Electrolytic capacitor

By designing the filling structure of the porous body containing valve metal and the solid electrolyte layer in the electrolytic capacitor, the problem of ESR increase of the electrolytic capacitor in high temperature environment is solved, and the low ESR effect of low cost and high capacity is achieved.

CN118805232APending Publication Date: 2024-10-18PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380024941.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-09
Filing Date
2023-03-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The ESR (equivalent series resistance) of existing electrolytic capacitors increases in high-temperature environments, and the effect of reducing ESR is insufficient.

Method used

Design an electrolytic capacitor whose anode body has a porous body containing valve metal and a covering dielectric layer. The solid electrolyte layer is filled in the pores of the porous body, and the filling rate decreases from the outer surface toward the center to meet a specific distance. relation( 0.1D ≤ X < 0.7D, 0.05D ≤ X < 0.3D or 0.03D ≤

Benefits of technology

It achieves low ESR in low-frequency and high-frequency areas, reduces the cost and ESR of electrolytic capacitors, and increases capacitance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118805232A_ABST
    Figure CN118805232A_ABST
Patent Text Reader

Abstract

An electrolytic capacitor is provided with a positive electrode body having a porous body containing a valve action metal and a dielectric layer covering the porous body, and a solid electrolyte layer that is filled in pores of the porous body and covers the dielectric layer. The filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface toward the center of the porous body. The shortest distance D from the outer surface to the center of the porous body and the distance X50 from the outer surface of the porous body when the filling rate R of the solid electrolyte layer reaches 50% satisfy a specific relationship. In other words, when the CV value of the porous body is less than 100000 [mu] F.V / g, the relationship 0.1 D < = X50 < 0.7 D is satisfied. When the CV value of the porous body is 100,000 [mu] F * V / g or more and less than 15,000 [mu] F * V / g, the relationship 0.05 D < = X50 < 0.3D is satisfied. When the CV value of the porous body is 15000 [mu] F.V / g or more, the relationship 0.03 D < = X50 < 0.2 D is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an electrolytic capacitor. Background Art

[0002] In recent years, electrolytic capacitors with low equivalent series resistance (ESR) and excellent frequency characteristics have been developed. The electrolytic capacitor includes a porous body containing a valve metal, a dielectric layer covering the porous body, and a solid electrolyte layer filling the pores of the porous body and covering the dielectric layer.

[0003] Patent Document 1 proposes a solid electrolytic capacitor in which the thickness of the conductive polymer compound layer in the center of the capacitor element is at least 0.02 μm or more and 0.14 μm or less. In addition, Patent Document 1 proposes that the difference between the thickness of the conductive polymer compound layer in the center of the capacitor element and the thickness of the conductive polymer compound layer near the outer surface of the capacitor element be within 0.08 μm for the above-mentioned solid electrolytic capacitor.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 11-87177 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In recent years, the reduction of the ESR of electrolytic capacitors has been sought. In the electrolytic capacitor described in Patent Document 1, although the increase of the ESR in a high temperature environment can be suppressed, the reduction of the ESR of the electrolytic capacitor is still insufficient.

[0009] Means for solving problems

[0010] One scheme of the present disclosure relates to an electrolytic capacitor, which includes an anode body and a solid electrolyte layer, wherein the anode body has a porous body containing a valve-acting metal and a dielectric layer covering the porous body, the solid electrolyte layer is filled in the pores of the porous body and covers the dielectric layer, wherein the CV value of the porous body is lower than 100000 μF·V / g, the filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface of the porous body toward the center, and the shortest distance D from the outer surface of the porous body to the center and the distance X from the outer surface of the porous body when the filling rate R of the solid electrolyte layer reaches 50% satisfy the relationship of 0.1D≤X<0.7D.

[0011] Another scheme of the present disclosure relates to an electrolytic capacitor, which includes an anode body and a solid electrolyte layer, wherein the anode body has a porous body containing a valve metal and a dielectric layer covering the porous body, the solid electrolyte layer is filled in the pores of the porous body and covers the dielectric layer, wherein the CV value of the porous body is greater than or equal to 100,000 μF·V / g and less than 150,000 μF·V / g, the filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface of the porous body toward the center, and the shortest distance D from the outer surface of the porous body to the center and the distance X from the outer surface of the porous body when the filling rate R of the solid electrolyte layer reaches 50% satisfy the relationship of 0.05D≤X<0.3D.

[0012] Another embodiment of the present disclosure relates to an electrolytic capacitor comprising an anode body and a solid electrolyte layer, wherein the anode body has a porous body containing a valve metal and a dielectric layer covering the porous body, the solid electrolyte layer is filled in the pores of the porous body and covers the dielectric layer, wherein the CV value of the porous body is greater than or equal to 150,000 μF·V / g, the filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface of the porous body toward the center, and the shortest distance D from the outer surface of the porous body to the center and the distance X from the outer surface of the porous body when the filling rate R of the solid electrolyte layer reaches 50% satisfy the relationship of 0.03D≤X<0.2D.

[0013] Effects of the Invention

[0014] According to the present disclosure, it is possible to provide an electrolytic capacitor with a low ESR.

[0015] The novel features of the present invention are described in the appended claims, but the present invention both in terms of configuration and content will be more clearly understood from the following detailed description taken in conjunction with other objects and features of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a cross-sectional view schematically showing an electrolytic capacitor according to one embodiment of the present disclosure.

