform slurry. The slurry was heated to 185°C and maintained at the temperature while stirring for 45 minutes to perform a reduction reaction. After cooling the reaction solution, the generated polyol copper powder was centrifuged, washed, and dried.
[0178] [Heat treatment process]
[0179] 3.2 g of copper powder was classified from the product obtained by centrifuging the generated polyol copper powder and redispersed in 13.5 g of tetraethylene glycol as the second polyol solvent. Then, 0.302 g of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) (9.44 mass % (1 mol %) relative to the total amount of copper in the treated copper) and 162 μl of a 25 mass volume % sodium hydroxide aqueous solution for neutralization were added and mixed in a uniform slurry. The slurry was heated to 280° C. and maintained at the temperature for 10 minutes while stirring to perform a heat treatment. After the reaction solution was cooled, the generated heat-treated polyol copper powder was centrifuged, washed, and dried.
[0180] (Example 11)
[0181] In the heat treatment step, the addition amount of PEG600 dibasic acid was set to 0.0302 g (0.94 mass % (0.1 mol %) relative to the total amount of copper in the treated copper) and 16 μl of a 25 mass volume % sodium hydroxide aqueous solution was added for neutralization. Polyol copper powder was obtained in the same manner as in Example 10.
[0182] (Example 12)
[0183] In the heat treatment step, the addition amount of PEG600 dibasic acid was set to 0.0030 g (0.094 mass % (0.01 mol %) relative to the total amount of copper in the treated copper) and 16 μl of a 25 mass volume % sodium hydroxide aqueous solution was added for neutralization. Polyol copper powder was obtained in the same manner as in Example 10.
[0184] (Example 13)
[0185] In the heat treatment step, the addition amount of PEG600 dibasic acid was set to 0.0003 g (0.0094 mass % (0.001 mol %) relative to the total amount of copper in the treated copper) and 16 μl of a 25 mass volume % sodium hydroxide aqueous solution was added for neutralization. Polyol copper powder was obtained in the same manner as in Example 10.
[0186] (Example 14)
[0187] In the heat treatment step, the heating temperature of the slurry was set to 260° C., and the same procedure as in Example 10 was carried out to obtain a heat-treated polyol copper powder.
[0188] (Example 15)
[0189] In the heat treatment step, the heating temperature of the slurry was set to 240° C., and the same procedure as in Example 10 was carried out to obtain a heat-treated polyol copper powder.
[0190] (Example 16)
[0191] In the heat treatment step, the heating temperature of the slurry was set to 230° C., and the same procedure as in Example 10 was carried out to obtain a heat-treated polyol copper powder.
[0192] (Example 17)
[0193] In the heat treatment step, the same operation as in Example 10 was carried out except that 0.1724 g of eicosanedioic acid (5.39 mass % (1 mol %) relative to the total amount of copper in the treated copper) was added instead of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) to obtain a heat-treated polyol copper powder.
[0194] (Example 18)
[0195] In the heat treatment step, the same operation as in Example 10 was carried out except that 0.1018 g of sebacic acid (3.18 mass % (1 mol %) relative to the total amount of copper in the treated copper) was added instead of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) to obtain a heat-treated polyol copper powder.
[0196] (Example 19)
[0197] In the heat treatment step, the same operation as in Example 10 was carried out except that 0.1159 g of dodecanedioic acid (3.63 mass % (1 mol %) relative to the total amount of copper in the treated copper) was added instead of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) to obtain a heat-treated polyol copper powder.
[0198] (Comparative Example 1)
[0199] [Reduction process]
[0200] 30 g of copper oxide (CuO) powder (manufactured by Furukawa Chemical Co., Ltd., product number: FCO-M6) as copper oxide powder was placed in a 200 ml separable flask, and 100 g of tetraethylene glycol as the first polyol solvent was added and mixed in a uniform slurry. The slurry was heated to 300° C. and maintained at the temperature for 45 minutes while stirring to perform a reduction reaction. After the reaction solution was cooled, the generated polyol copper powder was centrifuged, washed, and dried.
[0201] (Comparative Example 2)
[0202] In the reduction step, the same operation as in Example 2 was carried out except that PEG600 dibasic acid and a 25 mass volume % sodium hydroxide aqueous solution for neutralization were not added to obtain a polyol copper powder.
