High-toughness polyester heat shrinkage film
By adding toughening resin and opening slip agent to the heat-shrinkable polyester film and adopting a multi-directional stretching process, the problem of heat-shrinkable film being easily broken under normal temperature and humidity and high temperature and high humidity conditions is solved, and high toughness is achieved and uniform performance polyester heat shrink film.
Patent Information
- Application Number
- CN202411261616.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
AI Technical Summary
The existing heat-shrinkable polyester films are prone to suddenly decrease in the elongation rate of break along the MD direction under normal temperature and humidity conditions, showing brittleness problems, resulting in uneven performance and easy breakage.
A high-tough polyester heat shrink film was used to achieve a shrinkage of ≥40% in transverse direction and -1% to 20% in longitudinal direction after 10 seconds of treatment at 90°C, and 85-98.9% polyester was added to the formula. Raw materials, 0.1-5% opening slip agent and 1-10% toughening resin were carried out in one-way or multi-directional stretching process, combined with cold setting and corona treatment, and made a film with high toughness.
Under normal temperature and humidity and high temperature and high humidity conditions, the longitudinal elongation of break is significantly improved, avoiding the sudden decrease in the elongation of break along the MD direction, showing good toughness and unprone fracture performance.
Abstract
Description
Technical Field
[0001] The invention relates to a high-toughness polyester heat shrinkable film, belonging to the field of heat shrinkable films. Background Art
[0002] Heat shrink film refers to a special material that has a certain shrinkage ability when heated at a predetermined temperature. Heat shrink film is mainly used for identification (labels) and cluster packaging of new products such as beverages, detergents, electronic products, industrial products and fast food. It has the characteristics of bright gloss and close-fitting packaging, and can redefine beverage brands when used. Its gloss and shrinkage can make the packaging pattern on bottled beverages more vivid. The use of shrink film can achieve 360° label design, highlighting the image on supermarket shelves.
[0003] Since heat-shrinkable polyester film requires a larger shrinkage rate in the transverse direction, the heat-shrinkable polyester film production lines at home and abroad currently all adopt a unidirectional stretching process, that is, generally only transverse stretching is adopted, including preheating, stretching, heat setting and cooling areas. Since only unidirectional stretching is performed, or a very small stretching ratio in the longitudinal direction, the performance of the product in the unstretched direction is difficult to be effectively controlled, which will lead to uneven shrinkage in the unstretched direction. Moreover, at room temperature, especially after being placed under high temperature and high humidity for a period of time, the shrink film will suddenly decrease its elongation at break along the MD direction, and even appear in single digits, which shows that it is very easy to break and brittle.
[0004] Since heat-shrinkable polyester film requires a larger transverse shrinkage rate, the heat-shrinkable polyester film production lines at home and abroad currently all adopt a unidirectional stretching process, that is, generally only transverse stretching is adopted, or a very small stretching ratio in the longitudinal direction. The performance of the product in the direction of ineffective stretching is difficult to effectively control, and the shrink film shows a sudden decrease in the elongation at break along the MD direction, and even single digits, which makes it very easy to break and brittle. The reason is that the polyester resin undergoes slow crystallization under certain temperature and humidity conditions. Summary of the invention
[0005] According to the background problem, the problem to be solved by the present invention is:
[0006] (1) After being placed at room temperature and humidity (temperature ≤ 30°C, humidity ≤ 60%) for a period of time, the shrink film shows a sudden decrease in elongation at break along the MD direction.
[0007] (2) In order to achieve an appropriate shrinkage range, especially a lower shrinkage rate, it is necessary to increase the heat shrinkage process temperature and place it at room temperature and humidity for a shorter time, or even just after production, the shrink film will have a sudden decrease in the elongation at break along the MD direction.
[0008] (3) In summer storage and transportation, after being placed at high temperature and high humidity (temperature 40°C, humidity 85%) for a period of time, the elongation at break of the shrink film along the MD direction suddenly decreases.
[0009] (4) The polyester heat shrinkable film can be directly or after pattern printing, and then wrapped on the surface of the container at 60-150°C or left for a period of time, and the elongation at break of the shrinkable film along the MD direction will suddenly decrease.
