Method for preparing 3D printing substrate by recycling 3D printing residual powder
By screening and hot isostatic pressing of 3D printing residual powder, a 3D printing substrate that meets the requirements is prepared, which solves the problems of insufficient recycling and high cost in the existing technology, and achieves efficient and economical resource recycling and excellent quality. substrate performance.
Patent Information
- Application Number
- CN202410828492.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-22
Smart Images

Figure CN118808631A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of 3D printing, and in particular to a method for recycling 3D printing waste powder to prepare a 3D printing substrate. Background Art
[0002] In metal 3D printing, there are strict requirements for the particle size of metal powder. The powder particle size directly affects the fluidity, spreadability and uniformity of the powder during melting, which in turn affects the quality and performance of the printed parts. A large number of experiments have shown that the powder particle size range in metal 3D printing is generally required to be 15μm to 53μm.
[0003] The current mainstream methods for preparing 3D printing metal powders include: gas atomization, plasma rotating electrode, plasma atomization, radio frequency plasma spheroidization, etc. Powders produced by various processes are not 100% used in the 3D printing production process, and all need to be screened. Powders with a particle size between 15μm and 53μm are used for 3D printing, while powders with a particle size less than 15μm and greater than 53μm cannot be used, resulting in more than 50% waste of resources. At present, the recycling methods for residual powders from 3D printing mainly include: powder remelting, powder ball milling, powder reactivation, etc. However, current recycling methods have problems such as insufficient recycling, high recycling costs, complex recycling processes, and poor performance of recycled products, for example: a) Insufficient recycling: Existing technologies cannot effectively recycle residual powder in all size ranges; b) High recycling costs: The recycling process often requires expensive equipment and energy, resulting in higher costs than directly using new powder; c) Complex recycling processes: The recycling process may involve multiple steps, including cleaning, drying, reactivation, etc., which increases technical difficulty and operational complexity; d) Poor performance of recycled products; The above problems make it difficult to promote and apply existing recycling methods. In fact, most of the 3D printing residual powder is still not fully utilized and is discarded, resulting in a waste of resources.
[0004] In summary, in order to realize the resource utilization of 3D printing waste powder, thereby avoiding resource waste and saving costs, it is very necessary to develop an economically feasible method for recycling 3D printing waste powder. Summary of the invention
[0005] In view of the above analysis, the present invention aims to provide a method for recycling 3D printing waste powder to prepare 3D printing substrates, so as to solve at least one of the problems of insufficient recycling, high cost, complex process, and poor mechanical properties of the recycled products in the prior art of 3D printing waste powder recycling methods.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] The present invention provides a method for recycling 3D printing waste powder to prepare a 3D printing substrate, comprising the following steps:
[0008] S1. The remaining powder from 3D printing is divided into four particle size segments by sieving;
[0009] The first particle size segment: D1>150μm; the second particle size segment: 106μm<D2≤150μm; the third particle size segment: 53μm<D3≤106μm; the fourth particle size segment: D4<15μm; D1, D2, D3, D4 are the powder particle sizes from the first particle size segment to the fourth particle size segment respectively;
[0010] S2, mixing the powders of the four particle size segments uniformly according to the proportions, wherein the proportions calculated by mass percentage are as follows: the first particle size segment accounts for 10% to 20%, the second particle size segment accounts for 20% to 40%, the third particle size segment accounts for 20% to 40%, and the fourth particle size segment accounts for 20% to 30%;
[0011] S3. Put the evenly mixed powder into the bag and compact it to make the packing density ρ f Satisfy: ρ f ≥60%×ρ t , ρ t is the theoretical density of the powder;
[0012] S4, vacuum degassing and sealing the bag filled with powder;
[0013] S5, placing the vacuum degassed and sealed package into a hot isostatic pressing device for hot isostatic pressing to obtain an ingot with a package;
[0014] S6. Forging the ingot with the sheath to obtain a blank, and machining the blank to obtain a 3D printing substrate.
[0015] Furthermore, when the powder is titanium alloy powder, in S2, the first particle size segment accounts for 10% to 12%, the second particle size segment accounts for 35% to 40%, the third particle size segment accounts for 30% to 35%, and the fourth particle size segment accounts for 20% to 25%.
[0016] Furthermore, when the powder is a high-temperature alloy powder, in S2, the first particle size segment accounts for 12% to 15%, the second particle size segment accounts for 24% to 30%, the third particle size segment accounts for 34% to 40%, and the fourth particle size segment accounts for 24% to 30%.
[0017] Furthermore, when the powder is aluminum alloy powder, in S2, the first particle size segment accounts for 10% to 14%, the second particle size segment accounts for 30% to 34%, the third particle size segment accounts for 34% to 38%, and the fourth particle size segment accounts for 22% to 26%.
