Lithium battery top cover plate and anti-explosion valve mounting hole forming process thereof
Through the pre-punching and stretching back pier forming process, the problem of insufficient material and poor flatness in the formation of the installation hole for the explosion-proof valve of the lithium battery top cover is solved, achieving better material utilization and product flatness.
Patent Information
- Application Number
- CN202411062400.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
In the existing molding process of the lithium battery top cover sheet and its explosion-proof valve mounting hole, insufficient material makes it difficult to form the convex hull, and the materials on both sides of the explosion-proof valve mounting hole are severely gushed, crushing the edges, and the conflict between the upper and lower forming forces results in product flatness. Poor.
The pre-punching stretch back pier forming process is used. By setting pre-punching holes in the pier pressing position, it provides a material feeding space for the lower concave part to be formed. The remaining material part is removed to form the side wall, and the annular flange is separately pressed to avoid upper and lower forming. The force conflicts, and annular positioning grooves and depressions are formed through multi-step stamping to ensure the formation of the explosion-proof valve installation hole.
It effectively solves the problem of insufficient materials, avoids material surge and crushed edges, improves the flatness of the lithium battery top cover, meets the flange thickness and height requirements, and ensures the correct formation of the explosion-proof valve installation hole.
Smart Images

Figure CN118808449A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of battery manufacturing for new energy vehicles, and specifically to a lithium battery top cover sheet and a forming process for an explosion-proof valve mounting hole thereof. Background Art
[0002] At present, new energy lithium batteries are becoming more and more popular, and have become an important direction for future energy competition. Green energy will also become a key development direction in the future. In order to enhance the market competitiveness of lithium batteries, product accuracy requirements and dimensional consistency requirements have become more stringent. Under the fierce market competition, equipment stability and product consistency have become more important.
[0003] like Fig. 9 The figure shows a lithium battery top cover sheet, which is characterized in that the back of the explosion-proof valve has a bulge with a material thickness exceeding 2mm. However, the molding of such a bulge often has the difficulty of insufficient materials. In order to solve this problem, the existing lithium battery top cover sheet and its explosion-proof valve mounting hole molding process can refer to the lithium battery top cover sheet and its explosion-proof valve mounting hole molding process disclosed in CN114985594B. This process includes the following steps: Step S1: Continuously step-by-step conveying a metal material strip, and punching and forming a lithium battery top cover sheet and a pole hole on it. Step S2: Punching the punching and forming area on the lithium battery top cover sheet to form a closed concave portion. Step S3: Punching the annular side and the closed concave portion to form an annular side wall and pressuring the annular surface to make it sink so that its edge forms an annular side wall, and adjusting the height of the closed concave portion at the same time. Step S4: Punch the annular surface at the upper end of the annular side portion to form an annular depression continuously arranged along the annular side wall, and form a convex ring on the inner edge of the annular depression. At the same time, punch the lower end of the closed lower concave portion to form a concave portion, and form an annular boss according to the inner wall of the concave portion. Step S5: Punch the middle part of the closed lower concave portion to form an explosion-proof valve installation hole and an annular positioning groove, and chamfer the edge of the lithium battery top cover sheet. Step S6: Punch the edges of the pole hole, explosion-proof valve installation hole and injection hole to form chamfers.
[0004] In step S2 of the prior art, when the convex hump on the back is pressed and thickened to form a closed recess, since the interior of the recess is closed and the two sides are open, the material in the recess will preferentially flow to the two sides during the pressing and thickening. There is a serious material surge on both sides of the explosion-proof valve mounting hole, which may cause the risk of crushing the edge and requires a large forming force, resulting in difficulty in material movement. In step S3, the annular side and the closed recess are stamped to form an annular side wall and pressure is applied to the annular surface to make it sink so that an annular side wall is formed at its edge. At the same time, the height of the closed recess is adjusted. Due to the conflict between the upper and lower forming forces and the large deformation of the product in this step, the flatness of the lithium battery top cover sheet is poor. Summary of the invention
[0005] The problem to be solved by the present invention is to provide a lithium battery top cover sheet and a forming process for an explosion-proof valve mounting hole thereof. The pre-punching, stretching and back-forming process of the present invention can be used to form the explosion-proof valve mounting hole, which can effectively solve the difficulty of insufficient materials in the forming of the convex hump, and at the same time avoid the serious gushing of materials on both sides of the explosion-proof valve mounting hole in the prior art, which squeezes and crushes the edge, and due to the conflict between the upper and lower forming forces, the product undergoes large deformation at the same time, resulting in the problem of poor flatness of the lithium battery top cover sheet.
