Hydrogel composite material containing flexible piezoelectric nano generator and preparation method thereof

By combining conductive hydrogel, drug-loaded hydrogel and flexible piezoelectric nanogenerator materials to form a "sandwich" structure hydrogel composite material, the problem of combining electrical stimulation and drug therapy in the treatment of diabetic foot ulcers is solved, achieving It provides wireless self-power and effective wound healing effects, improving patient compliance and safety.

CN118806973APending Publication Date: 2024-10-22NORTHWEST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410668871.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Among existing treatments for diabetic foot ulcers, electrical stimulation therapy suffers from problems such as impaired signal transmission, insufficient antibacterial and anti-inflammatory environment, use of toxic reagents in material preparation, and insufficient patient compliance and safety.

Method used

Using hydrogel composite materials containing flexible piezoelectric nanogenerators, the conductive hydrogel and drug-loaded conductive hydrogel are combined with flexible piezoelectric nanogenerator materials to form a "sandwich" structure to achieve wireless self-powered electricity. Stimulation and medication.

Benefits of technology

The material has good biocompatibility, electrical energy output, antibacterial and mechanical properties, and can effectively promote the healing of diabetic foot ulcers, provide appropriate current and voltage, reduce inflammation, increase tissue oxygenation and blood flow, promote angiogenesis and Cell proliferation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118806973A_ABST
    Figure CN118806973A_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogel composite material containing a flexible piezoelectric nano-generator and a preparation method of the hydrogel composite material. The composite material comprises conductive hydrogel, drug-loaded conductive hydrogel and a flexible piezoelectric nano-generator material arranged between the conductive hydrogel and the drug-loaded conductive hydrogel. The preparation method comprises the step of placing the flexible piezoelectric nano-generator material between conductive hydrogel and drug-loaded hydrogel. The composite material is based on a'sandwich 'structure formed by the flexible piezoelectric nano generator material, the conductive hydrogel and the drug-loaded hydrogel, healing of diabetic foot ulcer can be effectively promoted, and as a wireless self-powered device, the purpose of combining wireless self-powered electrical stimulation therapy and drug therapy can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomaterials, and in particular relates to a hydrogel composite material containing a flexible piezoelectric nanogenerator and a preparation method thereof. Background Art

[0002] Diabetic foot ulcer (DFU) is a common complication of diabetic patients with hyperglycemia, which increases the risk of infection, non-traumatic amputation and even premature death. Electrical stimulation and wound dressings play an important and positive role in the prevention and treatment of DFU. Electrical stimulation (ES) promotes wound healing and tissue regeneration by enhancing intercellular signal transduction, accelerating blood circulation and promoting cell proliferation. However, as an independent therapy, the wound is still in a state of impaired signal transmission, and ES cannot provide the antibacterial and anti-inflammatory environment required for wound repair, and the treatment effect is not satisfactory. Conductive hydrogel dressings have the advantages of providing a conductive medium for cell signal transduction and regulating cell activity and promoting cell adhesion. At present, the combination of drug-loaded conductive hydrogels with external power sources can further promote diabetic wound healing, but external power sources have many limitations. For example, direct current stimulation, which is commonly used in clinical practice, requires high voltage for direct current stimulation of wounds due to the large impedance of human skin, which is harmful to the human body, and patients may not comply with regulations and do not use electrical stimulation treatment regularly in clinics.

[0003] In order to improve patient compliance, researchers have designed a dressing with a piezoelectric-driven triboelectric nanogenerator (PTENG), which uses conductive hydrogel as electrodes for wound healing of diabetic foot. However, during the clinical use of this dressing, wound healing relies more on a single electrical stimulation, and toxic reagents are used in the preparation of the material. The residues of toxic reagents may have adverse effects on the wound.

[0004] In order to meet the current requirements for clinical dressings, dressings based on patients with diabetic foot ulcers need to have the following properties: a) be able to provide ES; b) be easy to use; c) be wearable; d) be non-invasive; e) provide a moist wound environment and be able to deliver drugs to the wound; and f) have properties similar to electronic skin. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a hydrogel composite material containing a flexible piezoelectric nanogenerator and a preparation method thereof in view of the deficiencies of the above-mentioned prior art. The composite material includes a conductive hydrogel and a drug-loaded conductive hydrogel, and a flexible piezoelectric nanogenerator material arranged between the conductive hydrogel and the drug-loaded conductive hydrogel. The composite material is based on a "sandwich" structure formed by the flexible piezoelectric nanogenerator material, the conductive hydrogel and the drug-loaded hydrogel, and can effectively promote the healing of diabetic foot ulcers. As a wireless self-powered device, it can achieve the purpose of combining wireless self-powered electrical stimulation therapy with drug therapy.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a hydrogel composite material containing a flexible piezoelectric nanogenerator, characterized in that it includes a conductive hydrogel and a drug-loaded conductive hydrogel, and a flexible piezoelectric nanogenerator material arranged between the conductive hydrogel and the drug-loaded conductive hydrogel.

[0007] In addition, the present invention also provides a method for preparing the above-mentioned hydrogel composite material containing flexible piezoelectric nanogenerator, which is characterized by comprising:

[0008] Provide flexible piezoelectric nanogenerator materials, conductive hydrogels and drug-loaded hydrogels;

[0009] The flexible piezoelectric nanogenerator material is placed between the conductive hydrogel and the drug-loaded hydrogel.

[0010] The above method is characterized in that the preparation method of the flexible piezoelectric nanogenerator material comprises:

[0011] Step 1: providing barium titanate nanowires, specifically comprising:

[0012] Step 101, adding titanium dioxide powder to a sodium hydroxide aqueous solution, stirring for 10 to 24 hours, to obtain a titanium dioxide-containing system;

[0013] Step 102, reacting the titanium dioxide-containing system at 160-200° C. in a closed environment for 12-24 hours;

[0014] Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed to neutrality, and centrifuged to dry to obtain sodium titanate nanowires;

[0015] Step 104, adding the sodium titanate nanowires to the barium hydroxide aqueous solution, stirring at a speed of 400-600 rpm for 0.5-5 h, sealing, and reacting at 160-240° C. for 60-120 min;

[0016] Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed to neutrality, and centrifuged to dry to obtain barium titanate nanowires;

[0017] Step 2: providing a flexible piezoelectric nanogenerator, specifically including:

[0018] Step 201, placing bacterial cellulose in deionized water, homogenizing, and obtaining a suspension;

[0019] Step 202: Add the barium titanate nanowires to the suspension, stir evenly at a speed of 400-600 rpm, vacuum filter at a vacuum degree of 0.1-10 Pa, and then dry to obtain a flexible piezoelectric nanogenerator material.