[0203] (Comparative Example 3)
[0204] In the reduction step, the same operation as in Example 3 was carried out except that PEG600 dibasic acid and a 25 mass volume % sodium hydroxide aqueous solution for neutralization were not added to obtain a polyol copper powder.
[0205] (Comparative Example 4)
[0206] In the reduction step, the same operation as in Example 4 was carried out except that PEG600 dibasic acid and a 25 mass volume % sodium hydroxide aqueous solution for neutralization were not added to obtain a polyol copper powder.
[0207] (Existing Example 1)
[0208] [Reduction process]
[0209] Copper powder was prepared by the method of Example 5 described in Japanese Patent Application Laid-Open No. 2022-128445. After the reaction solution was cooled, the generated polyol copper powder was centrifuged, washed, and dried. Unlike Example 8, the polyol copper powder was not subjected to heat treatment.
[0210] (Existing Example 2)
[0211] A polyol copper powder was obtained in the same manner as in Conventional Example 1 except that the temperature of the reduction reaction was changed to 180° C. Unlike Example 9, this polyol copper powder was not subjected to a heat treatment.
[0212] (Existing Example 3)
[0213] [Reduction process]
[0214] Copper powder was prepared by the method of Example 24 described in Japanese Patent Application Laid-Open No. 2022-128445. After the reaction solution was cooled, the generated polyol copper powder was centrifuged, washed, and dried. Unlike Examples 10 to 19, this polyol copper powder was not subjected to heat treatment.
[0215] (Comparative Example 5)
[0216] In the heat treatment step, the heating temperature of the slurry was set to 200° C., and the same procedure as in Example 10 was carried out to obtain a heat-treated polyol copper powder.
[0217] (Comparative Example 6)
[0218] In the heat treatment step, the same operation as in Example 10 was carried out except that PEG600 dibasic acid and 25 mass volume % sodium hydroxide aqueous solution were not added to obtain a polyol copper powder.
[0219] Table 1 shows the production conditions of Examples 1 to 19, Comparative Examples 1 to 6, and Conventional Examples 1 to 3 described above.
[0220] [Table 1]
[0221]
[0222] (Evaluation result)
[0223] For the polyol copper powder obtained in Examples 1 to 19, Comparative Examples 1 to 6 and Existing Examples 1 to 3, the average particle size, the detection of surface organic matter of the copper powder based on GC / MS and LC / MS, the temperature at which the thermal shrinkage of the compressed powder of the polyol copper powder obtained in an inert atmosphere measured by TMA becomes 1% (hereinafter, also referred to as TMA1%), and the temperature difference (absolute value) between the temperature at which the thermal shrinkage of the compressed powder in an inert atmosphere becomes 3% (hereinafter, also referred to as TMA3%) and the temperature at which the thermal shrinkage of the compressed powder in a reducing atmosphere becomes 3% are determined according to the above method. These results are shown in Table 2. It should be noted that in Table 2, "not detected" means below the detection limit. In addition, the results of GC / MS in Example 17 and Existing Example 3 are shown in Table 2. Figure 2 .
[0224] [Table 2]
[0225]
[0226] In all the examples, organic substances satisfying the above conditions (1) and (2) were detected by GC / MS and LC / MS. In addition, in all the examples, the temperature at which TMA 1% was reached in the inert atmosphere was below 230°C, and the temperature difference at which TMA 3% was reached in the inert atmosphere and in the reducing atmosphere was less than 10°C. For example, as shown in the temperature-TMA distribution diagram in Example 10 ( Figure 1 ) shows that the sintering (thermal shrinkage) behavior in an inert atmosphere and a reducing atmosphere is almost unchanged, indicating that an oxide film that hinders sintering is formed on the surface of the copper powder, or the oxide film is so thin that it does not hinder sintering.
[0227] On the other hand, in the comparative examples and the prior art examples, no organic matter satisfying both the above-mentioned conditions (1) and (2) was detected by GC / MS and LC / MS. In addition, in the prior art examples 1 to 3, the temperature at which TMA 1% was reached in the inert atmosphere was greater than 230°C, and in the comparative examples and the prior art examples, the temperature difference at which TMA 3% was reached in the inert atmosphere and in the reducing atmosphere was greater than 10°C.
