Ultrasonic coupling agent for enhancing sound wave penetrating power and reducing attenuation and preparation method thereof
By using a combination of polymer base material, sound velocity regulator and sound attenuation regulator in the ultrasonic coupling agent, the problem of insufficient penetration ability in high-frequency ultrasonic transmission is solved, efficient sound wave transmission in different media is achieved, and the Quality of ultrasound imaging.
Patent Information
- Application Number
- CN202410779631.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-22
AI Technical Summary
Existing ultrasonic coupling agents have insufficient penetration capabilities in high-frequency ultrasonic transmission, resulting in energy attenuation and reduced imaging clarity. Especially when the difference in acoustic impedance between different media is large, the loss of acoustic energy is serious.
A new type of ultrasonic coupling agent is prepared using a combination of polymer base materials, sound velocity regulators, sound attenuation regulators, plasticizers and cross-linking agents through specific proportions and preparation methods, including 50%-70% polymerization Basic materials, 10%-30% sound velocity regulator, 10%-30% sound attenuation regulator, 1% plasticizer and 0.5% cross-linking agent form an ultrasonic coupling agent with optimized acoustic properties.
It effectively improves the penetration ability of ultrasound in various media, reduces attenuation, and optimizes the quality of ultrasound imaging. Especially in high-frequency ultrasound applications, it significantly improves image resolution and contrast.
Smart Images

Figure CN118806937A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultrasonic coupling agents, and in particular to an ultrasonic coupling agent capable of enhancing the penetration ability of sound waves and reducing attenuation, and a preparation method thereof. Background Art
[0002] Ultrasound technology is favored by the medical community and patients in the field of medical imaging because of its non-invasive, real-time imaging capabilities and low cost. When ultrasound passes through human tissue, it can capture the structure and function information of internal organs in real time, providing an important basis for the diagnosis and treatment of diseases.
[0003] When ultrasound waves pass through different media, such as air, skin, and fat, they will experience energy attenuation and decreased penetration. This is mainly because the physical properties of ultrasound waves, such as propagation speed and acoustic impedance, vary in different media, causing reflection and refraction of the sound waves at the interface, thereby losing some energy. Especially in high-frequency ultrasound imaging, due to the increase in the frequency of the sound waves, this problem of energy attenuation and decreased penetration becomes more prominent, seriously affecting the clarity and accuracy of the imaging.
[0004] In order to improve the transmission efficiency of ultrasound, ultrasonic coupling agent is widely used as an important auxiliary material in the process of ultrasound imaging. The main function of ultrasonic coupling agent is to form a continuous medium between the ultrasound probe and human skin to exclude air and reduce the reflection and refraction of sound waves at the interface, thereby improving the transmission efficiency of sound waves.
[0005] However, existing ultrasonic coupling agents are mainly designed for ultrasound in the conventional frequency range and are not optimized for the transmission of high-frequency ultrasound. In addition, the matching performance of existing ultrasonic coupling agents between different media is limited. Due to the complexity of human internal tissues, the acoustic impedance differences between different tissues are large, and the energy loss of sound waves at the interface is large, resulting in reduced image resolution and contrast. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides an ultrasonic coupling agent for enhancing the sound wave penetration ability and reducing attenuation and a preparation method thereof.
[0007] The technical problem solved by the present invention can be achieved by adopting the following technical solutions:
[0008] An ultrasonic coupling agent for enhancing the penetration ability of sound waves and reducing attenuation, comprising:
[0009] The polymer base material is 50%-70%, the sound velocity regulator is 10%-30%, the sound attenuation regulator is 10%-30%, the plasticizer is 1%, the cross-linking agent is 0.5%, and the rest is water.
[0010] Preferably, the polymer base material includes at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyurethane, polydimethylsiloxane, and polymethyl methacrylate.
[0011] Preferably, the sonic velocity regulator includes at least one of glycerol, ethylene glycol, propylene glycol, polyethylene glycol, and vegetable oil.
[0012] Preferably, the sound attenuation regulator includes at least one of zinc oxide, titanium oxide, aluminum oxide, carbon nanotubes, graphene oxide, and barium titanate.