[0017] Figure 2 It is a cross-sectional view schematically showing an anode body having a solid electrolyte layer formed on the surface.

[0018] Figure 3 This is a cross-sectional view schematically showing an example of a porous body.

[0019] Figure 4 is along Figure 3 A cross-sectional view taken along line IV-IV. DETAILED DESCRIPTION

[0020] Hereinafter, the embodiments of the present disclosure will be described as examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​or materials are sometimes exemplified, but other numerical values ​​or materials, etc. may also be applied as long as the effects of the present disclosure can be obtained. In this specification, a description such as "numerical value A to numerical value B" includes numerical value A and numerical value B, which can be replaced by "above numerical value A and below numerical value B". In the following description, when the lower limit and upper limit of numerical values ​​related to specific physical properties and conditions are exemplified, as long as the lower limit is not above the upper limit, any of the exemplified lower limits can be arbitrarily combined with any of the exemplified upper limits. When multiple materials are exemplified, one of them can be selected and used alone, or two or more can be used in combination.

[0021] The electrolytic capacitor has an anode body and a solid electrolyte layer, wherein the anode body has a porous body containing a valve metal and a dielectric layer covering the porous body, and the solid electrolyte layer is filled in the pores of the porous body and covers the dielectric layer. Hereinafter, the anode body and the solid electrolyte layer (or the anode body, the solid electrolyte layer and the cathode layer described later) are collectively referred to as a "capacitor element". The filling rate R of the solid electrolyte layer in the porous body generally decreases from the outer surface of the porous body toward the center. In other words, the filling rate R decreases as the distance X from the outer surface of the porous body increases.

[0022] The present inventors investigated the relationship between the filling rate R and the ESR in the depth direction of a porous body and obtained the following findings.

[0023] The influence of the filling rate R on the surface side of the porous body on the ESR varies with the CV value of the porous body. The larger the CV value, the smaller the influence of the filling rate R in the deep part of the porous body on the ESR, and the larger the influence of the filling rate R on the surface of the porous body on the ESR. In addition, the higher the measurement frequency, the smaller the influence of the filling rate R in the deep part of the porous body on the ESR, and the larger the influence of the filling rate R on the surface.

[0024] In addition, when the polymerization reaction rate is reduced to slowly form the solid electrolyte layer, especially when electrolytic polymerization suitable for precisely controlling the polymerization rate is performed, the filling rate R can be increased from the surface of the porous body toward the deep part, and the polymerization time is prolonged. If the polymerization time is prolonged, the polymerization solution is deteriorated due to the formation of oligomers, etc., and the conductivity of the formed solid electrolyte is reduced, thereby increasing the ESR.

[0025] The inventors of the present invention have conducted intensive research based on the obtained insights. As a result, it was found that when the shortest distance D from the outer surface to the center of the porous body and the distance X 50When the following relationship (i), (ii) or (iii) is satisfied, the solid electrolyte layer can be effectively filled into the pores of the porous body, and the ESR can be reduced in both the low frequency region and the high frequency region. 50 , is the distance X from the outer surface of the porous body when the filling rate R of the solid electrolyte layer is 50%.

[0026] (i) When the CV value of the porous body is less than 100000 μF·V / g, 0.1D≤X 50 <0.7D

[0027] (ii) When the CV value of the porous body is 100000 μF·V / g or more and less than 150000 μF·V / g, 0.05D≤X 50 <0.3D

[0028] (iii) When the CV value of the porous body is 150000 μF·V / g or more, 0.03D≤X 50 <0.2D

[0029] Hereinafter, the distance X from the outer surface of the porous body is also referred to as X 50 The following region (region where the filling rate R is 50% or more) is referred to as the "first region". 50 The region (region where the filling rate R is lower than 50%) is referred to as the “second region”.

[0030] When the CV value is high, the filling rate R in the deep part of the porous body has a small influence on the ESR, and the tendency of the ESR increase can be easily suppressed even when the first region is small. By appropriately forming the first region according to the CV value, the formation time of the solid electrolyte layer containing the conductive polymer is shortened, and the decrease in the conductivity of the solid electrolyte layer caused by the increase in the formation time can be suppressed. Therefore, a low ESR and high-capacity electrolytic capacitor can be realized at a low cost.

[0031] Compared with the case where the measurement frequency is low (e.g., 100 kHz), when the measurement frequency is high (e.g., 500 kHz), the filling rate R in the deep part of the porous body has a small influence on the ESR, and the ESR is difficult to increase even when the first region is small. Therefore, by shortening the formation time of the solid electrolyte layer, it is easy to obtain the effect of suppressing the increase in ESR and the high cost caused by long-term formation.

[0032] When (i) X 50 When X is 0.1D or more, the first region can be appropriately formed, and a conductive path based on the solid electrolyte layer can be effectively formed, thereby significantly reducing ESR. 50When it is 0.05D or more and X in (iii) 50 When the value is 0.03D or more, the ESR is also greatly reduced.

[0033] When (i) X 50 When it is less than 0.7D, the polymerization time for forming the solid electrolyte layer can be shortened, the degradation of the polymerization solution caused by the increase of the polymerization time can be suppressed, and the decrease in the conductivity of the solid electrolyte caused by the degradation of the polymerization solution and the increase in ESR caused by it can be suppressed. 50 When it is less than 0.3D and (iii) X 50 When it is less than 0.2D, the increase of ESR is also suppressed in the same manner.