[0010] To achieve the above object, the present invention provides the following technical solutions:
[0011] A high-toughness polyester heat-shrinkable film, wherein the heat-shrinkable polyester film is treated at 90°C for 10 seconds, has a shrinkage rate of ≥40% in the transverse direction (TD), a shrinkage rate of -1% to 20% in the longitudinal direction (MD), and
[0012] a) When the shrinkage rate in the transverse direction is 40-70%, after being placed at room temperature and humidity (temperature ≤ 30°C, humidity ≤ 60%) for 12 months, the longitudinal elongation at break is ≥ 250%, and after being placed at high temperature and humidity (temperature 40°C, humidity 85%) for 4 days (including 4 days), the longitudinal elongation at break is ≥ 250%;
[0013] b) When the shrinkage rate in the transverse direction is ≥70%, after being placed at room temperature and humidity (temperature ≤30°C, humidity ≤60%) for 24 months, the longitudinal elongation at break is ≥250%, and after being placed at high temperature and humidity (temperature 40°C, humidity 85%) for 14 days (including 14 days), the longitudinal elongation at break is ≥250%;
[0014] The formula of the heat shrinkable polyester film is as follows: the mass percentage of polyester raw material is 85-98.9%, the mass percentage of opening lubricant is 0.1-5%, and the mass percentage of toughening resin is 1-10%;
[0015] The normal temperature and humidity conditions are: temperature ≤30°C, humidity ≤60%; the high temperature and high humidity conditions are: temperature 40°C, humidity 85%;
[0016] The modified polyethylene terephthalate is prepared by copolymerizing terephthalic acid (TPA) and ethylene glycol (EG) with at least one dibasic acid or diol as a copolymer component; the content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the dibasic acid as the copolymer component is 0 to 50%; the content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the diol as the copolymer component is 10 to 50%.
[0017] The toughening resin is polyolefin elastomer POE grafted with glycidyl methacrylate, or polyolefin elastomer POE grafted with maleic anhydride, wherein the grafting rate is 1-8%;
[0018] Preferably, the high-toughness polyester heat shrinkable film may have a single-layer structure or a multi-layer structure of two or more layers. When having a structure of two or more layers, the polyester heat shrinkable film may be divided into a polyester core layer or a polyester surface layer, wherein the thickness of the polyester surface layer is 5-20% of the total thickness.
[0019] Preferably, the opening lubricant is a mixture of one or more of silicon dioxide, mica powder, alumina, kaolin and paraffin, wherein the particle size of silicon dioxide is ≤4 um.
[0020] Preferably, the preparation method of the high-toughness polyester heat shrinkable film is:
[0021] (1) Batching: Various polyester raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.
[0022] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.
[0023] (3) Unstretched sheet: After preheating at 10-50°C above the softening point, the film is stretched 1.0-1.5 times in the longitudinal direction and 5.0-5.5 times in the transverse direction. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.
[0024] Preferably, the high-toughness polyester heat shrinkable film has a thickness of 20-100 μm.
[0025] Preferably, the intrinsic viscosity of the modified polyethylene terephthalate is 0.6 to 1.2 dl / g.
[0026] After adding the toughening resin, a good compatibility process is achieved with the polar polyester resin through the grafted polar technology of glycidyl methacrylate or maleic anhydride, and a polyolefin elastomer may be produced, which has good toughness itself, further reducing the crystallization ability of the polyester resin, and producing irregular entanglement of the molecular chains in the direction of ineffective stretching, thereby achieving a period of significantly improving the elongation at break of the shrink film along the MD direction, and achieving high-toughness product performance.
[0027] High-toughness polyester heat shrinkable film can be directly or after pattern printing, shrink sleeve label at 60-150℃, and can be heated by steam, hot air, infrared heating and other forms.
[0028] As a choice of the above-mentioned high-toughness polyester heat shrinkable film, various additives can be added as needed, such as waxes, antioxidants, antistatic agents, nucleating agents, viscosity reducers, tackifiers, chain extenders, heat stabilizers, coloring pigments, anti-coloring agents, anti-ultraviolet absorbers, etc. It is worth noting that the raw material formulas with the above-mentioned additives should all be within the innovative concept of the present invention and belong to the protection scope of the present invention.