[0013] The present invention also provides a method for preparing an ultrasonic coupling agent that enhances the sound wave penetration ability and reduces attenuation, comprising:
[0014] Step S1, adding 50%-70% of the polymer base material and 10%-30% of the sonic velocity regulator into solvent water, then heating to a preset temperature and continuously stirring to obtain a first mixed solution;
[0015] Step S2, adding 1% plasticizer to the first mixed solution, and maintaining heating and stirring to obtain a second mixed solution;
[0016] Step S3, continuously stirring the second mixed solution while it is naturally cooled to room temperature, and adding 0.5% of a cross-linking agent to the second mixed solution cooled to room temperature to obtain a third mixed solution;
[0017] Step S4, adding 10%-30% of an acoustic attenuation regulator to the third mixed solution to obtain a fourth mixed solution;
[0018] Step S5, placing the fourth mixed solution into a mold for solidification to obtain an ultrasonic coupling agent.
[0019] Preferably, in step S1, the polymer base material includes at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyurethane, polydimethylsiloxane, and polymethyl methacrylate.
[0020] Preferably, in step S1, the sonic velocity regulator includes at least one of glycerol, ethylene glycol, propylene glycol, polyethylene glycol, and vegetable oil.
[0021] Preferably, in step S1, the preset temperature is 80°C-90°C.
[0022] Preferably, in step S4, the sound attenuation regulator includes at least one of zinc oxide, titanium oxide, aluminum oxide, carbon nanotubes, graphene oxide, and barium titanate.
[0023] The advantages or beneficial effects of the technical solution of the present invention are:
[0024] The present invention provides a novel ultrasonic coupling agent as a transmission medium for high-frequency ultrasonic waves, which can effectively improve the penetration ability of ultrasonic waves in various media and reduce attenuation, so as to optimize the quality of ultrasonic imaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The figure is a flow chart of a method for preparing an ultrasonic coupling agent in a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0028] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but they are not intended to limit the present invention.
[0029] See also Figure 1 In a preferred embodiment of the present invention, based on the above-mentioned problems existing in the prior art, an ultrasonic coupling agent and a preparation method thereof are provided for enhancing the sound wave penetration ability and reducing the attenuation.
[0030] The components of the ultrasonic coupling agent include: 50%-70% of polymer base material, 10%-30% of sound velocity regulator, 10%-30% of sound attenuation regulator, 1% of plasticizer, 0.5% of cross-linking agent, and the rest is water.
[0031] The preparation method of the ultrasonic coupling agent comprises the following steps:
[0032] Step S1, adding 50%-70% of the polymer base material and 10%-30% of the sonic velocity regulator into solvent water, then heating to a preset temperature and continuously stirring to obtain a first mixed solution;
[0033] Among them, the preset temperature is 80℃-90℃.
[0034] Step S2, adding 1% plasticizer to the first mixed solution, and maintaining heating and stirring to obtain a second mixed solution;
[0035] Step S3, continuously stirring the second mixed solution while it is naturally cooled to room temperature, and adding 0.5% of a cross-linking agent to the second mixed solution cooled to room temperature to obtain a third mixed solution;
[0036] Step S4, adding 10%-30% of an acoustic attenuation regulator to the third mixed solution to obtain a fourth mixed solution;
[0037] Step S5, placing the fourth mixed solution into a mold for solidification to obtain an ultrasonic coupling agent.
[0038] As a preferred embodiment, the polymer base material includes at least one of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyurethane (PU), polydimethylsiloxane (PDMS), and polymethyl methacrylate (PMMA).
[0039] Specifically, the polymer base material is selected from one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyurethane, polydimethylsiloxane, and polymethyl methacrylate. Among them, polyvinyl pyrrolidone has good biocompatibility and film-forming properties; polyurethane has excellent mechanical properties and elasticity; polydimethylsiloxane (PDMS): has good flexibility and biocompatibility, and is easy to process; polymethyl methacrylate (PMMA): has good optical transparency and mechanical strength. Different single polymers or combinations of polymers are selected according to specific needs.