[0228] Regarding Comparative Example 1, although the surface of the copper powder is covered with organic matter that can be detected by GC / MS and satisfies the above-mentioned condition (1), there is no organic matter that can be detected by LC / MS and satisfies the above-mentioned condition (2). Therefore, it is believed that compared with Examples 1 to 4, the surface coverage of the organic matter is insufficient, and an oxide film that hinders sintering is easily formed on the surface of the copper powder. Therefore, it is believed that the sinterability under an inert atmosphere is deteriorated, which is different from the sintering state under a reducing atmosphere. (The above-mentioned condition (4) is not satisfied.)
[0229] Regarding Comparative Examples 2 to 5 and Existing Examples 1 to 3, the organic matter detected by GC / MS is not an organic matter that satisfies the above-mentioned condition (1), so it is believed that the organic matter on the surface of the copper powder hinders sintering and does not satisfy the above-mentioned condition (3). In addition, there is no organic matter on the surface of the copper powder that can be detected by LC / MS and satisfies the above-mentioned condition (2), so it is believed that an oxide film that hinders sintering is easily formed on the surface of the copper powder, and the sintering property under an inert atmosphere is deteriorated, resulting in a difference from the sintering state under a reducing atmosphere. (The above-mentioned condition (4) is not satisfied.)
[0230] In Comparative Example 6, the copper powders treated during the heat treatment aggregated to form large agglomerates, so the subsequent analysis was recorded as unmeasurable. This is believed to be because the chain organic substance that functions as an anti-linking agent for the copper powder was not added.
[0231] Examples 8 to 19 are examples in which existing Examples 1 to 3 are subjected to heat treatment, respectively. It is therefore believed that organic matter satisfying the above-mentioned conditions (1) and (2) detected by GC / MS and LC / MS is reconstructed on the surface of the copper powder by heat treatment, and as a result, copper powder satisfying the above-mentioned conditions (3) and (4) can be obtained.
[0232] According to the embodiments, comparative examples, and conventional examples, it can be confirmed that: the average particle size of the copper powder in the present embodiment is less than 250nm, and the surface is covered with both specific organic matter detected by GC / MS and specific organic matter detected by LC / MS. When the above copper powder is heated at a temperature increase rate of 10°C / min from 25°C in an inert atmosphere to obtain a powder compact, in the measurement of the thermal shrinkage based on the thickness of the above powder compact at 25°C, the temperature at which the thermal shrinkage becomes 1% is less than 230°C; when the above copper powder is heated at a temperature increase rate of 10°C / min from 25°C in an inert atmosphere and in a reducing atmosphere to obtain a powder compact, in the measurement of the thermal shrinkage based on the thickness of the above powder compact at 25°C, the temperature difference between the temperature at which the thermal shrinkage becomes 3% in the inert atmosphere and the temperature at which the thermal shrinkage becomes 3% in the reducing atmosphere is less than 10°C.
[0233] It should be noted that the technical scope of the present invention is not limited to the methods described in the above-mentioned embodiments, etc. Sometimes one or more of the conditions described in the above-mentioned embodiments, etc. can be omitted. In addition, the conditions described in the above-mentioned embodiments, etc. can be appropriately combined. In addition, within the scope permitted by laws and regulations, the disclosure contents of all documents cited in Japanese Patent Application No. 2022-030202 and the above-mentioned embodiments, etc. are cited as part of the description herein.
[0234] The embodiments of the present invention include the following configurations. [1]
[0236] A copper powder having an average particle size of 250 nm or less, a surface covered with an organic substance, and satisfying all of the following conditions (1) to (4).
[0237] Condition (1) When the organic matter present on the surface of the copper powder is detected by gas chromatography-mass spectrometry, a selected organic compound is detected.
[0238] H(-O-CH2-CH2) n -OH (wherein n is an integer from 1 to 4),
[0239] HOOC-CH2(-O-CH2-CH2) m -OH (wherein m is an integer from 1 to 3), HOOC-CH2 (-O-CH2-CH2) l-O-CH2-COOH (wherein l is 1 or 2),
[0240] H(-C3H6O) s -OH (wherein s is an integer from 1 to 4),
[0241] HOOC-CH(CH3)(-C3H6O) t -OH (wherein t is an integer from 1 to 3), HOOC-CH(CH3)(-C3H6O) u One or more members selected from the group consisting of -O-CH(CH3)-COOH (wherein u is 1 or 2).