[0018] Furthermore, the main steps of S2 include: weighing powders of four particle size segments according to the ratio and loading them into a mixer, evacuating the mixture, filling with argon, controlling the mixing time to be 4h to 6h, and the mixer speed to be 12r / min to 20r / min, so that the powders are mixed evenly and prevent oxidation.
[0019] Furthermore, during the vacuum degassing process in S4: the temperature is set to 300° C. to 500° C. and maintained for 2 h to 6 h.
[0020] Further, during the vacuum degassing process described in S4:
[0021] When the powder is titanium alloy powder, the temperature is set to 400℃~450℃ and maintained for 2h~3h; or,
[0022] When the powder is a high temperature alloy powder, the temperature is set to 400℃~500℃ and maintained for 4h~6h; or,
[0023] When the powder is aluminum alloy powder, the temperature is set to 350°C to 400°C and maintained for 5h to 6h.
[0024] Further, when the powder is titanium alloy powder, in S5, the temperature of hot isostatic pressing treatment is 900°C-950°C, the pressure is maintained at 120 MPa or more, and the time is 2h-3h; in S6, the forging temperature is 980°C-1020°C; or,
[0025] When the powder is a high temperature alloy powder, in S5, the temperature of the hot isostatic pressing treatment is 1150°C to 1200°C, the pressure is maintained at 140 MPa or more, and the time is 3h to 4h; in S6, the forging temperature is 1150°C to 1200°C; or,
[0026] When the powder is aluminum alloy powder, in S5, the temperature of hot isostatic pressing treatment is 480℃~520℃, the pressure is maintained at more than 130Mpa, and the time is 2h~3h; in S6, the forging temperature is 400℃~450℃.
[0027] Furthermore, in S6, during the forging process, the forging speed is set to 5 m / s to 8 m / s, and the forging ratio is set to 1.5 to 4.
[0028] Furthermore, in S6, before forging, the ingot with the jacket is heated to a forging temperature and then kept at that temperature for 2 h to 5 h.
[0029] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0030] (1) The present invention provides a method for recycling 3D printing waste powder to prepare a 3D printing substrate. By recycling the waste powder of 3D printing and converting it into a useful substrate, the waste powder that might have been discarded is effectively used to prepare a useful substrate, thereby avoiding waste of resources and industrial waste, achieving cost savings and resource recycling, and being highly consistent with the current concepts of sustainable development and green economy.
[0031] (2) The present invention combines the control of process parameters (such as the particle size distribution and ratio of the powder, the packing density ρ) with the design of a reasonable process path. f ), to obtain a 3D printing substrate with mechanical properties that meet the requirements, overcoming the problem that it is difficult to prepare a qualified 3D printing substrate through existing methods because the particle size distribution of the remaining powder is uneven, there is a lack of powder with an intermediate particle size of 15μm-53μm, and only powder with a particle size that is too large or too small is left.
[0032] (3) The present invention ensures uniform densification of the powder blank during hot isostatic pressing by controlling the particle size distribution, proportion and packing density of the powder, so as to form an ingot with good microstructure uniformity and a density of more than 99%; combined with vacuum degassing and hot isostatic pressing process flow and parameter control, the powder is prevented from undergoing undesirable reactions such as high-temperature oxidation during hot isostatic pressing, effectively improving the density and microstructure uniformity of the ingot obtained by hot isostatic pressing, and providing high-quality billets for subsequent forging and machining; forging with a sheath protects the ingot from oxidation and contamination during the forging process, thereby ensuring the performance and quality of the substrate. The method for preparing a substrate by recycling 3D printing residual powder provided by the present invention realizes nearly 100% recycling and reuse of 3D printing residual powder, has simple process steps, strong operability, does not require expensive and energy-intensive equipment investment, is cost-effective, and is suitable for large-scale production and wide promotion; moreover, the substrate product obtained by the present invention has good thermal stability and quality consistency, and reaches a level comparable to that of a newly purchased substrate in terms of mechanical properties, which can fully meet the performance requirements of 3D printing for substrates and has huge market potential.
[0033] (4) In some preferred embodiments, the present invention can further effectively improve the mechanical properties and microstructural uniformity of the substrate products obtained by hot isostatic pressing and forging by selecting a more preferred powder particle size distribution and ratio for three common 3D printing waste powders, namely, titanium alloy powder, high-temperature alloy powder, and aluminum alloy powder.
[0034] (5) In some preferred embodiments, the present invention helps to ensure uniform mixing and consistency between powder particles and prevent oxidation and contamination in the mixture by selecting preferred mixing parameters (e.g., time, rotation speed) and coordinating preferred mixing equipment and steps such as vacuuming and argon filling, thereby further improving the mechanical properties and microstructural uniformity of the products obtained by hot isostatic pressing and forging, and at the same time, improving mixing efficiency, strong adaptability, and convenient operation.