[0006] The technical solution adopted by the present invention to solve the above-mentioned problem is: a lithium battery top cover sheet and its explosion-proof valve installation hole forming process, comprising the following steps:
[0007] Step S1, the metal strip is conveyed in a continuous step-by-step manner in a blanking direction between an upper die and a lower die of a continuous punching die, and a lithium battery top cover sheet, a liquid injection hole 1, a pre-punched hole on the lithium battery top cover sheet and at least one pole hole are punched out on the metal strip during the conveying process;
[0008] Step S2, during the continuous step-by-step conveying process, a concave portion is punched at the outer edge of the pre-punched hole in the punching area of the top cover plate, wherein the concave portion includes an annular flange formed by the extrusion force during punching and a residual material portion at the bottom of the annular flange formed by excess material of the annular flange flowing into the pre-punched hole, and the height of the annular flange is H;
[0009] Step S3, during the continuous step-by-step conveying process of the metal strip, the excess material is punched out to form a first side wall;
[0010] Step S4, during the continuous step-by-step conveying process of the metal strip, the protective side wall is inserted into the first side wall, and the lower end surface of the annular flange is punched to make the height of the annular flange HX;
[0011] Step S5, during the continuous step-by-step conveying process of the metal strip, the upper half end surface of the annular flange is punched to form a first recessed portion, wherein the first recessed portion includes an annular side wall formed by the extrusion force during punching and an annular surface located at the bottom of the annular side wall;
[0012] Step S6, during the continuous step-by-step conveying process of the metal strip, the lower half end surface of the annular flange is punched to form an annular positioning groove, and at the same time, under the extrusion force during punching, the inner edge of the annular surface is raised to form a convex ring, and the outer edge of the annular surface is connected to the convex ring and the annular side wall on both sides to form an annular depression;
[0013] Step S7, during the continuous step-by-step conveying process of the metal strip, the inner wall of the annular flange is punched out to form an explosion-proof valve installation hole, and the lower half of the annular flange serves as a flange at the edge of the explosion-proof valve installation hole.
[0014] Preferably, step S2 also includes forming a pole positioning groove 1: punching and forming a continuously arranged pole positioning groove 1 on the edge of the mouth of the pole hole adjacent to the upper end surface of the lithium battery top cover sheet.
[0015] Preferably, step S4 also includes the forming of the second injection hole and the second pole positioning groove: during the continuous step-by-step conveying process of the metal strip, the edge of the first injection hole is punched out to form the second injection hole, and the edge of the pole hole adjacent to the lower end surface of the lithium battery top cover sheet is punched out to form the second pole positioning groove which is continuously arranged.
[0016] Preferably, step S5 also includes a step of trimming and punching the second injection hole. During the continuous step-by-step conveying process of the metal strip, the second injection hole is trimmed and punched by a injection hole punch.
[0017] Preferably, step S6 also includes a shape chamfering step, in which the metal strip is continuously conveyed in a step-by-step manner, and the edge of the formed lithium battery top cover sheet is punched and chamfered.
[0018] Preferably, after step S7, there is further provided a step S71 of chamfering the explosion-proof valve installation hole, in which the lower edge of the formed explosion-proof valve installation hole is punched and chamfered during the continuous step-by-step conveying process of the metal strip.