[0242] Condition (2) When organic matter present on the surface of the copper powder is detected by liquid chromatography-mass spectrometry,
[0243] Chain organic matter with a molecular weight of more than 200 and less than 1000 was detected, and the chain organic matter had at the end of the molecule one selected from the group consisting of a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), an aldehyde group (-CHO), a nitro group (-NO2), a thiol group (-SH), a sulfone group (-SO3HHH), a phosphate group (-PO4H2), a cyano group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodo group (-I), which are functional groups that can coordinate with copper ions.
[0244] Condition (3): When a powder compact obtained by press-forming the copper powder is heated from 25°C in an inert atmosphere, the temperature at which the thermal shrinkage rate reaches 1% is 230°C or less in measurement of the thermal shrinkage rate based on the thickness of the powder compact at 25°C.
[0245] Condition (4): When the powder compact obtained by press-forming the copper powder is heated from 25°C in an inert atmosphere and in a reducing atmosphere, in the measurement of thermal shrinkage based on the thickness of the powder compact at 25°C, the temperature difference between the temperature at which the thermal shrinkage reaches 3% in the inert atmosphere and the temperature at which the thermal shrinkage reaches 3% in the reducing atmosphere is less than 10°C.
[0246] [2] The copper powder according to [1], wherein the average particle size is 200 nm or less.
[0247] [3] The copper powder according to [1] or [2], wherein the average particle size is 150 nm or less.
[0248] [4] A method for producing copper powder according to any one of [1] to [3], characterized in that:
[0249] The copper oxide powder slurry is heated at 230° C. or less. The copper oxide powder slurry is obtained by mixing the copper oxide powder with a polyol solvent having a boiling point of 230° C. or less to which the chain organic substance is added.
[0250] [5] The method for producing copper powder according to [4], wherein the amount of the chain organic matter added is 0.005 mass % or more and 10 mass % or less relative to the total amount of copper contained in the copper oxide powder.
[0251] [6] The method for producing copper powder according to [4] or [5], characterized in that the polyol solvent having a boiling point of 230°C or less is one or more selected from the group consisting of ethylene glycol (boiling point: 196°C), propylene glycol (boiling point: 188°C), 1,3-propanediol (boiling point: 214°C), 1,2-butanediol (boiling point: 194°C), 1,3-butanediol (boiling point: 207°C), 1,4-butanediol (boiling point: 228°C), 1,2-pentanediol (boiling point: 210°C), and 1,2-hexanediol (boiling point: 223°C).
[0252] [7] A method for producing copper powder according to any one of [1] to [3], characterized in that:
[0253] The copper powder slurry is heated at 230°C or above, wherein the copper powder slurry is obtained by mixing a copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) described in [1] with a polyol solvent having a boiling point of 250°C or above to which the chain organic substance is added.
[0254] [8] The method for producing copper powder according to [7], characterized in that the amount of the chain organic matter added is 0.005 mass % or more and 10 mass % or less relative to the total amount of copper contained in the copper powder to be heat treated.
[0255] [9] The method for producing copper powder according to [7] or [8], characterized in that the polyol solvent having a boiling point of 250°C or higher is one or more selected from the group consisting of triethylene glycol (boiling point: 287°C), tetraethylene glycol (boiling point: 327°C) and polyethylene glycol having an average molecular weight of 200 to 600 (boiling point: around 300°C).
[0256]
[10] The method for producing copper powder according to any one of [7] to [9], wherein the temperature of the heat treatment is 250° C. or higher.
[0257]
[11] The method for producing copper powder according to any one of [7] to
[10] , wherein the temperature of the heat treatment is 270° C. or higher.