[0035] (6) In some preferred embodiments, the present invention has a positive effect on improving the mechanical properties and microstructural uniformity of the final substrate product by adopting preferred vacuum degassing parameters (for example, suitable temperature and holding time); further, according to different powder types, more preferred vacuum degassing parameters are selected to ensure the best degassing effect and improve the mechanical properties and microstructural uniformity of the final product.
[0036] (7) In some preferred embodiments, the present invention selects preferred hot isostatic pressing parameters (e.g., temperature, holding pressure, and time) and forging temperature according to different powder types, thereby ensuring optimal hot isostatic pressing and forging strengthening effects and improving the mechanical properties and microstructural uniformity of the final product.
[0037] (8) In some preferred embodiments, the present invention can further improve the mechanical properties and microstructural uniformity of the substrate obtained by recycling 3D printing waste powder by selecting preferred forging parameters (for example: forging speed, forging ratio, and holding time before forging).
[0038] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0040] Figure 1 A schematic diagram of a process for recycling 3D printing waste powder to prepare a 3D printing substrate provided by the present invention;
[0041] Figure 2 This is a metallographic microscope (OM) photograph of the ingot formed by hot isostatic pressing of the TC4 titanium alloy residual powder recovered in Example 1 of the present invention;
[0042] Figure 3This is a scanning electron microscope (SEM) photograph of the recovered Inconel718 nickel-based alloy residual powder after hot isostatic pressing in Example 2 of the present invention. DETAILED DESCRIPTION
[0043] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0044] In metal 3D printing, there are strict requirements on the particle size of metal powder. The particle size range of metal 3D printing is generally required to be 15μm-53μm. After screening the powders produced by various processes, powders with particle sizes less than 15μm and greater than 53μm cannot be used, resulting in more than 50% waste of resources.
[0045] At present, the recycling methods for 3D printing residual powder mainly include: powder remelting, powder ball milling, powder reactivation, etc. These recycling methods have problems such as insufficient recycling, high recycling cost, complex recycling process, and poor performance of recycled products. It is very necessary to develop an economically feasible method for fully recycling 3D printing residual powder.
[0046] Based on this, the present invention provides a method for recycling 3D printing waste powder to prepare a 3D printing substrate, comprising the following steps:
[0047] S1. The remaining powder from 3D printing is divided into four particle size segments by sieving;
[0048] The first particle size segment: D1>150μm; the second particle size segment: 106μm<D2≤150μm; the third particle size segment: 53μm<D3≤106μm; the fourth particle size segment: D4<15μm; D1, D2, D3, D4 are the powder particle sizes from the first particle size segment to the fourth particle size segment respectively;
[0049] S2, mixing the powders of the four particle size segments uniformly according to the proportions, wherein the proportions calculated by mass percentage are as follows: the first particle size segment accounts for 10% to 20%, the second particle size segment accounts for 20% to 40%, the third particle size segment accounts for 20% to 40%, and the fourth particle size segment accounts for 20% to 30%;
[0050] S3. Put the evenly mixed powder into the bag and compact it to make the packing density ρ f Satisfy: ρ f ≥60%×ρ t , ρ t is the theoretical density of the powder;
[0051] S4, vacuum degassing and sealing the bag filled with powder;
[0052] S5, placing the vacuum degassed and sealed package into a hot isostatic pressing device for hot isostatic pressing to obtain an ingot with a package;
[0053] S6. Forging the ingot with the sheath to obtain a blank, and machining the blank to obtain a 3D printing substrate.
[0054] The present invention uses recycled 3D printing residual powder to prepare 3D printing substrates, but because the particle size distribution of the residual powder is uneven, there is a lack of powder with an intermediate particle size of 15μm-53μm, and only coarse powder with excessively large particle sizes at both ends and fine powder with excessively small particle sizes are left. Therefore, in order to use this type of residual powder with non-full particle size distribution to prepare mechanical properties that meet the requirements of 3D printing substrates and ensure product thermal stability and quality consistency, the main technical difficulties that need to be overcome include: how to ensure that the coarse powder and fine powder with large differences in particle size distribution can be tightly combined, and at the same time, the microstructure is uniform. The former (tight combination) can ensure the mechanical properties of the final product, and the latter (uniform organization) can ensure the thermal stability and quality stability / consistency of the substrate. Substrates with uniform microstructures usually have better thermal stability, because the uniform microstructure reduces the stress concentration and defects inside the material, so that it is less likely to deform or damage at high temperatures during the 3D process. At the same time, substrates with uniform microstructures exhibit similar mechanical properties and physical properties at different positions, which helps to ensure the quality stability and consistency of each batch of final products. In addition, substrates with uniform microstructures usually have better mechanical properties.