[0020] The above method is characterized in that, in step 101, the concentration of titanium dioxide in the titanium dioxide-containing system is 0.01-0.07 g / mL, and the concentration of the sodium hydroxide aqueous solution is 5-12M.

[0021] The above method is characterized in that, in step 104, the concentration of the barium hydroxide aqueous solution is 0.08-0.16M, the mass of the sodium titanate nanowires is 0.002-0.006 times the volume of the barium hydroxide aqueous solution, the unit of the mass of the sodium titanate nanowires is g, and the unit of the volume of the barium hydroxide aqueous solution is mL.

[0022] The above method is characterized in that, in step 202, the mass of the bacterial cellulose is 50 to 250 times the mass of the barium titanate nanowires.

[0023] The above method is characterized in that the conductive hydrogel and the drug-loaded conductive hydrogel are both made of a polyvinyl pyrrolidone-wrapped silver nanowire suspension as a main raw material, and the preparation method of the polyvinyl pyrrolidone-wrapped silver nanowire suspension comprises:

[0024] Step 101, adding the prepared sodium chloride ethylene glycol solution and silver nitrate ethylene glycol solution to the polyvinyl pyrrolidone ethylene glycol solution, stirring at a speed of 300-600 rpm for 10-30 min, sealing, reacting at 120-160° C. for 100-150 min, and reacting at 150-180° C. for 30-60 min;

[0025] Step 102, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed alternately with anhydrous ethanol and deionized water 2 to 3 times;

[0026] Step 103: Disperse the washed solid phase in deionized water to obtain a suspension of silver nanowires coated with polyvinyl pyrrolidone.

[0027] The above method is characterized in that, in step 101, the concentration of the sodium chloride ethylene glycol solution is 0.01-0.03M, the concentration of the silver nitrate ethylene glycol solution is 0.1-0.4M, the concentration of the polyvinyl pyrrolidone ethylene glycol solution is 0.2-0.6M, and the volume ratio of the sodium chloride ethylene glycol solution, the silver nitrate ethylene glycol solution and the polyvinyl pyrrolidone ethylene glycol solution is 1:2:2; in step 103, in the polyvinyl pyrrolidone-coated silver nanowire suspension, the concentration of the polyvinyl pyrrolidone-coated silver nanowire is 10 mg / mL.

[0028] The above method is characterized in that the preparation method of the conductive hydrogel comprises:

[0029] Step 201, dissolving polyvinyl alcohol in deionized water at 90° C. to obtain a polyvinyl alcohol aqueous solution; the concentration of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 0.05 to 0.175 g / mL;

[0030] Step 202, adding the silver nanowire suspension wrapped in polyvinyl pyrrolidone to the polyvinyl alcohol aqueous solution in step 201, stirring to mix; the volume of the silver nanowire suspension wrapped in polyvinyl pyrrolidone is 1 / 4 of the volume of the polyvinyl alcohol aqueous solution;

[0031] Step 203, pour the mixed system in step 202 into a mold, freeze it at -10 to -40°C for 20 to 48 hours, thaw it at room temperature for 3 to 10 hours, repeat the above freezing and thawing cycle 3 to 5 times to obtain a conductive hydrogel.

[0032] The above method is characterized in that the preparation method of the drug-loaded conductive hydrogel comprises:

[0033] Step 201, dissolving polyvinyl alcohol in deionized water at 90° C. to obtain a polyvinyl alcohol aqueous solution; the concentration of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 0.07 to 0.23 g / mL;

[0034] Step 202, sequentially adding the silver nanowire suspension wrapped with polyvinyl pyrrolidone and the ginsenoside Rg3 aqueous solution to the polyvinyl alcohol aqueous solution in step 201, and stirring to make the mixture uniform; the volume of the silver nanowire suspension wrapped with polyvinyl pyrrolidone and the volume of the ginsenoside Rg3 aqueous solution are both 1 / 3 of the volume of the polyvinyl alcohol aqueous solution;

[0035] Step 203, pour the mixed system in step 202 into a mold, freeze it at -10 to -40°C for 20 to 48 hours, thaw it at room temperature for 3 to 10 hours, repeat the above freezing and thawing cycle 3 to 5 times to obtain a conductive hydrogel.

[0036] Compared with the prior art, the present invention has the following advantages:

[0037] 1. The present invention provides a hydrogel composite material containing a flexible piezoelectric nanogenerator, wherein the composite material comprises a conductive hydrogel and a drug-loaded conductive hydrogel, and a flexible piezoelectric nanogenerator material arranged between the conductive hydrogel and the drug-loaded conductive hydrogel. The composite material is based on a "sandwich" structure formed by the flexible piezoelectric nanogenerator material, the conductive hydrogel and the drug-loaded hydrogel, and can effectively promote the healing of diabetic foot ulcers. As a wireless self-powered device, the composite material can achieve the purpose of combining wireless self-powered electrical stimulation therapy with drug therapy.

[0038] 2. The hydrogel composite material containing flexible piezoelectric nanogenerators of the present invention has good biocompatibility, as well as suitable functions such as electrical energy output, conductivity, antibacterial properties, mechanical properties, and promoting cell proliferation and cell migration.

[0039] 3. Preferably, the hydrogel composite material containing a flexible piezoelectric nanogenerator of the present invention includes a conductive hydrogel and a drug-loaded conductive hydrogel arranged on both sides of the flexible piezoelectric nanogenerator. The conductive hydrogel serves as a triboelectric layer and an electrode, and constitutes a piezoelectrically driven triboelectric nanogenerator with the flexible piezoelectric nanogenerator to provide a suitable current and voltage for wound healing. The drug-loaded conductive hydrogel directly contacts the wound, and forms a perfect closed loop with the flexible piezoelectric nanogenerator and the conductive hydrogel, thereby downregulating inflammation, increasing tissue oxygenation, wound blood flow and hemoglobin levels, promoting angiogenesis and fibroblast proliferation, and achieving electrical stimulation and drug treatment of the wound.

[0040] 4. The preparation method of the hydrogel composite material containing flexible piezoelectric nanogenerator of the present invention creatively introduces the flexible piezoelectric nanogenerator and uses it as the core of the "sandwich" structure, which can give full play to its good flexibility and piezoelectric output performance.

[0041] 5. Preferably, in the preparation method of the hydrogel composite material containing flexible piezoelectric nanogenerator of the present invention, the flexible piezoelectric nanogenerator is obtained by stirring and evenly mixing homogenized bacterial cellulose and inorganic nanomaterial barium titanate nanowires, and drying them. The preparation process is reasonable and the raw materials are non-toxic.