[0029] The beneficial effects of the present invention are:
[0030] (1) When placed at room temperature and humidity, or at high temperature and high humidity, the shrink film will not experience a sudden decrease in elongation at break along the MD direction, and it is not easy to break and has good toughness.
[0031] (2) The longitudinal elongation at break is higher when placed at room temperature and humidity, and higher when placed at high temperature and high humidity.
[0032] (3) High-toughness polyester heat shrinkable film can be directly or after pattern printing, and then shrink the sleeve at 60-150℃. The heating method can be steam, hot air, infrared heating, etc. DETAILED DESCRIPTION
[0033] Example 1
[0034] A high-toughness polyester heat shrinkable film, the formula (mass percentage) is:
[0035] The mass percentage of ester raw materials is 85%
[0036] The mass percentage of the opening lubricant is 0.5%
[0037] The mass percentage of toughening resin is 9.5%;
[0038] in,
[0039] The content of the copolymer component of the modified polyethylene terephthalate is as follows: the molar percentage of the diol neopentyl glycol NPG as the copolymer component is 28%, and the molar percentage of the diethylene glycol DEG is 6%.
[0040] The toughening resin is polyolefin elastomer POE grafted with glycidyl methacrylate, with a grafting rate of 2%.
[0041] The opening lubricant is silicon dioxide, wherein the particle size of the silicon dioxide is 4 um.
[0042] The preparation method is:
[0043] (1) Batching: Various polyester raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.
[0044] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.
[0045] (3) Unstretched sheet: After preheating at 25°C above the softening point, the film is stretched 1.0 times in the longitudinal direction and 5.2 times in the transverse direction. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.
[0046] The high-toughness polyester heat shrinkable film has a thickness of 30 μm.
[0047] Example 2
[0048] A high-toughness polyester heat shrinkable film, the formula (mass percentage) is:
[0049] The mass percentage of ester raw materials is 93%
[0050] The mass percentage of the opening lubricant is 2%
[0051] The mass percentage of toughening resin is 5%;
[0052] in,
[0053] The content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the dibasic acid isophthalic acid IPA as the copolymer component is 5%;
[0054] The content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the diol neopentyl glycol NPG as the copolymer component is 17%, and the molar percentage of the diethylene glycol DEG is 6%.
[0055] The toughening resin is polyolefin elastomer POE grafted with glycidyl methacrylate, with a grafting rate of 4%.
[0056] The opening lubricant is silicon dioxide, wherein the particle size of the silicon dioxide is 3 um.
[0057] The preparation method is:
[0058] (1) Batching: Various polyester raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.
[0059] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.
[0060] (3) Unstretched sheet: After preheating at 15°C above the softening point, the film is stretched 1.05 times in the longitudinal direction and 5.5 times in the transverse direction. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.
[0061] The high-toughness polyester heat shrinkable film has a thickness of 40 μm.
[0062] Example 3
[0063] A high-toughness polyester heat shrinkable film, the formula (mass percentage) is:
[0064] The mass percentage of ester raw materials is 94%
[0065] The mass percentage of the opening lubricant is 5%
[0066] The mass percentage of toughening resin is 1%;
[0067] in,
[0068] The content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the diol 1,4-cyclohexanedimethanol (CHDM) as the copolymer component is 30%.
[0069] The toughening resin is polyolefin elastomer POE grafted with maleic anhydride, wherein the grafting rate is 8%;
[0070] The opening lubricant is silicon dioxide, wherein the particle size of the silicon dioxide is 1 um.
[0071] The preparation method is:
[0072] (1) Batching: Various polyester raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.
[0073] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.
[0074] (3) Unstretched sheet: After preheating at 28°C above the softening point, the film is stretched 1.1 times in the longitudinal direction and 5.0 times in the transverse direction. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.
[0075] The high-toughness polyester heat shrinkable film has a thickness of 45 μm.
[0076] Comparative Example 1
[0077] A high-toughness polyester heat shrinkable film, the formula (mass percentage) is:
[0078] The mass percentage of ester raw materials is 95.5%
[0079] The mass percentage of the opening lubricant is 0.5%
[0080] in,
[0081] The content of the copolymer component of the modified polyethylene terephthalate is as follows: the molar percentage of the diol neopentyl glycol NPG as the copolymer component is 28%, and the molar percentage of the diethylene glycol DEG is 6%.