[0055] Therefore, in order to solve and overcome these technical difficulties, the present invention designs a reasonable process path combined with process parameter control (such as powder particle size distribution and ratio, filling density, etc.) to obtain the mechanical properties of the substrate product that fully meet the requirements of 3D printing, and effectively ensure the thermal stability and quality consistency of the substrate.
[0056] The present invention recycles the remaining powder of 3D printing through the above method, converts it into a useful substrate, effectively utilizes the remaining powder that may have been discarded to prepare a useful substrate, avoids waste of resources and industrial waste, achieves cost savings and resource recycling, and is highly consistent with the current concept of sustainable development and green economy. The present invention ensures the uniform densification of the powder blank during the hot isostatic pressing process by controlling the particle size distribution, proportion and packing density of the powder to form an ingot with good microstructure uniformity and a density of more than 99%; combines vacuum degassing and hot isostatic pressing process flow and parameter control to avoid high-temperature oxidation and other undesirable reactions of the powder during the hot isostatic pressing process, effectively improves the density and microstructure uniformity of the ingot obtained by hot isostatic pressing, and provides high-quality billets for subsequent forging and machining; forging with a sleeve can protect the ingot from oxidation and contamination during the forging process, ensuring the performance and quality of the substrate. The present invention can achieve nearly 100% recycling and reuse of 3D printing residual powder, has simple process steps, strong operability, does not require expensive and energy-intensive equipment investment, is cost-effective, and is suitable for large-scale production and wide promotion; and the obtained substrate product has good thermal stability and quality consistency, and its mechanical properties reach a level comparable to that of a newly purchased substrate, which can fully meet the performance requirements of 3D printing for the substrate and has huge market potential.
[0057] Optionally, the type of powder in step S1 includes but is not limited to titanium alloy powder, high-temperature alloy powder, and aluminum alloy powder; illustratively, the high-temperature alloy powder includes but is not limited to nickel-based high-temperature alloy powder and cobalt-based high-temperature alloy powder.
[0058] Specifically, in step S2, a more preferred powder particle size ratio is selected according to the type of powder. The following are some preferred implementations:
[0059] (a) When the powder is titanium alloy powder, in S2, the first particle size segment accounts for 10% to 12%, the second particle size segment accounts for 35% to 40%, the third particle size segment accounts for 30% to 35%, and the fourth particle size segment accounts for 20% to 25%.
[0060] (b) When the powder is a high temperature alloy powder, in S2, the first particle size segment accounts for 12% to 15%, the second particle size segment accounts for 24% to 30%, the third particle size segment accounts for 34% to 40%, and the fourth particle size segment accounts for 24% to 30%.
[0061] (c) When the powder is aluminum alloy powder, in S2, the first particle size segment accounts for 10% to 14%, the second particle size segment accounts for 30% to 34%, the third particle size segment accounts for 34% to 38%, and the fourth particle size segment accounts for 22% to 26%.
[0062] It should be noted that, through the above preferred particle size distribution and ratio, in the absence of an intermediate particle size segment, the ratio of coarse powder (particle size greater than 53 μm) and fine powder (particle size less than 15 μm) can be accurately separated and adjusted using screening technology to improve the mechanical properties, thermal stability and quality consistency of the products obtained by hot isostatic pressing and forging. Specifically, a) a suitable particle size distribution helps the powder to fill the package more evenly and achieve a better tap density, and also helps to improve the densification uniformity of the powder during hot isostatic pressing, reduce the formation of pores and defects, thereby improving the density and microstructure uniformity of the ingot after hot isostatic pressing, and uniform organization is conducive to improving thermal stability; b) a suitable particle size distribution can also improve the fluidity and deformation uniformity of the ingot during the forging process, reduce defects such as cracks, and thereby improve the mechanical properties of the final substrate product; c) a suitable particle size distribution helps to produce products with consistent performance and reduce performance differences between products.
[0063] Specifically, S1 includes the following steps:
[0064] S1.1. Prepare the sieve:
[0065] Prepare three sieves with pore sizes of 150 μm, 106 μm, and 53 μm respectively.
[0066] S1.2, screening:
[0067] The remaining powder from 3D printing was evenly distributed on a sieve with a pore size of 150 μm, and then sieved using a sieving device so that the powder passed through sieves with pore sizes of 150 μm, 106 μm, and 53 μm in turn.
[0068] S1.3. Collect powders of different particle sizes:
[0069] After the powder passes through the sieve, it will fall into different sieves or receiving containers according to the particle size; collect the powder of each particle size segment. Specifically, the powder left on the 150μm sieve is the powder of the first particle size segment; the powder that passes through the 150μm sieve but is intercepted by the 106μm sieve is the powder of the second particle size segment; the powder that passes through the 106μm sieve but is intercepted by the 53μm sieve is the powder of the third particle size segment; the powder that passes through the 53μm sieve and falls into the receiving container is the powder of the fourth particle size segment.