[0042] 6. Preferably, in the preparation method of the hydrogel composite material containing flexible piezoelectric nanogenerator of the present invention, the conductive hydrogel and the drug-loaded conductive hydrogel are both prepared with silver nanowires wrapped in polyvinyl pyrrolidone as the main raw material through repeated freezing and thawing, which can effectively utilize the antibacterial, conductive and mechanical properties of the silver nanowires to give the hydrogel composite material good biological properties.

[0043] 7. The preparation method of the hydrogel composite material containing flexible piezoelectric nanogenerators of the present invention has reliable principles and non-toxic raw materials, and is a green process for preparing biological dressings for diabetic foot ulcers.

[0044] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0045] Instruction Manual

[0046] Figure 1 a is a scanning electron microscope image of the barium titanate nanowires of Example 1-2;

[0047] Figure 1 b is a transmission electron microscopy image of the barium titanate nanowires of Example 1-2;

[0048] Figure 1 c is the XRD pattern of barium titanate nanowires in Example 1-2;

[0049] Figure 1 d is the Raman spectrum of the barium titanate nanowires of Example 1-2;

[0050] Figure 2 a is the SEM image of bacterial cellulose in Example 1-2;

[0051] Figure 2 b is the XRD pattern of bacterial cellulose in Example 1-2;

[0052] Figure 2 c is the structural formula of bacterial cellulose in Example 1-2;

[0053] Figure 3 a is the morphology of the flexible piezoelectric nanogenerator material in Example 1-2;

[0054] Figure 3 b is the SEM image of the flexible piezoelectric nanogenerator material of Example 1-2;

[0055] Figure 3 c is the AFM image of the flexible piezoelectric nanogenerator material of Example 1-2;

[0056] Figure 4 a is a SEM image of silver nanowires Ag NWs in Example 3-1;

[0057] Figure 4 b is the TEM image of silver nanowires Ag NWs in Example 3-1;

[0058] Figure 4 c is the XRD pattern of silver nanowires Ag NWs in Example 3-1;

[0059] Figure 5a is the morphology of the conductive hydrogel of Example 3-1;

[0060] Figure 5 b is the SEM image of the conductive hydrogel of Example 3-1;

[0061] Figure 6 The cytotoxicity results of the polyvinyl alcohol hydrogel of Example 2-1, the conductive hydrogel of Example 3-1, and the drug-loaded conductive hydrogel of Example 4-1 on fibroblast L929;

[0062] Figure 7 The mechanical properties test results of the polyvinyl alcohol hydrogel of Example 2-1, the conductive hydrogel of Example 3-1, and the drug-loaded conductive hydrogel of Example 4-1;

[0063] Figure 8 The antibacterial test results of the polyvinyl alcohol hydrogel of Example 2-1, the conductive hydrogel of Example 3-1 and the drug-loaded conductive hydrogel of Example 4-1;

[0064] Fig. 9 These are the electrical energy output results of the sandwich composite structures described in Examples 5-1 to 5-3. DETAILED DESCRIPTION

[0065] Example 1-1

[0066] This embodiment provides a method for preparing a flexible piezoelectric nanogenerator material, comprising:

[0067] Step 1: providing barium titanate nanowires (BaTiO3 NWs), specifically comprising:

[0068] Step 101, adding 1.02 g of titanium dioxide powder to 50 mL of 10 M sodium hydroxide aqueous solution, stirring at room temperature for 12 h to obtain a titanium dioxide-containing system;

[0069] Step 102, reacting the titanium dioxide-containing system at 180° C. in a sealed manner for 18 hours;

[0070] Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed with 3M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain sodium titanate nanowires;

[0071] Step 104, adding 0.15 g of the sodium titanate nanowires to 50 mL of 0.16 M barium hydroxide aqueous solution, stirring at 500 rpm for 30 min, sealing, and reacting at 210° C. for 90 min;

[0072] Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed with 3M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain barium titanate nanowires;

[0073] Step 2: providing a flexible piezoelectric nanogenerator, specifically including:

[0074] Step 201, 5g of bacterial cellulose is placed in 20g of deionized water, and homogenized with a crusher with a power of 400W to obtain a suspension; the mass percentage of bacterial cellulose in the suspension is 20%; the bacterial cellulose is biosynthesized by Acetobacter xylinum, has a crystallinity of 95%, and a degree of polymerization of 2000-8000, and is purchased from Hainan Yide Food Co., Ltd.

[0075] Step 202 , adding 20 mg of the barium titanate nanowires into the above suspension, stirring evenly at a rotation speed of 500 rpm, vacuum filtering at a vacuum degree of 5 Pa, and then drying at 60° C. to obtain a flexible piezoelectric nanogenerator material, recorded as sample 1.

[0076] Example 1-2

[0077] This embodiment provides a method for preparing a flexible piezoelectric nanogenerator material, comprising:

[0078] Step 1: providing barium titanate nanowires (BaTiO3 NWs), specifically comprising:

[0079] Step 101, adding 1.02 g of titanium dioxide powder to 50 mL of 10 M sodium hydroxide aqueous solution, stirring at room temperature for 12 h to obtain a titanium dioxide-containing system; the stirring speed is 500 rpm; the room temperature is 20-25° C.;

[0080] Step 102, reacting the titanium dioxide-containing system at 180° C. in a sealed manner for 18 hours;

[0081] Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed with 3M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain sodium titanate nanowires;

[0082] Step 104, adding 0.15 g of the sodium titanate nanowires to 50 mL of 0.16 M barium hydroxide aqueous solution, stirring at 500 rpm for 30 min, sealing, and reacting at 210° C. for 90 min;

[0083] Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed with 3M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain barium titanate nanowires;

[0084] Step 2: providing a flexible piezoelectric nanogenerator, specifically including:

[0085] Step 201, placing 5 g of bacterial cellulose in 20 g of deionized water, and homogenizing with a crusher with a power of 450 W to obtain a suspension; the mass percentage of bacterial cellulose in the suspension is 20%;

[0086] Step 202 , adding 50 mg of the barium titanate nanowires into the above suspension, stirring evenly at a rotation speed of 500 rpm, vacuum filtering at a vacuum degree of 5 Pa, and then drying at 60° C. to obtain a flexible piezoelectric nanogenerator material, recorded as sample 2.