[0040] As a preferred embodiment, the sonic velocity regulator includes at least one of glycerol, ethylene glycol, propylene glycol, polyethylene glycol (PEG), and vegetable oil.
[0041] Specifically, the sound velocity regulator includes, but is not limited to, one or more of glycerol, ethylene glycol, propylene glycol, polyethylene glycol, and vegetable oil. Among them, regulators such as glycerol can adjust the sound velocity of the coupling agent to make it closer to the sound velocity of human tissue, which helps to reduce the reflection and refraction of sound waves when they are transmitted between media; ethylene glycol is similar to glycerol, but has different viscosity and acoustic properties; propylene glycol has lower viscosity and good miscibility; polyethylene glycol can be selected within different molecular weight ranges to adjust the sound velocity and mechanical properties; vegetable oil (such as olive oil, castor oil): can be used as a natural plasticizer and sound velocity regulator.
[0042] As a preferred embodiment, the sound attenuation regulator includes at least one of zinc oxide (ZnO), titanium oxide (TiO2), aluminum oxide (Al2O3), carbon nanotubes (CNTs), graphene oxide (GO), and barium titanate (BaTiO3).
[0043] Specifically, by introducing zinc oxide ZnO particles as fillers, zinc oxide ZnO has piezoelectric properties, phonon scattering, and sound absorption properties, which can be used to adjust the sound attenuation characteristics to increase the penetration depth while reducing the loss of sound wave energy. Titanium oxide also has good piezoelectric and acoustic properties; aluminum oxide can provide good sound attenuation properties; carbon nanotubes have excellent mechanical and electrical properties and can be used to adjust sound wave propagation; graphene oxide has good acoustic properties and mechanical strength; barium titanate is a commonly used piezoelectric material with excellent piezoelectric effect.
[0044] The goal of the embodiments of the present invention is to design a coupling agent with high sound penetration and low sound attenuation for medical ultrasound applications. The following shows the experimental process of the proportion configuration of the basic materials, including:
[0045] a) Preliminary screening:
[0046] First, collect samples of polyvinyl alcohol (PVA), polyacrylic acid (PAA), polydimethylsiloxane (PDMS) and other materials with different molecular weights that may be used as coupling agent base materials from the market. By consulting relevant materials and consulting experts, understand the acoustic properties and biocompatibility of these materials. Perform preliminary screening to exclude materials with poor acoustic properties or poor biocompatibility.
[0047] b) Theoretical calculation
[0048] Theoretical calculations are performed for the selected basic materials. The acoustic impedance (Z = ρc) of each material is calculated by consulting the standard data of material density (ρ) and sound velocity (c). In addition, computer simulation software can be used to predict the acoustic performance of different materials after mixing.
[0049] c) Experimental design
[0050] Design an experimental plan to test the effect of different proportions of base materials on the acoustic performance of the coupling agent. The experimental plan includes: determining the test ratio range (such as 10% to 90%, with a gradient of 10%), preparing experimental equipment and materials, and formulating experimental steps and operating procedures.
[0051] d) Small batch preparation
[0052] Prepare small batches of coupling agent samples according to the experimental design. For example, if PVA is selected as the base material, you can prepare coupling agent samples containing 10%, 20%, 30%... up to 90% PVA. During the preparation process, the addition amount and mixing uniformity of each component must be strictly controlled.
[0053] e) Acoustic performance test
[0054] Perform acoustic performance tests on each sample, such as using impedance tubes, ultrasonic velocimeters and other special equipment to measure the acoustic impedance and sound velocity of each sample, record the test data, and compare them with the corresponding values of human soft tissue.
[0055] Parameter nomenclature and expected values with corresponding values for human soft tissues:
[0056] Ztarget: Target acoustic impedance, approximately 1.5 MRayl (acoustic impedance of human soft tissue).
[0057] Ctarget: Target sound speed, approximately 1540 m / s (the speed of sound in human soft tissue).