[0070] Specifically, the main steps of step S2 include: weighing powders of four particle size segments according to the ratio and loading them into a mixer, evacuating the mixture, filling with argon, controlling the mixing time to be 4h to 6h, and the mixer speed to be 12r / min to 20r / min, so that the powders are mixed evenly and prevent oxidation.
[0071] Further, more preferred mixing parameters can be selected according to the type of powder, and the following are some preferred embodiments:
[0072] (a) When the powder is titanium alloy powder: the mixing time is 4h to 5h, and the mixer speed is 15r / min to 16r / min;
[0073] (b) When the powder is a high temperature alloy powder: the mixing time is 4h to 4.5h; the mixer speed is 15r / min to 16r / min;
[0074] (c) When the powder is aluminum alloy powder: the mixing time is 2h to 4h; the mixer speed is 12r / min to 14r / min.
[0075] It can be understood that the use of the above-mentioned preferred mixing time and mixer speed helps to ensure uniform mixing and consistency between powder particles, prevent powder agglomeration, optimize production efficiency, and maintain powder properties.
[0076] Specifically, in step S2, the "vacuuming" means making the pressure in the mixer reach a negative pressure; preferably, the pressure reaches below -0.1 MPa, that is, the pressure in the mixer P ≤ -0.1 MPa.
[0077] Preferably, in step S2, the mixer is at least one of a V-shaped mixer, a double cone mixer or a three-dimensional mixer.
[0078] It should be noted that choosing a suitable mixer is crucial to ensuring the quality and efficiency of powder mixing, and it also helps to improve the mechanical properties, thermal stability and quality consistency of the final product. Choosing a V-type mixer, double cone mixer or three-dimensional mixer for powder mixing has at least the following advantages: (1) High mixing efficiency: These types of mixers are designed to achieve efficient powder mixing, ensuring that powders of different particle sizes can be quickly and evenly mixed; (2) Reduce agglomeration: V-type, double cone and three-dimensional mixers can usually effectively reduce the agglomeration of powder particles, which is crucial to improving the uniformity of the mixed powder and the mechanical properties, thermal stability and quality consistency of the final product; (3) Strong adaptability: These mixers can adapt to powders with different characteristics, including particle size, density and fluidity, thereby meeting the needs of mixing a variety of powders; 4) Easy operation: V-shaped, double cone and three-dimensional mixers are usually designed with easy-to-operate user interfaces, making the mixing process more convenient and controllable; (5) Vacuuming and argon filling functions: In the powder mixing process, vacuuming and argon filling are important steps to remove gas and moisture from the powder and prevent oxidation. These mixers have or are easy to use with vacuum pumps and gas control systems; (6) Reduce pollution: These mixers can be used to mix in a closed environment, reduce the entry of external pollutants, and ensure the purity of the powder; (7) Adjustable mixing parameters: These mixers can accurately control and adjust parameters such as mixing time and speed to achieve the best mixing quality; (8) Suitable for production of different scales: These mixers are available in a variety of specifications and capacities, suitable for different production scales from small batches to large batches.
[0079] Specifically, in step S2, the "weighing powders of four particle size segments according to the ratio" mainly includes the following steps: according to the expected total mass M0 of the mixed powder and the mass ratio of the four required particle size segments, the required mass of the powder of each particle size segment is calculated and weighed.
[0080] It should be noted that the total mass of the powder to be mixed is M0 ≥ M b , M b is the total mass of powder packed in the package.
[0081] It can be understood that to calculate the total mass M of the powder loaded into the package b First, we need to know the packing density of the powder (ρ f ) and theoretical density (ρ t ), and the volume of the package (V). Packing density refers to the actual filling density of the powder in the package, while theoretical density refers to the density of the powder in a completely dense state.
[0082] Specifically, step S3 includes the following steps:
[0083] S3.1. Calculate the minimum value of packing density: According to the condition ρf ≥60%×ρ t , calculate the packing density ρ f Minimum value of: ρ fmin =k×ρ t , 60%≤k≤100%;
[0084] S3.2. Calculate the total mass M of powder to be loaded into the package b :Use the minimum value of packing density and the volume of the bag to calculate the total mass of powder required M b :M b =ρ fmin ×V;
[0085] S3.3. Ensure that the packing density satisfies the condition ρ f ≥60%×ρ t : Weigh a mass of M from the uniformly mixed powder obtained in step S2. b The powder is packed into the bag and compacted to ensure the packing density of the powder f At least reach ρ fmin ;
[0086] S3.4, after the powder is filled, the opening of the package is closed. For example, the upper cover of the package is welded to achieve the closure of the opening.