[0034] In the above (i), the CV value of the porous body may be greater than 70000 μF·V / g and less than 100000 μF·V / g. In this case, the filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.1D may be greater than 50% and less than 80%. In this case, the filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.7D may be greater than 16% and less than 48%.

[0035] In the above (ii), the filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.05D may be 50% or more and 83% or less. In this case, the filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.3D may be more than 13% and 44% or less.

[0036] In the above (iii), the filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.03D may also be 56% or more and 83% or less. In this case, the filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.2D may also be 14% or more and 41% or less. In the above (iii), the CV value may be, for example, 150000μF·V / g or more and 350000μF·V / g or less, or 150000μF·V / g or more and 200000μF·V / g or less.

[0037] From the viewpoint of facilitating the formation time of the solid electrolyte layer and facilitating the lowering of the ESR, when the CV value of the porous body is less than 100000 μF·V / g, the distance X 50 It may be 0.1D or more and 0.69D or less, 0.1D or more and less than 0.5D or 0.1D or more and less than 0.4D. From the same point of view, when the CV value of the porous body is 100000 μF·V / g or more and less than 150000 μF·V / g, the distance X50 It may be 0.05D or more and 0.29D or less, or 0.05D or more and less than 0.2D. From the same viewpoint, when the CV value of the porous body is 150000 μF·V / g or more, the distance X 50 It may be greater than or equal to 0.03D and less than or equal to 0.19D, or may be greater than or equal to 0.03D and less than 0.1D.

[0038] The filling rate R (%) of the solid electrolyte layer refers to the filling rate of one area (for example, an area of ​​5 μm) of the cross section (a cross section in the longitudinal direction including the shortest distance D) of the anode body observed by an electron microscope. 2 ~30μm 2 The area occupied by the voids in the region refers to the value obtained by subtracting the area occupied by the anode body (the total of the porous body and the dielectric layer) in the region from the area of ​​the entire region. As an electron microscope, a scanning electron microscope (SEM) or a transmission electron microscope (TEM) can be used. The filling rate R of the solid electrolyte layer at a distance X from the outer surface of the porous body refers to the filling rate R in a region where the depth of the distance X is located near the center.

[0039] The filling rate R (%) of the solid electrolyte layer can be obtained by the following method.

[0040] The electrolytic capacitor is disassembled and the capacitor element is subjected to argon ion cross-section polishing (CP) to obtain a sample cross section (anode cross section). The sample cross section is observed by SEM or TEM to obtain an image (e.g., magnification: 20,000 to 40,000 times) showing a region of the cross section (hereinafter referred to as the measurement region). Using this image, the area S0 of the entire measurement region (e.g., 5 μm 2 ~30μm 2 ), the area S1 occupied by the anode body (the total of the porous body and the dielectric layer) in the measurement area, and the area S2 occupied by the solid electrolyte layer in the measurement area.

[0041] The filling rate (%) is calculated by the following formula using S0, S1 and S2 calculated as described above: The value obtained by subtracting S1 from S0 is the area occupied by the voids in the measurement region.

[0042] Filling rate R = {S2 / (S0-S1)} × 100

[0043] Distance X 50 It can be obtained by the following method.

[0044] The filling rate R is calculated at the measuring points where the distance X from the outer surface of the porous body is 0.01D, 0.03D, 0.05D, 0.1D, 0.2D, 0.3D, 0.4D, 0.5D, 0.7D and 0.9D respectively. The filling rate R at the distance X of 0.01D can be calculated by the following method: a few points (for example, 3 to 5 points) are randomly selected in the measuring area at the distance X = 0.01D, the filling rate R is measured respectively, and their average value is calculated. Furthermore, in the measuring area at the distance X = 0.01D, the depth of the distance X = 0.01D is included near the center of the measuring area. For the cases where the distance X is other than 0.01D, the filling rate R is calculated in the same manner. At this time, the measurement areas of X=0.01D, 0.03D, 0.05D, 0.1D, 0.2D, 0.3D, 0.4D, 0.5D, 0.7D, and 0.9D were set so as not to overlap with each other.

[0045] The filling rate R is calculated for each measuring point at the distance X. It is confirmed that the larger the distance X, the smaller the filling rate R. The maximum value M1 of the measuring point at the distance X where the filling rate R is 50% or more and the minimum value M2 of the measuring point at the distance X where the filling rate R is less than 50% are calculated. 50 ) is greater than M1 and less than M2.

[0046] The electrical conductivity of the solid electrolyte layer may be, for example, 50 S / cm to 300 S / cm, or 60 S / cm to 200 S / cm.

[0047] The electrical conductivity of the solid electrolyte layer can be obtained by the following method.

[0048] The electrolytic capacitor is disassembled, the capacitor element is taken out, and the composition of the solid electrolyte layer is analyzed. When a treatment liquid is used to form the solid electrolyte layer, the composition of the treatment liquid can also be analyzed. As an analysis method, TEM (transmission electron microscopy)-EELS method (electron energy loss spectroscopy), NMR method (nuclear magnetic resonance spectroscopy), Raman spectroscopy, etc. can be used.

[0049] Based on the analysis results, a sample film (e.g., 20 μm to 40 μm thick) containing the same components as the solid electrolyte layer is formed, and the conductivity of the sample film is obtained as the conductivity of the solid electrolyte layer. As a conductivity measurement device, LORESTA-GX and PSP probe (hydrogen polysulfide fluorescent probe) manufactured by Nitto Seiko Analytech can be used.