[0058] αtarget: Target acoustic attenuation coefficient, as low as possible, usually less than 0.5dB / cm / MHz.
[0059] The acoustic properties test of ultrasonic coupling agent is to evaluate its parameters such as acoustic impedance, sound velocity and acoustic attenuation coefficient to ensure that the performance of the coupling agent meets the requirements of medical ultrasound applications. The following are the specific test methods:
[0060] Acoustic impedance (Z) measurement:
[0061] Impedance Tube Test: The acoustic impedance of the couplant is measured using an impedance tube. In an impedance tube, a sound wave generated by a sound source propagates through the tube, and the couplant sample is placed at one end of the tube. By measuring the amplitude of the reflected and transmitted sound waves, the acoustic impedance (Z) of the sample can be calculated.
[0062] Pulse reflection method: This is a non-contact measurement technique that uses the reflection of an ultrasonic pulse at the interface of two media to determine the acoustic impedance. By measuring the reflection coefficient and the known acoustic impedance of one medium, the acoustic impedance (Z) of the unknown medium can be calculated.
[0063] Sound velocity (C) determination:
[0064] Ultrasonic Velocimeter: The speed of sound through the couplant is measured using an ultrasonic velocimeter. This device typically has a transmitter and a receiver with the couplant sample placed between them. By measuring the time it takes for the ultrasound to travel through the sample and the known distance, the speed of sound (C) can be calculated.
[0065] Phase comparison method: This method calculates the speed of sound by comparing the phase change of ultrasound when it propagates in the sample. The speed of sound (C) of the couplant can be calculated by the phase difference between the couplant and the reference medium.
[0066] Determination of sound attenuation coefficient (α):
[0067] Transmission method: The intensity of the ultrasonic wave passing through the coupling agent sample is measured and compared with the intensity of the ultrasonic wave not passing through the sample. The attenuation coefficient (α) can be calculated from the attenuation of the sound wave intensity and the thickness of the sample.
[0068] Pulse-echo method: This method determines the acoustic attenuation coefficient by measuring the attenuation of a pulse echo reflected from a sample. By comparing the echo strength at different depths, the attenuation coefficient can be estimated.
[0069] Each test method has its own specific equipment and operating procedures. In actual testing, the appropriate method needs to be selected according to the physical state of the couplant, the test environment, and the required accuracy. The test results need to be recorded and analyzed for use in subsequent formulation optimization. In addition, environmental conditions such as temperature and pressure need to be controlled during the test, as these factors also affect the acoustic performance.
[0070] f) Data analysis
[0071] Collect and analyze experimental data; based on the test results, draw a curve chart showing the change in acoustic impedance and sound velocity with the base material ratio. Analyze the test results, compare with the target values, and find the base material ratio with the acoustic impedance and sound velocity closest to human soft tissue.
[0072] g) Iterative Optimization
[0073] Based on the results of the preliminary analysis, adjust the ratio, re-prepare the samples and test them for iterative optimization. If it is found that a certain ratio of base materials causes the acoustic impedance or acoustic velocity to be too high or too low, the ratio can be adjusted appropriately, and new samples can be re-prepared and tested. Repeat the iterative process until the optimal ratio that meets the requirements is found.
[0074] For example, if Z and C are significantly different from the target values, the ratio of PVA to glycerol may be adjusted, for example, by increasing the ratio of PVA to increase the acoustic impedance, or by increasing the ratio of glycerol to decrease the acoustic velocity.
[0075] h) Finalization
[0076] Repeat steps cg until Z, C, and α are close to the target values. After multiple iterations of optimization, the base material ratio that provides the best acoustic match is finally determined. Once the base material ratio that provides the best acoustic match is found, it can be used as the standard configuration of the coupling agent formula.
[0077] In practice, this process may require multiple iterations to ensure that the performance of the coupling agent fully meets the design requirements. Each iteration may involve fine-tuning multiple parameters, including the type of base material, its proportion, and its interaction with other components.