[0087] Specifically, in step S3, the main step of "compacting" includes: loading the uniformly mixed powder into the bag, and the powder loading process adopts vibration loading to compact the powder in the bag. It can be understood that vibration loading is a method of compacting the powder in the bag by using the principle of mechanical vibration to improve the packing density and uniformity of the powder. The device for implementing vibration loading includes but is not limited to a mechanical vibration table, a pneumatic vibrator, etc.
[0088] Preferably, during the vacuum degassing process described in S4, the temperature is set to 300°C to 500°C, maintained for 2h to 6h, and the vacuum degree reaches 2×10 -3 Below Pa.
[0089] Specifically, in the vacuum degassing process described in S4, more preferred vacuum degassing parameters can be selected according to the type of powder. The following are some preferred implementations:
[0090] When the powder is titanium alloy powder, the temperature is set to 400℃~450℃ and maintained for 2h~3h; or,
[0091] When the powder is a high temperature alloy powder, the temperature is set to 400℃~500℃ and maintained for 4h~6h; or,
[0092] When the powder is aluminum alloy powder, the temperature is set to 350°C to 400°C and maintained for 5h to 6h.
[0093] It is worth noting that the use of the above-mentioned preferred vacuum degassing parameters (such as appropriate temperature and holding time) has a positive effect on improving the mechanical properties, thermal stability and quality consistency of the final product; specifically: (1) Improving the mechanical properties of the product: Vacuum degassing at high temperature can quickly and effectively remove the gas and moisture adsorbed in the powder, preventing the powder from oxidation and corrosion during the hot isostatic pressing process; and it helps to further increase the packing density of the powder, thereby increasing the density of the ingot after hot isostatic pressing and the bonding strength between the powders, thereby improving the mechanical properties of the product; (2) Improving the uniformity of the microstructure to improve the thermal stability and quality consistency of the product: By controlling parameters such as temperature and holding time during the vacuum degassing process, it helps to ensure the uniformity and consistency of the microstructural organization between different ingots after hot isostatic pressing, improve thermal stability, and reduce quality fluctuations of products obtained from different batches.
[0094] Furthermore, according to the different types of powders, more preferred vacuum degassing parameters can be selected to ensure the best degassing effect, improve the mechanical properties, thermal stability and quality consistency of the final product. For example, a) if the temperature is too low or the holding time is too short, the degassing effect is poor, and the gas and moisture in the powder may not be completely removed; b) if the temperature is too high or the holding time is too long, it may cause thermal degradation of the powder particles, affect the chemical properties and performance of the powder, and may also cause sintering or melting of the powder particles, changing the particle size distribution of the powder, all of which will affect the mechanical properties and thermal stability of the final product and cause quality fluctuations.
[0095] Specifically, step S4 includes the following steps:
[0096] S4.1. Place the bag filled with powder and with the opening sealed in a degassing furnace, and connect the vacuum hole on the bag to the vacuum device in the degassing furnace through a vacuum tube;
[0097] S4.2, start the heating system of the degassing furnace and raise the temperature to the required 300℃~500℃;
[0098] S4.3, vacuumize until the pressure inside the package reaches 2×10 -3 Pa below, maintain for 2h to 6h;
[0099] S4.4, after the vacuum degassing is completed, the exhaust holes on the package are sealed to ensure that the interior of the package is in a high vacuum state. Exemplarily, the exhaust holes are sealed by welding.
[0100] Specifically, in steps S5 and S6, the preferred hot isostatic pressing parameters and forging temperature are selected according to the different types of powders to ensure the best hot isostatic pressing and forging strengthening effects, and improve the mechanical properties, thermal stability and quality consistency of the final product. The following are some preferred implementations:
[0101] (a) When the powder is titanium alloy powder, in step S5, the temperature of hot isostatic pressing treatment is 900°C to 950°C, the pressure is maintained at more than 120 MPa, and the time is 2h to 3h; in step S6, the forging temperature is 980°C to 1020°C.
[0102] (b) When the powder is a high-temperature alloy powder, in step S5, the temperature of the hot isostatic pressing treatment is 1150°C to 1200°C, the pressure is maintained at above 140 MPa, and the time is 3h to 4h; in step S6, the forging temperature is 1150°C to 1200°C.
[0103] (c) When the powder is aluminum alloy powder, in step S5, the temperature of hot isostatic pressing treatment is 480°C to 520°C, the pressure is maintained at above 130 MPa, and the time is 2h to 3h; in step S6, the forging temperature is 400°C to 450°C.