[0050] (porous body)

[0051] The porous body contains a valve-acting metal. As the valve-acting metal, aluminum (Al), titanium (Ti), tantalum (Ta), niobium (Nb), zirconium (Zr), hafnium (Hf), etc. can be used.

[0052] As the porous body, for example, a sintered product of a molded body of raw material particles (raw material powder) containing a valve metal can be used. The particles can be particles of the valve metal, particles of an alloy containing the valve metal, or particles of a compound containing the valve metal. The particles can be used alone or in combination of two or more.

[0053] The porous body can be obtained, for example, by the following method: raw material particles are press-formed into a predetermined shape to obtain a formed body, and then the formed body is sintered. For example, an anode wire is arranged at a predetermined position of a mold, raw material particles are put into the mold, and a formed body can also be obtained by press-forming. By sintering the formed body, a porous body in which a part of the anode wire is buried can also be obtained. The porous body is usually a rectangular parallelepiped.

[0054] The average particle size of the raw material particles is preferably, for example, 0.05 μm or more and 0.5 μm or less. The average particle size referred to here is a median particle size (D50) in a volume particle size distribution determined by a laser diffraction particle size distribution analyzer.

[0055] The so-called CV value of the porous body is expressed by the product of the formation voltage and the measured electrostatic capacitance (electrostatic capacitance per unit mass excluding the anode wire) after the porous body is subjected to a formation treatment in a phosphoric acid aqueous solution (concentration of 0.02 mass %) at a formation voltage of 10 V and a temperature of 60°C for 2 hours and then the electrostatic capacitance is measured at a frequency of 120 Hz.

[0056] The raw material particles used to form the porous body have many fine irregularities. When the surface area of ​​the raw material particles themselves is large, a porous body with a small pore size and a large surface area is easily obtained. With such a porous body, a large CV value is easily obtained.

[0057] The most frequent pore diameter of a porous body having a CV value of 70000 μF·V / g or more and less than 100000 μF·V / g is, for example, 0.24 μm or more and 0.37 μm or less. The most frequent pore diameter of a porous body having a CV value of 100000 μF·V / g or more and less than 150000 μF·V / g is, for example, 0.17 μm or more and 0.26 μm or less. The most frequent pore diameter of a porous body having a CV value of 150000 μF·V / g or more is, for example, 0.10 μm or more and 0.21 μm or less. Furthermore, the most frequent pore diameter is the most frequent pore diameter in the volume-based pore diameter distribution measured by a mercury porosimeter. The anode body can be obtained by forming a thin oxide film on the surface of the porous body by chemical conversion treatment, etc., and the most frequent pore diameter of the anode body can be said to be approximately the same value as the most frequent pore diameter of the porous body.

[0058] The anode body may also include a rod-shaped anode wire partially embedded in the porous body. A portion of the anode wire may also be embedded in the porous body in a manner passing through the center of the porous body. When the porous body is a rectangular parallelepiped, the anode wire is planted (or erected) from one end face of the rectangular parallelepiped. The anode wire may also contain a valve-acting metal. A portion of the anode wire is embedded in the porous body, and the remaining portion protrudes from the porous body. The remaining portion is connected to the anode lead terminal by welding or the like.

[0059] (Dielectric layer)

[0060] The dielectric layer is formed in a manner covering the outer surface of the porous body and the inner wall surface of the pores of the porous body. The dielectric layer can be formed, for example, by subjecting the porous body to a chemical conversion treatment so that an oxide film grows on the surface of the porous body. The chemical conversion treatment can also be performed by immersing the porous body in a chemical conversion solution so that the surface of the porous body is anodic oxidized. Alternatively, the surface of the porous body can be oxidized by heating the porous body in an oxygen-containing atmosphere.

[0061] (Solid electrolyte layer)

[0062] The solid electrolyte layer is configured to cover at least a portion of the dielectric layer. The solid electrolyte layer may also be filled in the pores of the porous body via the dielectric layer and formed on the outer surface of the porous body. The solid electrolyte layer may also be a laminate of two or more different solid electrolyte layers.

[0063] The solid electrolyte layer contains a conductive polymer. The conductive polymer may also be a π-conjugated polymer. Examples of conductive polymers include polypyrrole, polythiophene, polyaniline, and derivatives thereof. They may be used alone or in combination. In addition, the conductive polymer may also be a copolymer of two or more monomers. Furthermore, the so-called derivative of the conductive polymer refers to a polymer with a conductive polymer as a basic skeleton. For example, examples of derivatives of polythiophene include poly(3,4-ethylenedioxythiophene) (PEDOT) and the like.

[0064] A dopant may also be added to the conductive polymer. That is, the solid electrolyte layer may also contain a conductive polymer and a dopant. The conductive polymer may also be contained in the solid electrolyte layer in a state doped with a dopant. The dopant may be selected according to the conductive polymer, and a known dopant may also be used. Examples of dopants include benzenesulfonic acid, alkylbenzenesulfonic acid, naphthalenesulfonic acid, alkylnaphthalenesulfonic acid, polystyrenesulfonic acid (PSS) and salts thereof. The solid electrolyte layer may contain, for example, PEDOT doped with PSS.