[0078] Through the above steps, an ultrasonic coupling agent with optimized acoustic properties can be obtained. The PVA-based ultrasonic coupling agent includes the following components:
[0079] Base material: PVA (50-70%)
[0080] Sonic velocity regulator: glycerol (10-30%)
[0081] Sound attenuation modifier: ZnO (10-30%)
[0082] Solvent: Water (3-5%)
[0083] Plasticizer: triethyl citrate (1%)
[0084] Cross-linking agent: Glutaraldehyde (0.5%)
[0085] The ultrasonic coupling agent with the above composition ratio is subjected to large-scale testing to verify its stability and repeatability, and the coupling agent is used in actual medical ultrasound equipment to verify whether its performance meets clinical requirements.
[0086] The acoustic impedance, acoustic velocity and acoustic attenuation coefficient of the above-mentioned PVA-based ultrasonic coupling agent are close to the corresponding values of human soft tissue, thereby improving the penetration ability of ultrasonic waves and reducing attenuation to obtain clearer imaging effects.
[0087] The following provides examples and comparative examples to further illustrate and describe the present technical solution:
[0088] Example 1
[0089] The components of the ultrasonic coupling agent in this embodiment 1 include:
[0090] Base material: PVA60%
[0091] Sonic velocity regulator: glycerol 24.5%
[0092] Sound attenuation modifier: ZnO 10%
[0093] Solvent: Water 4%
[0094] Plasticizer: Triethyl citrate 1%
[0095] Cross-linking agent: glutaraldehyde 0.5%
[0096] The preparation method of the ultrasonic coupling agent of this embodiment 1 comprises the following steps:
[0097] Step S1, preliminarily mixing 60% PVA powder, 24.5% glycerol and water at room temperature to ensure that all ingredients are evenly distributed; heating the mixture to 80-90° C. while continuously stirring for about 30 minutes, and promoting the full dissolution of PVA and the uniform distribution of ingredients by stirring until the PVA is completely dissolved to form a uniform first mixed solution;
[0098] Step S2, after the PVA is completely dissolved, 1% triethyl citrate (plasticizer) is added to the first mixed solution, and heating and stirring are continued for about 10-15 minutes to ensure that the plasticizer is fully mixed and evenly distributed in the second mixed solution;
[0099] Step S3, remove the second mixed solution from the heating source and allow it to cool naturally to room temperature, and continue to gently stir it during the cooling period to prevent any components from precipitating or stratifying; when the second mixed solution is cooled to room temperature, add 0.5% glutaraldehyde (cross-linking agent) and stir it thoroughly for 5-10 minutes to ensure that the cross-linking agent is evenly distributed and starts a cross-linking reaction with PVA.
[0100] Step S4, finally, adding ZnO particles and continuing stirring for about 20-30 minutes under controlled conditions to ensure that the ZnO particles are evenly distributed in the mixture.
[0101] In this step, the stirring speed can be appropriately adjusted to ensure that the ZnO particles do not aggregate or precipitate.
[0102] Step S5, pouring the fourth mixed solution into a preset mold, curing at room temperature or slightly higher temperature (about 25-30° C.), and curing at room temperature for 24 hours to ensure that the coupling agent forms a final product with consistency and stability.
[0103] Example 2
[0104] The components of the ultrasonic coupling agent in this embodiment 2 are similar to those in embodiment 1, but the proportions of the components are different, wherein:
[0105] Base material: PVA55%
[0106] Sonic velocity regulator: 19.5% glycerol
[0107] Sound attenuation modifier: ZnO 20%
[0108] The proportions of solvent, plasticizer and cross-linking agent are the same as those in Example 1.
[0109] The preparation method is the same as that in Example 1, except that the contents of components added in each step are different, which will not be described in detail here.
[0110] Example 3
[0111] The components of the ultrasonic coupling agent in this embodiment 3 are similar to those in embodiment 1, but the proportions of the components are different, wherein:
[0112] Base material: PVA50%
[0113] Sonic velocity regulator: 14.5% glycerol
[0114] Sound attenuation modifier: ZnO 30%
[0115] The proportions of solvent, plasticizer and cross-linking agent are the same as those in Example 1.