[0082] The opening lubricant is silicon dioxide, wherein the particle size of the silicon dioxide is 4 um.
[0083] The preparation method is:
[0084] (1) Batching: Various polyester raw materials are measured according to the raw material ratio and then enter the inlet of each extruder.
[0085] (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet.
[0086] (3) Unstretched sheet: After preheating at 25°C above the softening point, the film is stretched 1.0 times in the longitudinal direction and 5.2 times in the transverse direction. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.
[0087] The high-toughness polyester heat shrinkable film has a thickness of 30 μm.
[0088] project unit Example 1 Example 2 Example 3 Comparative Example 1 Measured thickness um 30.8 40.1 44.5 30.5 Longitudinal tensile strength MPa 52 58 75 51 Transverse tensile strength MPa 239 224 218 223 Longitudinal elongation at break % 529 485 404 5 Transverse elongation at break % 45 38 35 41 90℃ / 10s longitudinal shrinkage % 2.1 8.9 10.5 1.3 90℃ / 10s Transverse shrinkage % 78.1 63.8 58.2 57.5 Haze % 4.5 4.8 4.1 4.3 Light transmittance % 88.5 88.9 88.7 89.2 Glossiness (45°) % 88 87 97 92 Friction coefficient μS / μK 0.51 / 0.44 0.58 / 0.33 0.40 / 0.35 0.55 / 0.39 Surface tension mN / m ≥38 ≥38 ≥38 ≥38
[0089] Table 1 Performance test table of embodiments and comparative examples
[0090] project unit Example 1 Example 2 Example 3 Comparative Example 1 Longitudinal elongation at break (1 month) % 529 482 398 5 Longitudinal elongation at break (2 months) % 521 465 375 4 Longitudinal elongation at break (3 months) % 505 440 368 5 Longitudinal elongation at break (4 months) % 498 435 354 6 Longitudinal elongation at break (May) % 475 416 342 4 Longitudinal elongation at break (6 months) % 462 382 338 5 Longitudinal elongation at break (July) % 451 375 331 4 Longitudinal elongation at break (August) % 432 367 315 4 Longitudinal elongation at break (September) % 429 342 308 5 Longitudinal elongation at break (October) % 425 325 292 5 Longitudinal elongation at break (November) % 410 305 287 5 Longitudinal elongation at break (December) % 403 282 265 4 Longitudinal elongation at break (14 months) % 395 235 243 4 Longitudinal elongation at break (16 months) % 390 221 230 4 Longitudinal elongation at break (18 months) % 387 208 215 5 Longitudinal elongation at break (20 months) % 375 192 198 3 Longitudinal elongation at break (22 months) % 355 185 189 5 Longitudinal elongation at break (24 months) % 348 170 182 3
[0091] Table 2 Longitudinal elongation at break after placing at room temperature and humidity (temperature ≤ 30°C, humidity ≤ 60%)
[0092] project unit Example 1 Example 2 Example 3 Comparative Example 1 Longitudinal elongation at break (1 day) % 520 485 392 4 Longitudinal elongation at break (2 days) % 515 460 370 4 Longitudinal elongation at break (3 days) % 509 443 366 4 Longitudinal elongation at break (4 days) % 495 432 355 5 Longitudinal elongation at break (5 days) % 480 4 5 4 Longitudinal elongation at break (6 days) % 469 4 3 3 Longitudinal elongation at break (7 days) % 455 3 5 4 Longitudinal elongation at break (8 days) % 432 4 3 3 Longitudinal elongation at break (9 days) % 428 2 4 5 Longitudinal elongation at break (10 days) % 420 3 4 2 Longitudinal elongation at break (11 days) % 416 5 5 5 Longitudinal elongation at break (12 days) % 435 2 4 3 Longitudinal elongation at break (14 days) % 427 5 4 4 Longitudinal elongation at break (16 days) % 4 4 5 4 Longitudinal elongation at break (18 days) % 5 4 3 4
[0093] Table 3 Longitudinal elongation at break after high temperature and high humidity (temperature 40°C, humidity 85%)
[0094] According to the above table, when the present invention is placed at room temperature and humidity, or at high temperature and humidity, the shrink film does not suddenly decrease in elongation at break along the MD direction, and is not easy to break and has good toughness. When placed at room temperature and humidity, or at high temperature and humidity, the longitudinal elongation at break is higher. The present invention has good performance and is a polyester heat shrink film with excellent longitudinal elongation at break and good performance.