[0065] The solid electrolyte layer containing a conductive polymer can be formed, for example, by the following method: a first treatment liquid containing a monomer (or oligomer) is impregnated into a porous body (anode body) having a dielectric layer formed on the surface, and then the monomer (or oligomer) is polymerized by electrolytic polymerization or chemical polymerization. In the case of chemical polymerization, the first treatment liquid contains, for example, a monomer (or oligomer), an oxidant, and a solvent (or a dispersion medium). Examples of monomers include 3,4-ethylenedioxythiophene (EDOT), pyrrole, and the like. The first treatment liquid may also contain a dopant.

[0066] Alternatively, the solid electrolyte layer may be formed by impregnating a second treatment liquid containing a conductive polymer into a porous body (anode body) having a dielectric layer formed on the surface, and then drying the second treatment liquid. The second treatment liquid may contain, for example, a conductive polymer, a solvent (or a dispersion medium), and a dopant as required.

[0067] The filling rate R of the solid electrolyte layer in the depth direction of the porous body can be adjusted by, for example, changing the conditions of electrolytic polymerization (current value, polymerization time, composition of the electrolyte, temperature, etc.), chemical polymerization conditions (composition of the first treatment solution, polymerization time, temperature, etc.), etc. Electrolytic polymerization can easily control the reaction rate by the current value, thereby making it easy to control the filling rate.

[0068] The filling rate R of the solid electrolyte layer in the depth direction of the porous body can also be adjusted by combining the formation of the solid electrolyte layer based on electrolytic polymerization and the formation of the solid electrolyte layer based on chemical polymerization. In addition, the filling rate R of the solid electrolyte layer in the depth direction of the porous body can also be adjusted by combining the formation of the solid electrolyte layer based on the first treatment liquid and the formation of the solid electrolyte layer based on the second treatment liquid.

[0069] (other)

[0070] The capacitor element may also include a cathode layer covering at least a portion of the solid electrolyte layer. The electrolytic capacitor may also include an anode lead terminal and a cathode lead terminal electrically connected to the capacitor element, and an outer packaging resin arranged around the capacitor element. The cathode lead terminal is connected to the cathode portion through a conductive member. The anode lead terminal is connected to the end of the anode wire protruding from the porous body. The shape, size, etc. of the capacitor element are not particularly limited, and it may also be a known capacitor element or a capacitor element having the same structure as it.

[0071] (Cathode layer)

[0072] The cathode layer may also include a carbon layer formed on the solid electrolyte layer and a metal paste layer formed on the carbon layer. The carbon layer may also be formed of a conductive carbon material such as graphite and a resin. The metal paste layer may also be formed of metal particles (such as silver particles) and a resin, for example, it may also be formed of a known silver paste.

[0073] (Conductive member)

[0074] The cathode layer is connected to the connecting portion of the cathode lead terminal through a conductive member. That is, the cathode layer (cathode portion) is electrically connected to the cathode lead terminal. The conductive member is made of a conductive material. The conductive member can also be formed of a material containing metal particles (e.g., silver particles) and a resin, for example, it can also be formed using a known metal paste (e.g., silver paste). The conductive member is formed by heating the metal paste. Furthermore, the conductive member can also be composed of a plurality of conductive layers of different types.

[0075] (Outer packaging resin)

[0076] The outer packaging resin is arranged around the capacitor element in a manner that the capacitor element is not exposed on the surface of the electrolytic capacitor. In addition, the outer packaging resin insulates the anode lead terminal and the cathode lead terminal. As the outer packaging resin, a known outer packaging resin used in an electrolytic capacitor can also be used. For example, the outer packaging resin can also be formed by using an insulating resin material used in the sealing of the capacitor element. The outer packaging resin can also be formed by accommodating the capacitor element in a mold, and using a transfer molding method, a compression molding method, etc., to introduce an uncured thermosetting resin and a filler into the mold and solidify them.

[0077] Examples of the outer coating resin include epoxy resin, phenol resin, silicone resin, melamine resin, urea resin, alkyd resin, polyurethane, polyimide, and unsaturated polyester. The outer coating resin may contain substances other than the resin (eg, inorganic filler).

[0078] (Cathode lead terminal)

[0079] A portion of the cathode lead terminal is exposed from the outer packaging resin and can be used as a cathode external terminal. The material of the cathode lead terminal can be any material that can be used as a material of the cathode lead terminal of the electrolytic capacitor. For example, a known cathode lead terminal material used in an electrolytic capacitor can also be used. The cathode lead terminal can also be formed by processing a metal sheet (including a metal plate and a metal foil) composed of a metal (copper, copper alloy, etc.) using a known metal processing method.

[0080] (Anode lead terminal)

[0081] A portion of the anode lead terminal is exposed from the outer packaging resin and can be used as an anode external terminal. The material of the anode lead terminal can be any material that can be used as the material of the anode lead terminal of the electrolytic capacitor. For example, a known anode lead terminal material used in an electrolytic capacitor can also be used. The anode lead terminal can also be formed by processing a metal sheet (including a metal plate and a metal foil) composed of a metal (copper, copper alloy, etc.) using a known metal processing method.