[0116] The preparation method is the same as that in Example 1, except that the contents of components added in each step are different, which will not be described in detail here.
[0117] Comparative Example 1
[0118] The difference between the ultrasonic coupling agent provided in this comparative example 1 and that in Example 1 is that this comparative example 1 does not contain ZnO, and its components specifically include:
[0119] Base material: PVA65%
[0120] Sonic velocity regulator: glycerol 29.5%
[0121] Sound attenuation modifier: ZnO 0%
[0122] The proportions of solvent, plasticizer and cross-linking agent are the same as those in Example 1.
[0123] The preparation method is the same as that of Example 1, except that the contents of components added in each step are different, and the step of adding ZnO (ie, the above-mentioned step S4) is omitted.
[0124] Comparative Example 2
[0125] The ultrasonic coupling agent provided in this comparative example 2 contains ZnO, but the content is relatively high, and its components specifically include:
[0126] Base material: PVA45%
[0127] Sonic velocity regulator: 9.5% glycerol
[0128] Sound attenuation modifier: ZnO 40%
[0129] The proportions of solvent, plasticizer and cross-linking agent are the same as those in Example 1.
[0130] The preparation method is the same as that in Example 1, except that the contents of components added in each step are different, which will not be described in detail here.
[0131] Comparative Example 3
[0132] The ultrasonic coupling agent provided in this comparative example 2 contains ZnO, but the content is extremely high, and its components specifically include:
[0133] Base material: PVA40%
[0134] Sonic velocity regulator: 4.5% glycerol
[0135] Sound attenuation modifier: ZnO 50%
[0136] The proportions of solvent, plasticizer and cross-linking agent are the same as those in Example 1.
[0137] The preparation method is the same as that in Example 1, except that the contents of components added in each step are different, which will not be described in detail here.
[0138] The contents of the components in the above Examples 1-3 and Comparative Examples 1-3 are shown in Table 1 below:
[0139] Table 1 Components in Examples 1-3 and Comparative Examples 1-3
[0140] PVA glycerin ZnO water Plasticizers Crosslinking agent Example 1 60% 24.5% 10% 4% 1% 0.5% Example 2 55% 19.5% 20% 4% 1% 0.5% Example 3 50% 14.5% 30% 4% 1% 0.5% Comparative Example 1 65% 29.5% 0 4% 1% 0.5% Comparative Example 2 45% 9.5% 40% 4% 1% 0.5% Comparative Example 3 40% 4.5% 50% 4% 1% 0.5%
[0141] The acoustic properties of the ultrasonic coupling agents with the specified component contents in Table 1 above were tested respectively, and the test results are shown in Table 2 below:
[0142] Table 2 Acoustic properties test results of Examples 1-3 and Comparative Examples 1-3
[0143]
[0144] In the sound velocity test, the sound velocity of comparative example 1 is higher (1600m / s), but the sound attenuation is larger, indicating that in the absence of ZnO, the sound wave propagates fast but attenuates severely. As the ZnO content increases, the sound velocity decreases slightly, but is within a reasonable range.
[0145] In the sound attenuation test, the sound attenuation of Example 1 is the highest (1.50 dB / cm), indicating that the attenuation of sound waves is very serious when there is no ZnO; with the increase of ZnO content, the sound attenuation gradually decreases, indicating that ZnO effectively regulates the attenuation of sound waves; the sound attenuation of Examples 2 and 3 is relatively low, but too high ZnO content may lead to a decrease in other properties.
[0146] In the viscosity test, the viscosity of Comparative Examples 2 and 3 is relatively high and may be difficult to operate; the viscosity of Comparative Example 1 is relatively low, but the sound attenuation performance is poor; the viscosity of Examples 1-3 is moderate and easy to operate and use.
[0147] In the stability test, the stability of Comparative Example 1 is slightly lower, but still within an acceptable range; the stability of Comparative Examples 2 and 3 is relatively low, and stratification or precipitation may occur during storage; Examples 1-3 have the highest stability (level 5), indicating that stratification or precipitation is not easy during storage.