[0087] Examples 1-3

[0088] This embodiment provides a method for preparing a flexible piezoelectric nanogenerator material, comprising:

[0089] Step 1: providing barium titanate nanowires (BaTiO3 NWs), specifically comprising:

[0090] Step 101, adding 1.02 g of titanium dioxide powder to 50 mL of 10 M sodium hydroxide aqueous solution, stirring at room temperature for 12 h to obtain a titanium dioxide-containing system; the stirring speed is 500 rpm; the room temperature is 20-25° C.;

[0091] Step 102, reacting the titanium dioxide-containing system at 180° C. in a sealed manner for 18 hours;

[0092] Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed with 3M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain sodium titanate nanowires;

[0093] Step 104, adding 0.15 g of the sodium titanate nanowires to 50 mL of 0.16 M barium hydroxide aqueous solution, stirring at 500 rpm for 30 min, sealing, and reacting at 210° C. for 90 min;

[0094] Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed with 3M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain barium titanate nanowires;

[0095] Step 2: providing a flexible piezoelectric nanogenerator, specifically including:

[0096] Step 201, placing 5 g of bacterial cellulose in 20 g of deionized water, and homogenizing with a crusher with a power of 500 W to obtain a suspension; the mass percentage of bacterial cellulose in the suspension is 20%;

[0097] Step 202 , adding 100 mg of the barium titanate nanowires into the above suspension, stirring evenly at a rotation speed of 500 rpm, vacuum filtering at a vacuum degree of 5 Pa, and then drying at 60° C. to obtain a flexible piezoelectric nanogenerator material, recorded as sample 4.

[0098] Examples 1-4

[0099] This embodiment provides a method for preparing a flexible piezoelectric nanogenerator material, comprising:

[0100] Step 101, adding 0.5 g of titanium dioxide powder to 50 mL of 12 M sodium hydroxide aqueous solution, stirring at room temperature for 24 h to obtain a titanium dioxide-containing system; the stirring speed is 500 rpm; the room temperature is 20-25° C.;

[0101] Step 102, reacting the titanium dioxide-containing system at 160° C. in a sealed state for 24 hours;

[0102] Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed with 5M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain sodium titanate nanowires;

[0103] Step 104, adding 0.1 g of the sodium titanate nanowires to 50 mL of 0.10 M barium hydroxide aqueous solution, stirring at 400 rpm for 60 min, sealing, and reacting at 160° C. for 120 min;

[0104] Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed with 5M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain barium titanate nanowires;

[0105] Step 2: providing a flexible piezoelectric nanogenerator, specifically including:

[0106] Step 201, placing 5 g of bacterial cellulose in 20 g of deionized water, and homogenizing with a crusher with a power of 500 W to obtain a suspension; the mass percentage of bacterial cellulose in the suspension is 20%;

[0107] Step 202: Add 20 mg of the barium titanate nanowires into the above suspension, stir evenly at a speed of 400 rpm, vacuum filter at a vacuum degree of 10 Pa, and then dry at 60° C. to obtain a flexible piezoelectric nanogenerator material.

[0108] The material performance and structure of the flexible piezoelectric nanogenerator of this embodiment are basically consistent with those of embodiment 1-1.

[0109] Examples 1-5

[0110] This embodiment provides a method for preparing a flexible piezoelectric nanogenerator material, comprising:

[0111] Step 101, adding 3.5 g of titanium dioxide powder to 50 mL of 5 M sodium hydroxide aqueous solution, stirring at room temperature for 10 h to obtain a titanium dioxide-containing system; the stirring speed is 500 rpm; the room temperature is 20-25° C.;

[0112] Step 102, reacting the titanium dioxide-containing system at 200° C. in a sealed manner for 12 hours;

[0113] Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed with 1M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain sodium titanate nanowires;

[0114] Step 104, adding 0.3 g of the sodium titanate nanowires to 50 mL of 0.08 M barium hydroxide aqueous solution, stirring at 600 rpm for 5 h, sealing, and reacting at 240° C. for 60 min;

[0115] Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed with 1M dilute hydrochloric acid and deionized water until neutral, and centrifuged and dried to obtain barium titanate nanowires;

[0116] Step 2: providing a flexible piezoelectric nanogenerator, specifically including:

[0117] Step 201, placing 5 g of bacterial cellulose in 20 g of deionized water, and homogenizing with a crusher with a power of 400 W to obtain a suspension; the mass percentage of bacterial cellulose in the suspension is 20%;

[0118] Step 202: Add 100 mg of the barium titanate nanowires to the above suspension, stir evenly at a rotation speed of 600 rpm, vacuum filter at a vacuum degree of 0.1 Pa, and then dry at 60° C. to obtain a flexible piezoelectric nanogenerator material.

[0119] The material performance and structure of the flexible piezoelectric nanogenerator of this embodiment are basically consistent with those of embodiments 1-3.

[0120] Example 2-1

[0121] This embodiment provides a method for preparing a hydrogel, which specifically includes:

[0122] Step 1, at 90°C, dissolving 0.5g of polyvinyl alcohol in 5ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89-98KDa;

[0123] Step 2: Pour the polyvinyl alcohol aqueous solution into a mold, freeze it at -20°C for 20 hours, thaw it at room temperature for 4 hours, repeat the above freezing and thawing cycle 4 times to obtain a polyvinyl alcohol hydrogel, which is recorded as sample 4.

[0124] Example 3-1

[0125] This embodiment provides a method for preparing a conductive hydrogel, comprising:

[0126] Step 1: providing hydrophilic silver nanowires (Ag NWs), specifically comprising:

[0127] Step 101, dissolving sodium chloride, silver nitrate and polyvinyl pyrrolidone in ethylene glycol respectively, to obtain a sodium chloride ethylene glycol solution with a concentration of 0.01 M, a silver nitrate ethylene glycol solution with a concentration of 0.1 M and a polyvinyl pyrrolidone ethylene glycol solution with a concentration of 0.3 M respectively; the molecular weight of the polyvinyl pyrrolidone is 1300000;

[0128] Step 102, 5 mL of the sodium chloride ethylene glycol solution prepared in step 1 and 10 mL of the silver nitrate ethylene glycol solution are successively added to 10 mL of the polyvinyl pyrrolidone ethylene glycol solution, stirred at 500 rpm for 20 min, sealed, reacted at 140° C. for 120 min, and then reacted at 150° C. for 30 min;

[0129] Step 103, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed with anhydrous ethanol and deionized water alternately 2 to 3 times;

[0130] Step 104, dispersing the washed solid phase in deionized water to obtain a polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension; in the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension, the concentration of the polyvinyl pyrrolidone-wrapped silver nanowire is 10 mg / mL;

[0131] Step 2: providing a conductive hydrogel, specifically comprising:

[0132] Step 201, at 90° C., dissolving 0.5 g of polyvinyl alcohol in 4 ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89 to 98 KDa;

[0133] Step 202, adding 1 mL of the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension to the polyvinyl alcohol aqueous solution in step 201, and stirring to mix well;

[0134] Step 203, pour the mixed system in step 202 into a mold, freeze it at -20°C for 20 hours, thaw it at room temperature for 4 hours, repeat the above freezing and thawing cycle 4 times to obtain a conductive hydrogel, which is recorded as sample 5.