[0082] Figure 1 It is a cross-sectional view schematically showing an example of the electrolytic capacitor according to the present embodiment. Figure 2 It is a cross-sectional view schematically showing an anode body having a solid electrolyte layer formed on the surface. Figure 3 It is a cross-sectional view schematically showing a porous body. Figure 4 is along Figure 3 A cross-sectional view taken along line IV-IV. Figure 3 and 4 It is a cross-sectional view including the center C of the porous body. Figure 3 and Figure 4As an example, X is shown 50 =0.5D, but the electrolytic capacitor according to the present embodiment is not limited thereto. In addition, each figure is a schematic diagram, and the ratio of the dimensions (length, width, thickness, etc.) of each component is not limited to the actual one.

[0083] The electrolytic capacitor 20 includes a capacitor element 10, an outer packaging resin 11 that seals the capacitor element 10, and an anode lead terminal 12 and a cathode lead terminal 13 that are electrically connected to the capacitor element 10. A portion of the anode lead terminal 12 and the cathode lead terminal 13 are respectively exposed from the outer packaging resin 11. A portion of the anode lead terminal 12 and the cathode lead terminal 13 are covered with the outer packaging resin 11 together with the capacitor element 10.

[0084] The capacitor element 10 includes an anode body 1, a solid electrolyte layer 2 formed on the anode body 1, and a cathode layer 3 formed on the solid electrolyte layer 2. The anode body 1 includes a porous body 4 containing a valve-acting metal, and a dielectric layer 5 covering the porous body 4. The dielectric layer 5 is formed so as to cover the outer surface S of the porous body 4 and the inner wall surface of the pore 7. The anode body 1 has a porous shape substantially the same as that of the porous body 4.

[0085] The porous body 4 has a substantially rectangular parallelepiped shape and has six side surfaces. A portion of the anode wire 6 extends from one side surface of the porous body 4. That is, the anode wire 6 has a first portion 6a buried from one side surface of the porous body 4 toward the inside of the porous body 4, and a second portion 6b extending from one side surface of the porous body 4. The second portion 6b is joined to the anode lead terminal 12 by welding or the like. In the present embodiment, the first portion 6a is buried in the porous body 4 in a manner passing through the center C of the porous body 4, but may be buried in the porous body 4 in a manner not passing through the center C of the porous body 4.

[0086] The solid electrolyte layer 2 is formed so as to cover at least a portion of the dielectric layer 5. The solid electrolyte layer 2 is filled in the pores 7 of the porous body 4 (anode body 1). The solid electrolyte layer 2 is formed so as to cover the outer surface S of the porous body 4 and the inner wall surface of the pore 7 via the dielectric layer 5.

[0087] The filling rate R of the solid electrolyte layer 2 in the porous body decreases from the outer surface S of the porous body 4 toward the center C. That is, the filling rate R decreases as the distance X from the outer surface S of the porous body 4 increases. The shortest distance from the outer surface S of the porous body 4 to the center C is set to D. The distance X (X ) from the outer surface S of the porous body 4 when the filling rate R reaches 50% is 50 ) is 0.5D. Figure 3 and Figure 4As shown, the porous body 4 has a first region 4a on the outer surface side of the porous body 4 and a second region 4b outside the first region 4a. The first region 4a is a region where the distance X from the outer surface S of the porous body 4 is less than 0.5D ( Figure 3 and Figure 4 The portion where the grid is drawn) is an area where the filling rate R is greater than 50%.

[0088] The cathode layer 3 is formed in a manner covering the surface of the solid electrolyte layer 2. The cathode layer 3 has a carbon layer 3a formed in a manner covering the solid electrolyte layer 2, and a metal paste layer 3b formed on the surface of the carbon layer 3a. The cathode lead terminal 13 is bonded to the cathode layer 3 (metal paste layer 3b) through a conductive member 8. The carbon layer 3a contains a conductive carbon material such as graphite and a resin. The metal paste layer 3b contains, for example, metal particles (such as silver) and a resin. Furthermore, the composition of the cathode layer 3 is not limited to this composition. The cathode layer 3 can be any composition as long as it has a current collection function.

[0089] [Example]

[0090] Hereinafter, the present disclosure will be specifically described using Examples and Comparative Examples, but the present disclosure is not limited to the following Examples.

[0091] 《Examples 1 to 5, Comparative Examples 1 to 2》

[0092] (Production of porous body)

[0093] One end of the anode wire is buried in Ta particles, the Ta particles are formed into a rectangular parallelepiped, and then the formed body is sintered in a vacuum. In this way, a porous body (Ta sintered body) in which a part of the anode wire is buried is obtained. The shortest distance D from the outer surface to the center of the porous body is 450μm. Ta wire is used as the anode wire.

[0094] (Formation of Dielectric Layer)

[0095] The porous body in which a part of the anode wire is buried is subjected to chemical conversion treatment (anodization) to form a dielectric layer (thickness of 22 nm) on the surface of the porous body, thereby obtaining an anode body. The dielectric layer is a layer of tantalum oxide (Ta2O5). The porous body is subjected to chemical conversion treatment for 2 hours at a conversion voltage of 10 V and a temperature of 60°C in a 0.02 mass % phosphoric acid aqueous solution. The CV value of the porous body is 70000 μF·V / g. The CV value is adjusted by the Ta particles (surface area, etc.) used in the production process of the porous body.

[0096] (Formation of Solid Electrolyte Layer)

[0097] A solid electrolyte layer (conductivity 80 S / cm) containing polypyrrole and a dopant was formed in the pores of a porous body (anode body) having a dielectric layer on the surface. As the dopant, a sulfonate having a naphthalene skeleton was used.