[0019] Compared with the prior art, the lithium battery top cover sheet and the explosion-proof valve mounting hole forming process designed by the present invention have the following beneficial effects:
[0020] By adding a pre-punching action in step S1 before the step S2 of forming the back convex hump by piercing and thickening, the pre-punching hole is set in the middle of the piercing position, providing a material flow space for the metal strip when the lower concave portion is formed in step S2, preventing the material from flowing to both sides during the forming process, and removing the excess material formed by the excess material flowing into the pre-punching hole in step S3 to form the first side wall, so as to provide space for the protective side wall to be inserted into the first side wall in step S4, and the annular flange is separately pierced in step S4. The pressure is applied to avoid the conflict between the upper and lower forming forces. The deformation of the product is relatively large, resulting in the problem of poor flatness of the lithium battery top cover sheet. The protective type prevents the material of the annular flange from flowing into the first side wall on the annular flange. Under the action of the punching pressure, the height of the annular flange is HX, and the material is forced to extend only outside the first side wall, which increases the thickness of the annular flange. This prepares the flange for forming and meeting the flange thickness and height requirements in advance. By applying pressure to the annular flange separately in step S4 and applying pressure to the annular flange separately in step S5, The upper end face of the flange is punched to form a first recessed portion, and the annular side portion and the closed lower recessed portion are punched in two steps in the same step in the prior art, which solves the conflict between the upper and lower forming forces generated in the prior art, and the product has a large deformation amount at the same time, which leads to the problem of poor flatness of the lithium battery top cover sheet. The lower end face of the annular flange is punched to form an annular positioning groove through step S6. The forming of the annular positioning groove is mainly used for positioning and fixing the explosion-proof valve protective film. At the same time, under the extrusion force during punching, the inner edge of the annular surface is raised to form a convex ring, and the outer edge of the annular surface is respectively connected to the convex ring and the annular side wall on both sides to form an annular depression. The forming of the annular depression is mainly used for positioning the annular convex portion on the explosion-proof valve to meet the product requirements. The inner wall of the annular flange is punched and removed through step S7 to form an explosion-proof valve mounting hole, and the lower half of the annular flange is used as a flange at the edge of the explosion-proof valve mounting hole, so that the inner wall of the explosion-proof valve mounting hole is perpendicular to the bottom surface of the annular depression and the bottom surface of the annular positioning groove respectively, so as to meet the forming requirements of the explosion-proof valve mounting hole.
[0021] At the same time, in the case of pre-punching, the middle material is pulled up and squeezed to the annular side by a stretching process with a pier extrusion type, so that the thickness of the flange after forming is increased to meet the thickness and height requirements of the flange. When the pier is returned to the thin forming, the material resistance is designed to make the flange full and effectively solve the difficulty of insufficient materials in the forming of the convex hump.
[0022] In addition, the inventors have also experimented with stretching and punching the outer ring of the pre-punched hole on the basis of the pre-punched hole, so as to form the convex hull on the back of the explosion-proof valve. However, because the uneven cut surface at the tear edge left by the pre-punched hole will be left on the convex hull surface during the back-piercing process, a large amount of aluminum powder and aluminum wire will be generated on the convex hull surface after the back-piercing process. Compared with this solution, the uneven cut surface at the tear edge of the present invention is finely blanked and chamfered in step S7 after multiple deformations, avoiding the problem of generating a large amount of aluminum powder and aluminum wire; BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is an overall top view of the present invention;
[0024] Figure 2 It is a cross-sectional view of the metal strip of the present invention located at the sixth forming station;
[0025] Figure 3 It is a cross-sectional view of the metal strip of the present invention located at the seventh forming station;
[0026] Figure 4 It is a cross-sectional view of the metal strip of the present invention located at the eighth forming station;
[0027] Figure 5 It is a cross-sectional view of the metal strip of the present invention located at the ninth forming station;
[0028] Figure 6 It is a cross-sectional view of the metal strip of the present invention located at the tenth forming station;
[0029] Figure 7 It is a cross-sectional view of the metal strip of the present invention located at the eleventh forming station;
[0030] Figure 8 It is a cross-sectional view of the metal strip of the present invention located at the twelveth forming station;
[0031] Fig. 9 It is a schematic diagram of a lithium battery top cover;
[0032] Illustration: 100, metal strip; 101, forming station one; 102, forming station two; 103, forming station three; 104, forming station four; 105, forming station five; 106, forming station six; 107, forming station seven; 108, forming station eight; 109, forming station nine; 110, forming station ten; 111, forming station eleven; 112, forming station twelve; 113, blanking station; 1, lithium battery top cover; 2, guide hole; 3, pre-punching hole; 4, injection hole one; 5, injection hole 2; 6. T-shaped trimming hole; 7. Trimming hole 2; 8. Trimming hole 1; 9. Pole hole; 10. Lower recess; 10.1. Annular flange; 10.2. Residue; 10.2.1. First side wall; 10.3. First recessed portion; 10.3.1. Annular side wall; 10.3.2. Annular surface; 10.4. Protruding ring; 10.5. Annular recess; 10.6. Annular positioning groove; 10.7. Explosion-proof valve mounting hole; 10.8. Flange; 11. Pole positioning groove 1; 12. Pole positioning groove 2; 20. Protective type. DETAILED DESCRIPTION
[0033] Before describing in detail any embodiment of the present invention, it should be understood that the present invention is not limited in its application to the construction and arrangement details of the components described below or illustrated in the following figures. The present invention can have other embodiments and can be practiced or carried out in various ways. In addition, it should be understood that the words and terms used here are for descriptive purposes and should not be considered restrictive. The use of "including" or "having" and its variations herein is intended to cover the items and their equivalents and additional items displayed below. Unless otherwise specified or limited, the terms "install", "connect", "support" and "couple" and their variations are widely used and cover direct installation and indirect installation, connection, support and connection. In addition, "connect" and "couple" are not limited to physical or mechanical connections or connections.