[0104] It should be noted that the use of the above-mentioned preferred parameters of hot isostatic pressing (including temperature, pressure and time) with synergistic effects can significantly improve the mechanical properties, thermal stability and quality consistency of the substrate manufactured using 3D printing residual powder; specifically, (1) improving mechanical properties: using appropriate hot isostatic pressing parameters can achieve effective densification, reduce porosity, and improve the mechanical properties and bearing capacity of the substrate, for example, improving the tensile strength, yield strength, elongation, etc. of the substrate; (2) improving microstructural uniformity to improve product thermal stability and quality consistency: using appropriate hot isostatic pressing parameters can help improve the microstructural uniformity of the ingot obtained by hot isostatic pressing treatment. The ingot with good structural uniformity has higher consistency in mechanical properties (such as strength and toughness) at different positions, which reduces the performance differences between products and improves the thermal stability and quality consistency of the product.
[0105] It is understandable that if the parameters of hot isostatic pressing are not set properly, it will affect the mechanical properties, thermal stability and quality consistency of the final substrate product. For example: (a) If the temperature is too low, the pressure is too low or the time is too short, the expected densification effect cannot be achieved, the pores and defects are not effectively eliminated, and the bonding strength between the powder particles is insufficient, which affects the mechanical properties and quality of the final substrate product; (b) If the temperature is too high, the pressure is too high or the time is too long, it may cause excessive grain growth and undesirable phase changes during the hot isostatic pressing process, which will affect the mechanical properties and quality of the final substrate product.
[0106] Specifically, in step S6, before forging, the ingot with the jacket is heated to the forging temperature and then kept warm to ensure that the temperature of the ingot is uniform. Preferably, the temperature is kept warm for 2 hours to 5 hours.
[0107] Preferably, in step S6, during the forging process, the forging speed is set to 5 m / s to 8 m / s, and the forging ratio is 1.5 to 4. The use of the above preferred forging speed and forging ratio is helpful to improve the mechanical properties, thermal stability and quality consistency of the final substrate product.
[0108] Specifically, in step S6, the forging can be performed in an atmospheric environment, because forging with a jacket can effectively reduce oxidation, and no special protective atmosphere is required during the forging process, and the forging can be directly cooled in the air. It can be seen that the method provided by the present invention is simple and easy to implement.
[0109] It should be noted that the use of the above-mentioned preferred forging parameters (including forging speed, forging ratio, and holding time before forging) can significantly improve the mechanical properties, thermal stability, and quality consistency of the substrate manufactured using 3D printing residual powder. Specifically, 1) Improve mechanical properties: The use of appropriate forging parameters helps to obtain the best forging deformation strengthening effect, reduce residual stress, reduce the risk of deformation and cracking, and improve the mechanical properties of the final substrate product, such as strength, toughness, and ductility. 2) Improve microstructural uniformity to improve thermal stability and quality consistency: The use of appropriate forging parameters helps to obtain a blank with a more uniform microstructure. The blank with good organizational uniformity has higher consistency in mechanical properties (such as strength and toughness) at different positions, which reduces the performance differences between products and improves the thermal stability and quality consistency of the product.
[0110] It is understandable that if the forging parameters are not set properly, it will affect the mechanical properties, thermal stability and quality consistency of the final substrate product. For example: a) If the forging speed is too fast, it may lead to uneven temperature distribution inside the material, introduce thermal stress into the material, cause micro cracks, and affect the mechanical properties of the substrate product; if the forging speed is too slow, it may cause local overheating, increase the risk of defects, and slow forging may not be enough to maintain continuous metal flow, resulting in uneven microstructure after forging, affecting thermal stability and causing large differences in product quality; b) If the forging ratio is too large, it may cause greater stress concentration inside the material, increase the risk of crack formation, affect the mechanical properties of the substrate product, and may also cause work hardening on the surface of the material, increasing the difficulty of subsequent processing; if the forging ratio is too small, it is not enough to break the weak interface between the powder particles, and it is impossible to achieve sufficient grain refinement, affecting the mechanical properties of the substrate product, such as strength and toughness.
[0111] It should be noted that in step S6, after forging is completed, the sheath is removed to obtain a blank, and the blank is mechanically processed to obtain a 3D printing substrate. Optionally, the method of removing the sheath includes but is not limited to mechanical methods (such as cutting), pickling, etc.
[0112] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and comparative examples.
[0113] Embodiment 1:
[0114] This embodiment provides a method for recycling TC4 titanium alloy powder remaining from 3D printing to prepare a 3D printing substrate, comprising the following steps:
[0115] S1. The remaining TC4 titanium alloy powder from 3D printing is divided into four particle size segments by sieving;
[0116] Specifically, three sieves are prepared with apertures of 150μm, 106μm, and 53μm, respectively; a sieving machine that can be used to sieving metal powder is prepared, and the TC4 titanium alloy powder remaining from 3D printing is evenly distributed on the sieve with an aperture of 150μm in the sieving machine, and the sieving machine is started to allow the powder to pass through the sieves with apertures of 150μm, 106μm, and 53μm in turn, and powders of four particle size segments are collected from the three sieves and a receiving container, namely, the first particle size segment: D1>150μm; the second particle size segment: 106μm<D2≤150μm; the third particle size segment: 53μm<D3≤106μm; the fourth particle size segment: D4<15μm.