[0098] The solid electrolyte layer is formed by electrolytic polymerization. The electrolytic polymerization is carried out at 20° C. using a treatment solution containing pyrrole, a dopant and water. In the electrolytic polymerization, the current value and the polymerization time are appropriately adjusted so that the filling rate R of the solid electrolyte layer at a distance X from the outer surface of the porous body is the value shown in Table 1.

[0099]

[0100] In addition, the filling rate R of the solid electrolyte layer at a distance X from the outer surface of the porous body is obtained by the method described above.

[0101] (Formation of cathode layer)

[0102] A dispersion of carbon particles (carbon slurry) is applied to the solid electrolyte layer and then heated to form a carbon layer on the surface of the solid electrolyte layer. A metal slurry containing silver particles, a binder resin and a solvent is applied to the surface of the carbon layer and then heated to form a metal slurry layer, thereby obtaining a cathode layer composed of a carbon layer and a metal slurry layer. In this way, a capacitor element is obtained.

[0103] (Manufacturing of electrolytic capacitors)

[0104] A conductive adhesive material that becomes a conductive component is applied to the metal paste layer, and the cathode lead terminal is joined to the metal paste layer. The anode wire and the anode lead terminal are joined by impedance welding. Next, the capacitor element joined with each lead terminal is sealed with an outer packaging resin. In this way, an electrolytic capacitor is obtained. In Table 1, A1-1 to A1-5 represent the electrolytic capacitors of Examples 1 to 5, respectively. B1-1 to B1-2 represent the electrolytic capacitors of Comparative Examples 1 to 2, respectively.

[0105] [evaluate]

[0106] For each electrolytic capacitor obtained as described above, the ESR at a frequency of 100 kHz (hereinafter referred to as ESR1) and the ESR at a frequency of 500 kHz (hereinafter referred to as ESR2) were measured in an environment of 20°C using a 4-terminal LCR meter.

[0107] The evaluation results are shown in Table 2. ESR1 is expressed as a relative value when the ESR1 value of the electrolytic capacitor B1-1 of Comparative Example 2 is set to 100. ESR2 is expressed as a relative value when the ESR2 value of the electrolytic capacitor B1-2 of Comparative Example 2 is set to 100. In addition, Table 2 also shows the formation time of the solid electrolyte layer. The formation time is the polymerization time during electrolytic polymerization. The formation time is expressed as a relative value when the formation time in Comparative Example 2 is set to 100.

[0108]

[0109] In electrolytic capacitors A1-1 to A1-5, the solid electrolyte layer is formed in a short time, and both ESR1 and ESR2 are reduced. 50 In the electrolytic capacitor B1-1 with a value lower than 0.1D, ESR1 increases significantly. 50 In the electrolytic capacitor B1-2 having an ESR of 0.7 or more, the solid electrolyte layer takes a long time to form and ESR2 increases significantly.

[0110] 《Examples 6 to 8, Comparative Examples 3 to 4》

[0111] In the dielectric formation process, the porous body in which a part of the anode wire is buried is subjected to a chemical formation treatment (anodization) to form a dielectric layer (thickness of 22nm) on the surface of the porous body, thereby obtaining an anode body. The dielectric layer is a layer of tantalum oxide (Ta2O5). The porous body is subjected to a chemical formation treatment for 2 hours at a forming voltage of 10V and a temperature of 60°C in a 0.02 mass% phosphoric acid aqueous solution. The CV value of the porous body is 100000μF·V / g.

[0112] In the electrolytic polymerization in the solid electrolyte layer forming step, the current value and polymerization time were appropriately adjusted so that the filling rate R of the solid electrolyte layer at a distance X from the outer surface of the porous body became the value shown in Table 3.

[0113]

[0114] Electrolytic capacitors A2-1 to A2-3 of Examples 6 to 8 and electrolytic capacitors B2-1 to B2-2 of Comparative Examples 3 to 4 were produced and evaluated in the same manner as the electrolytic capacitor A1-1 of Example 1 except for the above.

[0115] The evaluation results are shown in Table 4. In Table 4, ESR1 is expressed as a relative value when the ESR1 value of the electrolytic capacitor B2-1 of Comparative Example 3 is set to 100. ESR2 is expressed as a relative value when the ESR2 value of the electrolytic capacitor B2-2 of Comparative Example 4 is set to 100. In addition, Table 4 also shows the formation time of the solid electrolyte layer. This formation time is the polymerization time in electrolytic polymerization.

[0116] This formation time is expressed as a relative value when the formation time in Comparative Example 4 is set to 100.

[0117]

[0118] In electrolytic capacitors A2-1 to A2-3, the solid electrolyte layer is formed in a short time, and both ESR1 and ESR2 are reduced. 50 In the electrolytic capacitor B2-1 with a value lower than 0.05D, ESR1 increases significantly. 50 In the electrolytic capacitor B2-2 having an ESR of 0.3 or more, the solid electrolyte layer takes a long time to form and ESR2 increases.

[0119] 《Examples 9-11, Comparative Examples 5-6》

[0120] In the dielectric formation process, the porous body in which a part of the anode wire is buried is subjected to a chemical formation treatment (anodization) to form a dielectric layer (thickness of 22nm) on the surface of the porous body, thereby obtaining an anode body. The dielectric layer is a layer of tantalum oxide (Ta2O5). The porous body is subjected to a chemical formation treatment for 2 hours at a forming voltage of 10V and a temperature of 60°C in a 0.02 mass% phosphoric acid aqueous solution. The CV value of the porous body is 150000μF·V / g.