[0034] Furthermore, on the first aspect, in the disclosure of the present invention, the orientation or positional relationship indicated by terms such as "longitudinal", "transverse", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or positional relationship shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore the above terms cannot be understood as limitations on the present invention; on the second aspect, the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" cannot be understood as a limitation on the quantity.
[0035] It should be understood by those skilled in the art that the embodiments of the present invention described above and shown in the accompanying drawings are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.
[0036] The embodiments of the present invention are further described below in conjunction with the accompanying drawings.
[0037] The forming process of the lithium battery top cover sheet and the explosion-proof valve installation hole thereof described in the embodiment adopts a continuous punching die for continuous stamping and punching forming, and the continuous punching die sequentially includes a forming station 101 for forming the guide hole 2, a forming station 2 102 for forming the pre-punching hole 3 and the injection hole 4, a forming station 3 103 for forming the T-shaped trimming hole 6, a forming station 4 104 for forming the trimming hole 7, a forming station 5 105 for forming the trimming hole 8 and the pole hole 9, a forming station 6 106 for forming the lower recess 10 and the pole positioning groove 11, a forming station 7 107 for forming the first side wall 10.2.1, and a forming station 7 108 for forming the injection hole 5 and the pole hole 9. The column positioning groove 2 12 and the forming station 8 108 for punching the lower end surface of the annular flange 10.1, the forming station 9 109 for trimming and punching the injection hole 2 5 and forming the annular side wall 10.3.1 and the annular surface 10.3.2, the forming station 10 110 for punching and forming the bevel chamfer of the edge of the lithium battery top cover sheet 1, and forming the annular positioning groove 10.6, the convex ring 10.4, and the annular depression 10.5, the forming station 11 111 for forming the explosion-proof valve mounting hole 10.7 and the flange 10.8, the forming station 12 112 for punching and forming the bevel chamfer of the lower end edge of the formed explosion-proof valve mounting hole 10.7, and the blanking station 113.
[0038] Thus, the metal strip 100 is punched out according to the above thirteen forming stations to form the lithium battery top cover sheet 1 and its explosion-proof valve mounting hole 10.7, and at the same time, a flange 10.8 that meets the thickness and height requirements is formed at the edge of the explosion-proof valve mounting hole 10.7. The specific forming steps are as follows:
[0039] Step S1, the metal strip 100 is conveyed in a continuous step-by-step manner in the blanking direction between the upper die and the lower die of the continuous punching die, and during the conveying process, the metal strip 100 passes through stations 1 to 5 to punch and form a lithium battery top cover sheet 1, a liquid injection hole 1 4, and a pre-punched hole 3 and at least one pole hole 9 on the lithium battery top cover sheet 1; wherein the pre-punched hole 3 is used to provide a material running space for the metal strip 100 when the lower concave portion 10 is subsequently formed, so as to prevent the material from surging to both sides during the forming process, and the metal strip 100 is an aluminum strip;
[0040] Step S2, during the continuous step-by-step conveying process, the metal strip 100 passes through the forming station 6 106, and a lower concave portion 10 is punched out at the outer edge of the pre-punched hole 3 in the punching area of the lithium battery top cover sheet 1, wherein the lower concave portion 10 includes an annular flange 10.1 formed by the aluminum material being depressed downward under the extrusion force during punching, and a residual material portion 10.2 located at the bottom of the annular flange 10.1 formed by the excess aluminum material of the annular flange 10.1 flowing into the pre-punched hole 3, and the height of the annular flange 10.1 is H; this step also includes the forming of a pole positioning groove 11: a continuously arranged pole positioning groove 11 is punched out on the edge of the mouth of the pole hole 9 adjacent to the upper end face of the lithium battery top cover sheet 1;