[0135] Example 3-2

[0136] This embodiment provides a method for preparing a conductive hydrogel, comprising:

[0137] Step 1: providing hydrophilic silver nanowires (Ag NWs), specifically comprising:

[0138] Step 101, dissolving sodium chloride, silver nitrate and polyvinyl pyrrolidone in ethylene glycol respectively, to obtain a 0.02M sodium chloride ethylene glycol solution, a 0.4M silver nitrate ethylene glycol solution and a 0.2M polyvinyl pyrrolidone ethylene glycol solution respectively; the molecular weight of the polyvinyl pyrrolidone is 1300000;

[0139] Step 102, 5 mL of the sodium chloride ethylene glycol solution prepared in step 1 and 10 mL of the silver nitrate ethylene glycol solution are added successively to 10 mL of the polyvinyl pyrrolidone ethylene glycol solution, stirred at 600 rpm for 10 min, sealed, reacted at 160° C. for 100 min, and then reacted at 170° C. for 40 min;

[0140] Step 103, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed with anhydrous ethanol and deionized water alternately 2 to 3 times;

[0141] Step 104, dispersing the washed solid phase in deionized water to obtain a polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension; in the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension, the concentration of the polyvinyl pyrrolidone-wrapped silver nanowire is 10 mg / mL;

[0142] Step 2: providing a conductive hydrogel, specifically comprising:

[0143] Step 201, at 90° C., dissolving 0.2 g of polyvinyl alcohol in 4 ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89 to 98 KDa;

[0144] Step 202, adding 1 mL of the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension to the polyvinyl alcohol aqueous solution in step 201, and stirring to mix well;

[0145] Step 203, pour the mixed system in step 202 into a mold, freeze it at -10°C for 48 hours, thaw it at room temperature for 10 hours, repeat the above freezing and thawing cycle 3 times to obtain a conductive hydrogel.

[0146] The structure and performance of the conductive hydrogel in this embodiment are basically consistent with those in Example 3-1.

[0147] Example 3-3

[0148] This embodiment provides a method for preparing a conductive hydrogel, comprising:

[0149] Step 1: providing hydrophilic silver nanowires (Ag NWs), specifically comprising:

[0150] Step 101, dissolving sodium chloride, silver nitrate and polyvinyl pyrrolidone in ethylene glycol respectively, to obtain a sodium chloride ethylene glycol solution with a concentration of 0.03M, a silver nitrate ethylene glycol solution with a concentration of 0.2M and a polyvinyl pyrrolidone ethylene glycol solution with a concentration of 0.6M respectively; the molecular weight of the polyvinyl pyrrolidone is 1300000;

[0151] Step 102, 5 mL of the sodium chloride ethylene glycol solution prepared in step 1 and 10 mL of the silver nitrate ethylene glycol solution are added successively to 10 mL of the polyvinyl pyrrolidone ethylene glycol solution, stirred at 300 rpm for 30 min, sealed, reacted at 120° C. for 150 min, and then reacted at 180° C. for 60 min;

[0152] Step 103, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed with anhydrous ethanol and deionized water alternately 2 to 3 times;

[0153] Step 104, dispersing the washed solid phase in deionized water to obtain a polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension; in the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension, the concentration of the polyvinyl pyrrolidone-wrapped silver nanowire is 10 mg / mL;

[0154] Step 2: providing a conductive hydrogel, specifically comprising:

[0155] Step 201, at 90° C., dissolving 0.7 g of polyvinyl alcohol in 4 ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89 to 98 KDa;

[0156] Step 202, adding 1 mL of the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension to the polyvinyl alcohol aqueous solution in step 201, and stirring to mix well;

[0157] Step 203, pour the mixed system in step 202 into a mold, freeze it at -40°C for 30 hours, thaw it at room temperature for 3 hours, repeat the above freezing and thawing cycle 5 times to obtain a conductive hydrogel.

[0158] The structure and performance of the conductive hydrogel in this embodiment are basically consistent with those in Example 3-1.

[0159] Example 4-1

[0160] This embodiment provides a method for preparing a drug-loaded conductive hydrogel, comprising:

[0161] Step 1: providing hydrophilic silver nanowires (Ag NWs), specifically comprising:

[0162] Step 101, dissolving sodium chloride, silver nitrate and polyvinyl pyrrolidone in ethylene glycol respectively, to obtain a sodium chloride ethylene glycol solution with a concentration of 0.01 M, a silver nitrate ethylene glycol solution with a concentration of 0.1 M and a polyvinyl pyrrolidone ethylene glycol solution with a concentration of 0.3 M respectively; the molecular weight of the polyvinyl pyrrolidone is 1300000;

[0163] Step 102, 5 mL of the sodium chloride ethylene glycol solution prepared in step 1 and 10 mL of the silver nitrate ethylene glycol solution are successively added to 10 mL of the polyvinyl pyrrolidone ethylene glycol solution, stirred at 500 rpm for 20 min, sealed, reacted at 140° C. for 120 min, and then reacted at 150° C. for 30 min;

[0164] Step 103, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed with anhydrous ethanol and deionized water alternately 2 to 3 times;

[0165] Step 104, dispersing the washed solid phase in deionized water to obtain a polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension; in the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension, the concentration of the polyvinyl pyrrolidone-wrapped silver nanowire is 10 mg / mL;

[0166] Step 2: providing a drug-loaded conductive hydrogel (PVA / Ag NWs / Rg3), specifically comprising:

[0167] Step 201, at 90° C., dissolving 0.5 g of polyvinyl alcohol in 3 ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89 to 98 KDa;

[0168] Step 202, sequentially adding 1 mL of the polyvinyl pyrrolidone-coated silver nanowire (PVP@Ag NWs) suspension and 1 mL of 250 ng / ml ginsenoside Rg3 (S-type) aqueous solution to the polyvinyl alcohol aqueous solution of step 201, and stirring at a speed of 500 rpm to mix evenly; the ginsenoside Rg3 is S-type ginsenoside Rg3 purchased from Juzi Biotechnology;

[0169] Step 203, pour the mixed system in step 202 into a mold, freeze it at -20°C for 20 hours, thaw it at room temperature for 4 hours, repeat the above freezing and thawing cycle 4 times to obtain a drug-loaded conductive hydrogel, which is recorded as sample 6.