Claims
1. A high-toughness polyester heat shrinkable film, characterized in that: The heat-shrinkable polyester film is treated at 90° C. for 10 seconds, and has a shrinkage rate of ≥40% in the transverse direction and a shrinkage rate of -1% to 20% in the longitudinal direction. When the shrinkage rate in the transverse direction is 40-70%, after being placed at room temperature and humidity for 12 months, the longitudinal elongation at break is ≥250%, and after being placed at high temperature and humidity for 4 days (including 4 days), the longitudinal elongation at break is ≥250%; when the shrinkage rate in the transverse direction is ≥70%, after being placed at room temperature and humidity for 24 months, the longitudinal elongation at break is ≥250%, and after being placed at high temperature and humidity for 14 days (including 14 days), the longitudinal elongation at break is ≥250%; The normal temperature and humidity conditions are: temperature ≤30°C, humidity ≤60%; the high temperature and high humidity conditions are: temperature 40°C, humidity 85%; The formula of the heat shrinkable polyester film is as follows: the mass percentage of polyester raw material is 85-98.9%, the mass percentage of opening lubricant is 0.1-5%, and the mass percentage of toughening resin is 1-10%; The modified polyethylene terephthalate is prepared by copolymerizing terephthalic acid (TPA) and ethylene glycol (EG) with at least one dibasic acid or diol as a copolymer component; the content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the dibasic acid as the copolymer component is 0 to 50%; the content of the copolymer component of the modified polyethylene terephthalate, wherein the molar percentage of the diol as the copolymer component is 10 to 50%. The toughening resin is polyolefin elastomer POE grafted with glycidyl methacrylate, or polyolefin elastomer POE grafted with maleic anhydride, wherein the grafting rate is 1-8%.
2. A high-toughness polyester heat shrinkable film according to claim 1, characterized in that: The high-toughness polyester heat shrinkable film may have a single-layer structure or a multi-layer structure with two or more layers. When the polyester heat shrinkable film has a structure with more than two layers, the polyester heat shrinkable film may be divided into a polyester core layer or a polyester surface layer, wherein the thickness of the polyester surface layer is 5-20% of the total thickness.
3. The high-toughness polyester heat shrinkable film according to claim 1, characterized in that: The opening lubricant is a mixture of one or more of silicon dioxide, mica powder, aluminum oxide, kaolin and paraffin, wherein the particle size of silicon dioxide is ≤4 um.
4. The high-toughness polyester heat shrinkable film according to claim 1, characterized in that: The preparation method of the high-toughness polyester heat shrinkable film is: (1) Batching: Various polyester raw materials are measured according to the raw material ratio and then enter the inlet of each extruder. (2) Extruded sheet: The melt extruded by the extruder enters the die through respective filters, metering pumps, etc. to extrude the melt into a sheet, and then cools on the casting roll to form an unstretched sheet. (3) Unstretched sheet: After preheating at 10-50°C above the softening point, the film is stretched 1.0-1.5 times in the longitudinal direction and 5.0-5.5 times in the transverse direction. The stretched film is cold-set and then pulled and rolled or corona treated to obtain a semi-finished film.
5. The high-toughness polyester heat shrinkable film according to claim 1, characterized in that: The high-toughness polyester heat shrinkable film has a thickness of 20-200 μm.
6. A high-toughness polyester heat shrinkable film according to claim 5, characterized in that: The high-toughness polyester heat shrinkable film has a thickness of 30-60 μm.
7. The high-toughness polyester heat shrinkable film according to claim 1, characterized in that: The intrinsic viscosity of the modified polyethylene terephthalate is 0.6 to 1.2 dl / g.
Citation Information
Cited By
Low-temperature high-shrinkage polyester heat shrinkage film capable of replacing PVC label and preparation method of low-temperature high-shrinkage polyester heat shrinkage film
CN120271982A
A polyester heat shrinkable film with low temperature and high shrinkage that can replace PVC labels and its preparation method
CN120271982B