[0041] Step S3, during the continuous step-by-step conveying process, the metal strip 100 passes through the seventh forming station 107, and the excess material portion 10.2 is punched out to form a first side wall 10.2.1, the inner wall of which is used for sleeve-mounting the protective mold 20;
[0042] Step S4, during the continuous step-by-step conveying process, the metal strip 100 passes through the forming station eight 108 to insert the side wall of the protective profile 20 into the first side wall 10.2.1, and punches the lower end face of the annular flange 10.1. The protective profile 20 is used to be sleeved in the first side wall 10.2.1. When punching the lower end face of the annular flange 10.1, it prevents the material of the annular flange 10.1 from flowing into the first side wall 10.2.1 on the annular flange 10.1. Under the action of the punching pressure, the height of the annular flange 10.1 is HX, and the material is forced to The material can only extend outward from the first side wall 10.2.1, so as to increase the thickness of the annular flange 10.1, and prepare in advance for the forming of the flange 10.8 and meet the thickness and height requirements of the flange 10.8; this step also includes the forming of the second injection hole 5 and the second pole positioning groove 12; during the continuous step-by-step conveying process of the metal strip 100, the edge of the injection hole 1 4 is punched and the second injection hole 5 is formed, and the edge of the pole hole 9 adjacent to the lower end surface of the lithium battery top cover sheet 1 is punched and formed with a continuously arranged pole positioning groove 12;
[0043] Step S5, during the continuous step-by-step conveying process, the metal strip 100 passes through the forming station 9 109 to punch the upper end surface of the annular flange 10.1 to form a first recessed portion 10.3, wherein the first recessed portion 10.3 includes an annular side wall 10.3.1 that is recessed downward under the extrusion force during the punching process and an annular surface 10.3.2 located at the bottom of the annular side wall 10.3.1; this step also includes a step of trimming and punching the injection hole 2 5, during the continuous step-by-step conveying process, the metal strip 100 uses the injection hole punch to trim and punch the injection hole 2 5;
[0044] Step S6, during the continuous step-by-step conveying process, the metal strip 100 passes through the forming station 110, and the lower end surface of the annular flange 10.1 is punched to form an annular positioning groove 10.6. The forming of the annular positioning groove 10.6 is mainly used for positioning and fixing the explosion-proof valve protective film. At the same time, under the extrusion force during punching, the inner edge of the annular surface 10.3.2 is raised to form a convex ring 10.4, and the outer edge of the annular surface 10.3.2 is connected to the convex ring 10.4 and the annular side wall 10.3.1 on both sides to form an annular depression 10.5. The forming of the annular depression 10.5 is mainly used for positioning the annular convex part on the explosion-proof valve, and the depth of the punched and shaped annular depression 10.5 meets the product requirements;
[0045] Step S6 also includes punching and chamfering the edges of the formed lithium battery top cover sheet 1;
[0046] Step S7, during the continuous step-by-step conveying process, the metal strip 100 passes through the forming station 111, and the inner wall of the annular flange 10.1 is punched out to form the explosion-proof valve installation hole 10.7, and the lower half of the annular flange 10.1 is used as the flange 10.8 at the edge of the explosion-proof valve installation hole 10.7, and the inner wall of the explosion-proof valve installation hole 10.7 is respectively perpendicular to the bottom surface of the annular recess 10.5 and the bottom surface of the annular positioning groove 10.6 to meet the forming requirements of the explosion-proof valve installation hole 10.7; during the continuous step-by-step conveying process, the metal strip 100 passes through the forming station 111, and the inner wall of the explosion-proof valve installation hole 10.7 is punched out to form the explosion-proof valve installation hole 10.7;
[0047] Step S71, passing through the forming station twelve 112, punching and chamfering the lower edge of the formed explosion-proof valve installation hole 10.7, and finally passing through the blanking station 113 to complete the blanking.
[0048] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. All changes made within the scope of protection of the independent claims of the present invention are within the scope of protection of the present invention.