[0170] Example 4-2

[0171] This embodiment provides a method for preparing a drug-loaded conductive hydrogel, comprising:

[0172] Step 1: providing hydrophilic silver nanowires (Ag NWs), specifically comprising:

[0173] Step 101, dissolving sodium chloride, silver nitrate and polyvinyl pyrrolidone in ethylene glycol respectively, to obtain a 0.02M sodium chloride ethylene glycol solution, a 0.4M silver nitrate ethylene glycol solution and a 0.2M polyvinyl pyrrolidone ethylene glycol solution respectively; the molecular weight of the polyvinyl pyrrolidone is 1300000;

[0174] Step 102, 5 mL of the sodium chloride ethylene glycol solution prepared in step 1 and 10 mL of the silver nitrate ethylene glycol solution are added successively to 10 mL of the polyvinyl pyrrolidone ethylene glycol solution, stirred at 600 rpm for 10 min, sealed, reacted at 160° C. for 100 min, and then reacted at 170° C. for 40 min;

[0175] Step 103, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed with anhydrous ethanol and deionized water alternately 2 to 3 times;

[0176] Step 104, dispersing the washed solid phase in deionized water to obtain a polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension; in the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension, the concentration of the polyvinyl pyrrolidone-wrapped silver nanowire is 10 mg / mL;

[0177] Step 2: providing a drug-loaded conductive hydrogel (PVA / Ag NWs / Rg3), specifically comprising:

[0178] Step 201, at 90° C., dissolving 0.7 g of polyvinyl alcohol in 3 ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89 to 98 KDa;

[0179] Step 202, sequentially add 1 mL of the polyvinyl pyrrolidone-coated silver nanowire (PVP@Ag NWs) suspension and 1 mL of 250 ng / ml ginsenoside Rg3 (S-type) aqueous solution to the polyvinyl alcohol aqueous solution of step 201, and stir at 500 rpm to mix evenly;

[0180] Step 203, pour the mixed system in step 202 into a mold, freeze it at -40°C for 30 hours, thaw it at room temperature for 3 hours, repeat the above freezing and thawing cycle 3 times to obtain the drug-loaded conductive hydrogel.

[0181] The structure and performance of the drug-loaded conductive hydrogel in this embodiment are basically consistent with those in Example 4-1.

[0182] Example 4-3

[0183] This embodiment provides a method for preparing a drug-loaded conductive hydrogel, comprising:

[0184] Step 1: providing hydrophilic silver nanowires (Ag NWs), specifically comprising:

[0185] Step 101, dissolving sodium chloride, silver nitrate and polyvinyl pyrrolidone in ethylene glycol respectively, to obtain a sodium chloride ethylene glycol solution with a concentration of 0.03M, a silver nitrate ethylene glycol solution with a concentration of 0.2M and a polyvinyl pyrrolidone ethylene glycol solution with a concentration of 0.6M respectively; the molecular weight of the polyvinyl pyrrolidone is 1300000;

[0186] Step 102, 5 mL of the sodium chloride ethylene glycol solution prepared in step 1 and 10 mL of the silver nitrate ethylene glycol solution are added successively to 10 mL of the polyvinyl pyrrolidone ethylene glycol solution, stirred at 300 rpm for 30 min, sealed, reacted at 120° C. for 150 min, and then reacted at 180° C. for 60 min;

[0187] Step 103, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed with anhydrous ethanol and deionized water alternately 2 to 3 times;

[0188] Step 104, dispersing the washed solid phase in deionized water to obtain a polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension; in the polyvinyl pyrrolidone-wrapped silver nanowire (PVP@Ag NWs) suspension, the concentration of the polyvinyl pyrrolidone-wrapped silver nanowire is 10 mg / mL;

[0189] Step 2: providing a drug-loaded conductive hydrogel (PVA / Ag NWs / Rg3), specifically comprising:

[0190] Step 201, at 90° C., dissolving 0.2 g of polyvinyl alcohol in 3 ml of deionized water to obtain a polyvinyl alcohol aqueous solution; the molecular weight of the polyvinyl alcohol is 89 to 98 KDa;

[0191] Step 202, sequentially adding 1 mL of the polyvinyl pyrrolidone-coated silver nanowire (PVP@Ag NWs) suspension and 1 mL of 250 ng / ml ginsenoside Rg3 (S-type) aqueous solution to the polyvinyl alcohol aqueous solution of step 201, and stirring at 500 rpm to mix evenly;

[0192] Step 203, pour the mixed system in step 202 into a mold, freeze it at -10°C for 48 hours, thaw it at room temperature for 10 hours, repeat the above freezing and thawing cycle 5 times to obtain the drug-loaded conductive hydrogel.

[0193] The structure and performance of the drug-loaded conductive hydrogel in this embodiment are basically consistent with those in Example 4-1.

[0194] Example 5-1

[0195] This embodiment provides a material with a "sandwich" composite structure, the raw materials include: the flexible piezoelectric nanogenerator material of embodiment 1-1, the conductive hydrogel of embodiment 3-1 and the drug-loaded conductive hydrogel of embodiment 4-1, and the preparation method of the composite structure material includes:

[0196] The flexible piezoelectric nanogenerator material of Example 1-1 was placed between the conductive hydrogel of Example 3-1 and the drug-loaded conductive hydrogel of Example 4-1 to obtain a material with a "sandwich" composite structure, which was recorded as Sample 7.

[0197] Example 5-2

[0198] This embodiment provides a "sandwich" composite structure material. The raw materials and preparation method are the same as those of Example 5-1, except that the flexible piezoelectric nanogenerator material is the flexible piezoelectric nanogenerator material of Example 1-2, recorded as sample 8.

[0199] Example 5-3

[0200] This embodiment provides a "sandwich" composite structure material, the raw materials and preparation method are the same as those of Example 5-1, the difference being that the flexible piezoelectric nanogenerator material is the flexible piezoelectric nanogenerator material of Example 1-3, recorded as Sample 9.