[0121] In the electrolytic polymerization in the solid electrolyte layer forming step, the current value and polymerization time were appropriately adjusted so that the filling rate R of the solid electrolyte layer at a distance X from the outer surface of the porous body became the value shown in Table 5.

[0122]

[0123] Electrolytic capacitors A3-1 to A3-3 of Examples 9 to 11 and electrolytic capacitors B3-1 to B3-2 of Comparative Examples 5 to 6 were produced and evaluated in the same manner as the electrolytic capacitor A1-1 of Example 1 except for the above.

[0124] The evaluation results are shown in Table 6. In Table 6, ESR1 is expressed as a relative value when the ESR1 value of the electrolytic capacitor B3-1 of Comparative Example 5 is set to 100. ESR2 is expressed as a relative value when the ESR2 value of the electrolytic capacitor B3-2 of Comparative Example 6 is set to 100. In addition, Table 6 also shows the formation time of the solid electrolyte layer. This formation time is the polymerization time in electrolytic polymerization.

[0125] This formation time is expressed as a relative value when the formation time in Comparative Example 6 is set to 100.

[0126]

[0127] In the electrolytic capacitors A3-1 to A3-3, the solid electrolyte layer is formed in a short time, and both ESR1 and ESR2 are reduced. 50 In the electrolytic capacitor B3-1 with a value lower than 0.03D, ESR1 increases significantly. 50 In the electrolytic capacitor B3-2 with a resistance of 0.2D or more, the formation time of the solid electrolyte layer is long and ESR2 increases significantly.

[0128] Industrial Applicability

[0129] The electrolytic capacitor according to the present disclosure can be used in various applications requiring low ESR.

[0130] The present invention has been described with respect to the currently preferred embodiments, but such disclosure is not to be construed in a limiting sense. Various modifications and changes will become apparent to those skilled in the art of the present invention upon reading the above disclosure. Therefore, the appended claims should be construed to include all modifications and changes without departing from the true spirit and scope of the present invention.

[0131] Explanation of symbols

[0132] 1: anode body, 2: solid electrolyte layer, 3: cathode layer, 3a: carbon layer, 3b: metal paste layer, 4: porous body, 4a: first region, 4b: second region, 5: dielectric layer, 6: anode wire, 6a: first part, 6b: second part, 7: hole, 8: conductive member, 10: capacitor element, 11: outer packaging resin, 12: anode lead terminal, 13: cathode lead terminal, 20: electrolytic capacitor

Claims

1. An electrolytic capacitor comprising: an anode body having a porous body containing a valve action metal and a dielectric layer covering the porous body; and a solid electrolyte layer filling the pores of the porous body and covering the dielectric layer; wherein, The CV value of the porous body is lower than 100000 μF·V / g, The filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface toward the center of the porous body. The shortest distance D from the outer surface to the center of the porous body and the distance X from the outer surface of the porous body when the filling rate R of the solid electrolyte layer reaches 50% satisfy the relationship of 0.1D≤X<0.7D.

2. The electrolytic capacitor according to claim 1, wherein: The CV value of the porous body is 70000 μF·V / g or more and less than 100000 μF·V / g, The filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.1D is 50% or more and 80% or less.

3. The electrolytic capacitor according to claim 1 or 2, wherein: The CV value of the porous body is 70000 μF·V / g or more and less than 100000 μF·V / g, The filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.7D is more than 16% and 48% or less.

4. An electrolytic capacitor comprising: an anode body having a porous body containing a valve action metal and a dielectric layer covering the porous body; and a solid electrolyte layer filling the pores of the porous body and covering the dielectric layer; wherein, The CV value of the porous body is 100000 μF·V / g or more and less than 150000 μF·V / g, The filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface toward the center of the porous body. The shortest distance D from the outer surface to the center of the porous body and the distance X from the outer surface of the porous body when the filling rate R of the solid electrolyte layer reaches 50% satisfy the relationship of 0.05D≤X<0.3D.

5. The electrolytic capacitor according to claim 4, wherein: The filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.05D is 50% or more and 83% or less.

6. The electrolytic capacitor according to claim 4 or 5, wherein: The filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.3D is more than 13% and 44% or less.

7. An electrolytic capacitor comprising: an anode body having a porous body containing a valve action metal and a dielectric layer covering the porous body; and a solid electrolyte layer filling the pores of the porous body and covering the dielectric layer; wherein, The CV value of the porous body is 150000 μF·V / g or more, The filling rate R of the solid electrolyte layer in the porous body decreases from the outer surface toward the center of the porous body. The shortest distance D from the outer surface to the center of the porous body and the distance X from the outer surface of the porous body when the filling rate of the solid electrolyte layer reaches 50% satisfy the relationship of 0.03D≤X<0.2D.

8. The electrolytic capacitor according to claim 7, wherein: The CV value of the porous body is 150000 μF·V / g or more, The filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.03D is 56% or more and 83% or less.

9. The electrolytic capacitor according to claim 7 or 8, wherein: The CV value of the porous body is 150000 μF·V / g or more, The filling rate R of the solid electrolyte layer when the distance X from the outer surface of the porous body is 0.2D is 14% or more and 41% or less.

Citation Information

Patent Citations

  • Solid electrolytic capacitor and its manufacture

    JP1999087177A