[0148] As can be seen from Table 2 above, ZnO plays a significant role in regulating sound attenuation. As the ZnO content increases, the sound attenuation gradually decreases, but too high a ZnO content will lead to increased viscosity and decreased stability. The embodiment (ZnO 10-30%) exhibits the best comprehensive performance in terms of sound velocity, sound attenuation, viscosity and stability.
[0149] The advantages or beneficial effects of adopting the above technical solution are: the present invention provides a new type of ultrasonic coupling agent as a transmission medium for high-frequency ultrasonic waves, which can effectively improve the penetration ability of ultrasonic waves in various media and reduce attenuation, so as to optimize the quality of ultrasonic imaging.
[0150] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of this specification and illustrations should be included in the protection scope of the present invention.
Claims
1. An ultrasonic coupling agent for enhancing the penetration ability of sound waves and reducing attenuation, characterized in that: include: The polymer base material is 50%-70%, the sound velocity regulator is 10%-30%, the sound attenuation regulator is 10%-30%, the plasticizer is 1%, the cross-linking agent is 0.5%, and the rest is water.
2. The ultrasonic coupling agent for enhancing the sound wave penetration ability and reducing attenuation according to claim 1, characterized in that: The polymer base material includes at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyurethane, polydimethylsiloxane, and polymethyl methacrylate.
3. The ultrasonic coupling agent for enhancing sound wave penetration and reducing attenuation according to claim 1, characterized in that: The sonic velocity regulator includes at least one of glycerol, ethylene glycol, propylene glycol, polyethylene glycol, and vegetable oil.
4. The ultrasonic coupling agent for enhancing sound wave penetration and reducing attenuation according to claim 1, characterized in that: The sound attenuation regulator includes at least one of zinc oxide, titanium oxide, aluminum oxide, carbon nanotubes, graphene oxide, and barium titanate.
5. A method for preparing an ultrasonic coupling agent for enhancing the penetration ability of sound waves and reducing attenuation, characterized in that: include: Step S1, adding 50%-70% of the polymer base material and 10%-30% of the sonic velocity regulator into solvent water, then heating to a preset temperature and continuously stirring to obtain a first mixed solution; Step S2, adding 1% plasticizer to the first mixed solution, and maintaining heating and stirring to obtain a second mixed solution; Step S3, continuously stirring the second mixed solution while it is naturally cooled to room temperature, and adding 0.5% of a cross-linking agent to the second mixed solution cooled to room temperature to obtain a third mixed solution; Step S4, adding 10%-30% of an acoustic attenuation regulator to the third mixed solution to obtain a fourth mixed solution; Step S5, placing the fourth mixed solution into a mold for curing to obtain an ultrasonic coupling agent.
6. The method for preparing an ultrasonic coupling agent for enhancing sound wave penetration and reducing attenuation according to claim 5, characterized in that: In the step S1, the polymer base material includes at least one of polyvinyl alcohol, polyvinyl pyrrolidone, polyurethane, polydimethylsiloxane, and polymethyl methacrylate.
7. The method for preparing an ultrasonic coupling agent for enhancing sound wave penetration and reducing attenuation according to claim 5, characterized in that: In the step S1, the sonic velocity regulator includes at least one of glycerol, ethylene glycol, propylene glycol, polyethylene glycol, and vegetable oil.
8. The method for preparing an ultrasonic coupling agent for enhancing sound wave penetration and reducing attenuation according to claim 5, characterized in that: In the step S1, the preset temperature is 80°C-90°C.
9. The method for preparing an ultrasonic coupling agent for enhancing sound wave penetration and reducing attenuation according to claim 5, characterized in that: In the step S4, the sound attenuation regulator includes at least one of zinc oxide, titanium oxide, aluminum oxide, carbon nanotubes, graphene oxide, and barium titanate.
Citation Information
Cited By
Gastrointestinal ultrasound contrast agent without scattering echoes as well as preparation method and application of gastrointestinal ultrasound contrast agent
CN121796642A
Gastrointestinal ultrasound contrast agent without scattering echo, and preparation method and application thereof
CN121796642B