[0201] Performance Evaluation

[0202] Figure 1 a is a scanning electron microscope image of barium titanate nanowires in Example 1-2, Figure 1 b is a transmission electron microscope image of the barium titanate nanowires of Example 1-2, Figure 1 c is the XRD diagram of barium titanate nanowires in Example 1-2, Figure 1 d is the Raman spectrum of barium titanate nanowires in Example 1-2. Figure 1 a and Figure 1 b As can be seen, barium titanate nanowires were successfully synthesized. Figure 1 c It can be seen that the diffraction peaks of barium titanate nanowires can all be attributed to the BaTiO3 crystal structure, and there is no sign of any crystalline byproducts such as BaCO3 or TiO2. Figure 1 d visible, located at 250cm -1 [A1(TO)], 302cm -1 [E, B1 (TO+LO)], 511cm -1 [E, A1(TO)] and 710cm -1 The peak at [E, A1(LO)] represents the high-voltage tetragonal phase of BaTiO3, indicating that the synthesized barium titanate nanowires have piezoelectric properties.

[0203] Figure 2 a and Figure 2 b are the SEM images and XRD images of bacterial cellulose in Examples 1-2, Figure 2 c is the structural formula of bacterial cellulose. Figure 1 a It can be seen that the raw bacterial cellulose is a gel-like film composed of cellulose nanofibers with a diameter of about 0-30nm. It is flexible and all the nanofibers are gathered together. Figure 1 b It can be seen that the diffraction peaks at 14.2°, 16.5° and 22.5° belong to the diffraction planes (101), (10-1) and (002) of natural cellulose I, respectively, indicating that the bacterial cellulose has crystalline and piezoelectric properties. This shows that the bacterial cellulose of the present invention can be used as a raw material for preparing a flexible piezoelectric nanogenerator.

[0204] Figure 3 a is the morphology of the flexible piezoelectric nanogenerator material in Example 1-2, Figure 3 b is the SEM image of the flexible piezoelectric nanogenerator material of Example 1-2, Figure 3 c is the AFM image of the flexible piezoelectric nanogenerator material of Example 1-2, according to Figure 3 a and 3b show that the structure morphology of the flexible piezoelectric nanogenerator material film in Example 1-2 is complete and uniform, the BaTiO3 nanowires and bacterial cellulose are evenly dispersed, and there is no void in the film. Figure 3 c It can be seen that the flexible piezoelectric nanogenerator material has good roughness and can be used for triboelectric charging.

[0205] Figure 4 a is the SEM image of silver nanowires Ag NWs in Example 3-1, Figure 4 b is the TEM image of silver nanowires AgNWs in Example 3-1, Figure 4 c is the XRD pattern of silver nanowires Ag NWs in Example 3-1. Figure 4 It can be seen that the silver nanowires were successfully synthesized, the wire bundles were uniform, and the silver nanowires were wrapped by a layer of polyvinyl pyrrolidone, which shows that the silver nanowires of the present invention have good water dispersibility, which is conducive to promoting the uniform dispersion of the silver nanowires in the hydrogel. Figure 4 c As can be seen, a strong (111) diffraction peak is observed at 38°, a (200) orientation peak is observed at 44°, and there is no peak corresponding to silver oxide, indicating that the synthesized silver nanowires are pure silver nanowires without other impurities.

[0206] Figure 5 a is the morphology of the conductive hydrogel of Example 3-1, Figure 5 b is the SEM image of the conductive hydrogel in Example 3-1. Figure 5 It can be seen from Figures 5a and 5b that the hydrogel is evenly dispersed and has uniform pores, indicating that the conductive hydrogel obtained by the freeze-thaw method of the present invention has good dispersibility.

[0207] Figure 6 These are the cytotoxicity results of the polyvinyl alcohol hydrogel of Example 2-1, the conductive hydrogel of Example 3-1, and the drug-loaded conductive hydrogel of Example 4-1 on fibroblast L929. The test method comprises: sterilizing the sample, placing 1 g of the sterilized sample in 10 mL of 1640 culture medium (in the 1640 culture medium, the serum mass percentage is 10%, and the double antibody mass percentage is 1%), extracting for 72 hours to obtain an extract, inoculating L929 cells at a density of 104 cells / well in a 96-well plate, incubating in a CO2 incubator for 24 hours, replacing the original culture medium with the extract, replacing the original culture medium with a new culture medium for the control group, continuing to culture for 24 hours, adding 50 μL of MTT to each well, incubating for 3 hours, measuring the absorbance at 490 nm, and calculating the cell survival rate by the following formula: Cell survival rate (%) = [(A sample-A blank) / (A pair-A blank)]×100%, wherein A sample is the absorbance of the sample to be tested, A pair is the absorbance of the control, and A blank is the absorbance of the culture medium. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that sample 4 has no cytotoxicity but also no obvious proliferation effect, indicating that polyvinyl alcohol has good biocompatibility. The cell survival rate of sample 5 decreased, which may be attributed to the low cell toxicity of silver nanowires. Sample 6 cells have a significant effect of promoting L929 cell proliferation, and the reason may be the cell proliferation-promoting effect of ginsenosides.

[0208] Figure 7 The mechanical properties test results of the polyvinyl alcohol hydrogel of Example 2-1, the conductive hydrogel of Example 3-1, and the drug-loaded conductive hydrogel of Example 4-1 are shown. The test method includes: setting the universal material testing machine to a compressive strain of 80% and a rate of 0.5 mm / min, testing a hydrogel with a height of 13 mm and a diameter of 22 mm, and recording the compressive stress and compressive strain. Figure 7 It can be seen that silver nanowires significantly enhanced the mechanical properties of the hydrogel, and the mechanical properties were enhanced with the addition of ginsenosides. This may be because ginsenosides combined with polyvinyl alcohol reduced the hydrogen bonds formed.

[0209] Figure 8 The antibacterial test results of the polyvinyl alcohol hydrogel of Example 2-1, the conductive hydrogel of Example 3-1 and the drug-loaded conductive hydrogel of Example 4-1 are shown in Figure 2. The test method includes: inoculating a single bacterial colony on the LB solid culture medium into the LB liquid culture medium, culturing on a shaker at 37°C and 200 rpm for 12 hours, measuring the absorbance (OD) with an ELISA reader (600 nm), and then diluting the bacterial solution to 1×10 5 The hydrogel and bacterial suspension were co-cultured at 37°C for 24 h, and the absorbance (OD) of the bacterial solution was measured (600 nm) using an enzyme marker, and the bacterial survival rate was calculated using the formula. Figure 8 It can be seen that pure polyvinyl alcohol hydrogel has no antibacterial effect, and the addition of silver nanowires makes the hydrogel have a strong antibacterial effect.

[0210] Fig. 9 The results of the power output of the sandwich composite structure described in Examples 5-1 to 5-3 are shown in the figure. The test method includes: using a linear motor at a frequency of 3HZ and a pressure of 16KPa to study the piezoelectric output performance of the "sandwich" composite hydrogel. Specifically, the "sandwich" composite material is fixed on one side, and a linear motor is used to apply pressure on the other side, and the output voltage and current are recorded using software. Fig. 9 It can be seen that when the flexible piezoelectric nanogenerator material of Example 1-2 is used as the core of the "sandwich" structure, there is an AC voltage of about 200 mV and an AC current of about 70 nA, indicating that the sandwich composite structure of the present invention can effectively promote wound healing.