Claims
1. A copper powder having an average particle size of 250 nm or less, a surface covered with an organic substance, and satisfying all of the following conditions (1) to (4): (1) When organic matter present on the surface of the copper powder is detected by gas chromatography-mass spectrometry, Detected by H(-O-CH2-CH2) n -OH (wherein, n is an integer of 1 to 4), HOOC-CH2(-O-CH2-CH2) m -OH (wherein m is an integer from 1 to 3), HOOC-CH2(-O-CH2-CH2) l -O-CH2-COOH (wherein l is 1 or 2), H(-C3H6O) s -OH (wherein s is an integer from 1 to 4), HOOC-CH(CH3)(-C3H6O) t -OH (wherein t is an integer from 1 to 3), HOOC-CH(CH3)(-C3H6O) u -O-CH(CH3)-COOH (wherein u is 1 or 2) or more; (2) When the organic matter present on the surface of the copper powder is detected by liquid chromatography-mass spectrometry, A chain organic substance having a molecular weight of 200 or more and 1000 or less is detected, wherein the chain organic substance has at the end of the molecule one selected from the group consisting of a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), an aldehyde group (-CHO), a nitro group (-NO2), a thiol group (-SH), a sulfone group (-SO3HHH), a phosphate group (-PO4H2), a cyano group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodo group (-I) as a functional group that can coordinate with copper ions; (3) when a powder compact obtained by press-forming the copper powder is heated from 25° C. in an inert atmosphere, the temperature at which the thermal shrinkage rate reaches 1% is 230° C. or less in a measurement of the thermal shrinkage rate based on the thickness of the powder compact at 25° C.; (4) When the powder compact obtained by press-forming the copper powder is heated from 25°C in an inert atmosphere and in a reducing atmosphere, in the measurement of thermal shrinkage based on the thickness of the powder compact at 25°C, the temperature difference between the temperature at which the thermal shrinkage in the inert atmosphere becomes 3% and the temperature at which the thermal shrinkage in the reducing atmosphere becomes 3% is less than 10°C.
2. The copper powder according to claim 1, characterized in that The average particle size is 200 nm or less.
3. The copper powder according to claim 1 or claim 2, characterized in that: The average particle size is 150 nm or less.
4. A method for producing copper powder according to any one of claims 1 to 3, characterized in that: The copper oxide powder slurry is heated at 230° C. or less. The copper oxide powder slurry is obtained by mixing the copper oxide powder with a polyol solvent having a boiling point of 230° C. or less to which the chain organic matter is added.
5. The method for producing copper powder according to claim 4, characterized in that: The amount of the chain organic substance added is 0.005 mass % or more and 10 mass % or less relative to the total amount of copper contained in the copper oxide powder.
6. The method for producing copper powder according to claim 4 or claim 5, characterized in that: The polyol solvent having a boiling point of 230°C or less is at least one selected from the group consisting of ethylene glycol (boiling point: 196°C), propylene glycol (boiling point: 188°C), 1,3-propanediol (boiling point: 214°C), 1,2-butanediol (boiling point: 194°C), 1,3-butanediol (boiling point: 207°C), 1,4-butanediol (boiling point: 228°C), 1,2-pentanediol (boiling point: 210°C), and 1,2-hexanediol (boiling point: 223°C).
7. A method for producing copper powder according to any one of claims 1 to 3, characterized in that: The copper powder slurry is heated at a temperature above 230°C, wherein the copper powder slurry is obtained by mixing a copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) described in claim 1 with a polyol solvent having a boiling point of 250°C or above to which the chain organic matter is added.
8. The method for producing copper powder according to claim 7, characterized in that: The amount of the chain organic substance added is 0.005 mass % or more and 10 mass % or less relative to the total amount of copper contained in the copper powder to be heat treated.
9. The method for producing copper powder according to claim 7 or claim 8, characterized in that: The polyol solvent having a boiling point of 250° C. or higher is one or more selected from the group consisting of triethylene glycol (boiling point: 287° C.), tetraethylene glycol (boiling point: 327° C.), and polyethylene glycol having an average molecular weight of 200 to 600 (boiling point: approximately 300° C.).
10. The method for producing copper powder according to any one of claims 7 to 9, characterized in that: The temperature of the heat treatment is 250° C. or higher.
11. The method for producing copper powder according to any one of claims 7 to 10, characterized in that: The temperature of the heat treatment is 270° C. or higher.
Citation Information
Patent Citations
Method for manufacturing copper particulate and copper particulate dispersion liquid
JP2005097677A
Coated copper particle
JP2016176146A
Production method of copper powder
JP2022128445A
Low-temperature-sinterable copper particle and method for manufacturing sintered compact using same
WO2019106739A1