Claims
1. A lithium battery top cover sheet and its explosion-proof valve mounting hole forming process, characterized in that: The steps include: Step S1, the metal strip (100) is conveyed in a continuous step-by-step manner in a blanking direction between an upper die and a lower die of a continuous punching die, and during the conveying process, a lithium battery top cover sheet (1), a liquid injection hole (4), and a pre-punched hole (3) and at least one pole hole (9) on the lithium battery top cover sheet (1) are punched out on the metal strip (100); Step S2, during the continuous step-by-step conveying process, the metal strip (100) is punched to form a concave portion (10) at the outer edge of the pre-punched hole (3) in the punching area of the top cover plate, wherein the concave portion (10) includes an annular flange (10.1) formed by the extrusion force during punching and a residual material portion (10.2) located at the bottom of the annular flange (10.1) formed by excess material of the annular flange (10.1) flowing into the pre-punched hole (3), and the height of the annular flange (10.1) is H; Step S3, during the continuous step-by-step conveying process of the metal strip (100), the excess material portion (10.2) is punched out to form a first side wall (10.2.1); Step S4, during the continuous step-by-step conveying process of the metal strip (100), the side wall of the protective profile (20) is inserted into the first side wall (10.2.1), and the lower end surface of the annular flange (10.1) is punched so that the height of the annular flange (10.1) is HX; Step S5, during the continuous step-by-step conveying process of the metal strip (100), the upper end surface of the annular flange (10.1) is punched to form a first recessed portion (10.3), wherein the first recessed portion (10.3) includes an annular side wall (10.3.1) formed by the extrusion force during punching and an annular surface (10.3.2) located at the bottom of the annular side wall (10.3.1); Step S6, during the continuous step-by-step conveying process of the metal strip (100), the lower end surface of the annular flange (10.1) is punched to form an annular positioning groove (10.6), and at the same time, under the extrusion force during punching, the inner edge of the annular surface (10.3.2) is raised to form a convex ring (10.4), and the outer edge of the annular surface (10.3.2) is respectively connected to the convex ring (10.4) and the annular side wall (10.3.1) to form an annular depression (10.5); Step S7, during the continuous step-by-step conveying process of the metal strip (100), the inner wall of the annular flange (10.1) is punched out to form an explosion-proof valve mounting hole (10.7), and the lower half of the annular flange (10.1) serves as a flange (10.8) at the edge of the explosion-proof valve mounting hole (10.7).
2. The lithium battery top cover sheet and explosion-proof valve mounting hole forming process according to claim 1, characterized in that: Step S2 also includes forming a pole positioning groove one (11): punching out a continuously arranged pole positioning groove one (11) on the edge of the mouth of the pole hole (9) adjacent to the upper end surface of the lithium battery top cover sheet (1).
3. The lithium battery top cover sheet and explosion-proof valve mounting hole forming process according to claim 2, characterized in that: Step S4 also includes the forming of the second injection hole (5) and the second pole positioning groove (12): during the continuous step-by-step conveying process of the metal strip (100), the edge of the first injection hole (4) is punched out to form the second injection hole (5), and the edge of the pole hole (9) adjacent to the lower end surface of the lithium battery top cover sheet (1) is punched out to form the second pole positioning groove (12) which is continuously arranged.
4. The lithium battery top cover sheet and explosion-proof valve mounting hole forming process according to claim 3, characterized in that: Step S5 also includes a step of trimming and punching the second injection hole (5). During the continuous step-by-step conveying process of the metal strip (100), the second injection hole (5) is trimmed and punched using a injection hole punch.
5. The lithium battery top cover sheet and the explosion-proof valve mounting hole forming process according to any one of claims 1 to 4, characterized in that: Step S6 also includes a shape chamfering step, in which the metal strip (100) is continuously conveyed in a stepwise manner, and the edge of the formed lithium battery top cover sheet (1) is punched out to form an inclined chamfer.
6. The lithium battery top cover sheet and explosion-proof valve mounting hole forming process according to claim 5, characterized in that: After step S7, there is also a step S71 of chamfering the explosion-proof valve installation hole (10.7), in which the lower edge of the formed explosion-proof valve installation hole (10.7) is punched and chamfered during the continuous step-by-step conveying process of the metal strip (100).
Citation Information
Patent Citations
Lithium battery top cover plate and anti-explosion valve mounting hole forming process thereof
CN114985594A
Integrated explosion-proof top cover, processing method of integrated explosion-proof top cover and battery
CN116207431A
Making process and mold for punched metal plate piece with stepped section
CN1974049A
Cell -phone fingerprint decoration stamping die
CN206373230U
Method for stamping and integrally molding top cover sheet, battery top cover structure and manufacturing method thereof
US20230256687A1
Cited By
Forming process for integrated top cover plate of explosion-proof valve
CN119141161A
Pressing ring integrated top cover sheet forming device and forming process thereof
CN119927058A
A pressure ring integrated top cover sheet forming device and forming process thereof
CN119927058B