[0211] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A hydrogel composite material containing a flexible piezoelectric nanogenerator, It is characterized in that The invention comprises a conductive hydrogel, a drug-loaded conductive hydrogel, and a flexible piezoelectric nanogenerator material arranged between the conductive hydrogel and the drug-loaded conductive hydrogel.

2. A method for preparing the hydrogel composite material containing a flexible piezoelectric nanogenerator as claimed in claim 1, It is characterized in that include: Provide flexible piezoelectric nanogenerator materials, conductive hydrogels and drug-loaded hydrogels; The flexible piezoelectric nanogenerator material is placed between the conductive hydrogel and the drug-loaded hydrogel.

3. The method according to claim 2, It is characterized in that The preparation method of the flexible piezoelectric nanogenerator material comprises: Step 1: providing barium titanate nanowires, specifically comprising: Step 101, adding titanium dioxide powder to a sodium hydroxide aqueous solution, stirring for 10 to 24 hours, to obtain a titanium dioxide-containing system; Step 102, reacting the titanium dioxide-containing system at 160-200° C. in a closed environment for 12-24 hours; Step 103, after the reaction, the system is cooled to room temperature, the precipitate is collected, washed to neutrality, and centrifuged to dry to obtain sodium titanate nanowires; Step 104, adding the sodium titanate nanowires to the barium hydroxide aqueous solution, stirring at a speed of 400-600 rpm for 0.5-5 h, sealing, and reacting at 160-240° C. for 60-120 min; Step 105, after the reaction in step 104, the system is cooled to room temperature, the precipitate is collected, washed to neutrality, and centrifuged to dry to obtain barium titanate nanowires; Step 2: providing a flexible piezoelectric nanogenerator, specifically including: Step 201, placing bacterial cellulose in deionized water, homogenizing, and obtaining a suspension; Step 202: Add the barium titanate nanowires to the suspension, stir evenly at a speed of 400-600 rpm, vacuum filter at a vacuum degree of 0.1-10 Pa, and then dry to obtain a flexible piezoelectric nanogenerator material.

4. The method according to claim 3, It is characterized in that In step 101, the concentration of titanium dioxide in the titanium dioxide-containing system is 0.01-0.07 g / mL, and the concentration of the sodium hydroxide aqueous solution is 5-12M.

5. The method according to claim 3, It is characterized in that In step 104, the concentration of the barium hydroxide aqueous solution is 0.08-0.16M, the mass of the sodium titanate nanowires is 0.002-0.006 times the volume of the barium hydroxide aqueous solution, the unit of the mass of the sodium titanate nanowires is g, and the unit of the volume of the barium hydroxide aqueous solution is mL.

6. The method according to claim 3, It is characterized in that In step 202, the mass of the bacterial cellulose is 50 to 250 times the mass of the barium titanate nanowires.

7. The method according to claim 2, It is characterized in that The conductive hydrogel and the drug-loaded conductive hydrogel both use a polyvinyl pyrrolidone-wrapped silver nanowire suspension as a main raw material. The preparation method of the polyvinyl pyrrolidone-wrapped silver nanowire suspension includes: Step 101, adding the prepared sodium chloride ethylene glycol solution and silver nitrate ethylene glycol solution to the polyvinyl pyrrolidone ethylene glycol solution, stirring at a speed of 300-600 rpm for 10-30 min, sealing, reacting at 120-160° C. for 100-150 min, and reacting at 150-180° C. for 30-60 min; Step 102, after the reaction, the system is cooled to room temperature to obtain a solid phase, and the solid phase is first washed with acetone 2 to 3 times, and then washed alternately with anhydrous ethanol and deionized water 2 to 3 times; Step 103: Disperse the washed solid phase in deionized water to obtain a suspension of silver nanowires coated with polyvinyl pyrrolidone.

8. The method according to claim 7, It is characterized in that In step 101, the concentration of the sodium chloride ethylene glycol solution is 0.01-0.03M, the concentration of the silver nitrate ethylene glycol solution is 0.1-0.4M, the concentration of the polyvinyl pyrrolidone ethylene glycol solution is 0.2-0.6M, and the volume ratio of the sodium chloride ethylene glycol solution, the silver nitrate ethylene glycol solution and the polyvinyl pyrrolidone ethylene glycol solution is 1:2:2; in step 103, in the polyvinyl pyrrolidone-coated silver nanowire suspension, the concentration of the polyvinyl pyrrolidone-coated silver nanowires is 10 mg / mL.

9. The method according to claim 7, It is characterized in that The preparation method of the conductive hydrogel comprises: Step 201, dissolving polyvinyl alcohol in deionized water at 90° C. to obtain a polyvinyl alcohol aqueous solution; the concentration of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 0.05 to 0.175 g / mL; Step 202, adding the silver nanowire suspension wrapped in polyvinyl pyrrolidone to the polyvinyl alcohol aqueous solution in step 201, stirring to mix; the volume of the silver nanowire suspension wrapped in polyvinyl pyrrolidone is 1 / 4 of the volume of the polyvinyl alcohol aqueous solution; Step 203, pour the mixed system in step 202 into a mold, freeze it at -10 to -40°C for 20 to 48 hours, thaw it at room temperature for 3 to 10 hours, repeat the above freezing and thawing cycle 3 to 5 times to obtain a conductive hydrogel.

10. The method according to claim 7, It is characterized in that The preparation method of the drug-loaded conductive hydrogel comprises: Step 201, dissolving polyvinyl alcohol in deionized water at 90° C. to obtain a polyvinyl alcohol aqueous solution; the concentration of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 0.07 to 0.23 g / mL; Step 202, sequentially adding the silver nanowire suspension wrapped with polyvinyl pyrrolidone and the ginsenoside Rg3 aqueous solution to the polyvinyl alcohol aqueous solution in step 201, and stirring to make the mixture uniform; the volume of the silver nanowire suspension wrapped with polyvinyl pyrrolidone and the volume of the ginsenoside Rg3 aqueous solution are both 1 / 3 of the volume of the polyvinyl alcohol aqueous solution; Step 203, pour the mixed system in step 202 into a mold, freeze it at -10 to -40°C for 20 to 48 hours, thaw it at room temperature for 3 to 10 hours, repeat the above freezing and thawing cycle 3 to 5 times to obtain a conductive hydrogel.