[0117] S2, mixing the powders of the four particle size segments evenly according to the proportions;
[0118] According to the total mass M0 of the expected mixed powder and the mass ratio of the four required particle size segments, the required mass of the powder of each particle size segment is calculated; wherein, M0 = 200Kg; the first particle size segment accounts for 10%, the second particle size segment accounts for 35%, the third particle size segment accounts for 33%, and the fourth particle size segment accounts for 22%; specifically,
[0119] The mass of the powder in the first particle size segment is m1=M0×10%=200Kg×10%=20Kg;
[0120] The mass of the powder in the second particle size range is m2 = M0 × 35% = 200 kg × 35% = 70 kg;
[0121] The mass of the powder in the third particle size range is m3 = M0 × 33% = 200 kg × 33% = 66 kg;
[0122] The mass of the powder in the fourth particle size segment is m4=M0×22%=200Kg×22%=44Kg;
[0123] Furthermore, the corresponding mass of powder is weighed from the powders of the four particle size segments obtained by screening in step S1 and loaded into a V-type mixer, the mixer is evacuated to -0.1 MPa, high-purity argon gas is filled into the mixer, the mixer is started, the mixer speed is set to 15 r / min, and the mixing time is 4 h, so that the powders of each particle size segment are evenly mixed.
[0124] S3, putting the evenly mixed powder into the bag and compacting it;
[0125] The package material is low-carbon steel, and the shape is designed to be a square package with a size of 30cm×30cm×60cm. It is sealed into a cavity by argon arc welding, and the inside is cleaned with alcohol and compressed air;
[0126] According to the packing density of the powder (ρ f ) and theoretical density (ρ t ), and the volume of the package (V), calculate the mass M of powder that needs to be loaded into the package b ;TC4 powder theoretical density ρ t 4.51g / cm 3 , V = 30 × 30 × 60 cm = 54000 cm 3 , M b =ρ fmin ×V=60%×ρ t ×V=60%×4.51g / cm 3×54000cm 3 =146124g, 147Kg of powder needs to be weighed;
[0127] Weigh 147 kg of powder from the uniformly mixed powder in step S2, place the bag on a vibration table, turn on the vibration table, and vibrate while filling the powder until all 147 kg of powder is filled into the bag. At this time, the packing density of the powder is f At least reach ρ fmin =60%×ρ t After the powder is filled, the upper cover of the package is welded closed.
[0128] S4, vacuum degassing and sealing the bag filled with powder;
[0129] The package filled with powder and sealed with an upper cover is placed in a degassing furnace, and the vacuum hole on the package is connected to the vacuum device in the degassing furnace through a vacuum tube;
[0130] Start the heating system of the degassing furnace and raise the temperature to 420°C;
[0131] Start the vacuum device in the degassing furnace and evacuate until the pressure inside the bag reaches 2×10 -3 Pa, maintained for 2.5h;
[0132] After the vacuum degassing is completed, the exhaust holes on the package are sealed and welded to ensure that the inside of the package is in a high vacuum state.
[0133] S5. Hot isostatic pressing: put the vacuum degassed and sealed package into the hot isostatic pressing equipment, set the hot isostatic pressing temperature to 930°C and the pressure to 120 MPa. After the temperature and pressure reach the set values, keep them for 2.5 hours and perform hot isostatic pressing to obtain an ingot with a package;
[0134] S6, forging and machining to obtain a TC4 titanium alloy substrate for 3D printing;
[0135] Forging: the ingot with the jacket obtained after hot isostatic pressing was placed in a heating furnace, heated to 1000°C and kept warm for 2 hours, then the ingot was taken out and forged by free forging in an atmospheric environment. The forging speed was set to 6 m / s and the forging ratio was 1.7 to obtain a rectangular blank with a size of 630 mm × 630 mm × 80 mm;
[0136] Processing: The forged blank is processed into a TC4 substrate of 614mm×614mm×75mm as required, and put into 3D printing equipment for use as a printing substrate.
[0137] In the method provided in this embodiment, the relative density of the TC4 ingot after hot isostatic pressing is greater than 99%, the microstructure is uniform, the grains in the structure are fine, and there are no defects such as cracks and holes. Figure 2 As shown; the TC4 ingot with uniform microstructure exhibits similar mechanical and physical properties at different locations, which helps to ensure the stability and consistency of the quality of the final product in each batch while improving thermal stability.
[0138] In the method provided in this embodiment, the mechanical properties of the TC4 ingot after hot isostatic pressing are already good. After further forging strengthening, the mechanical properties of the final substrate product reach a level comparable to that of the newly purchased TC4 titanium alloy substrate, as shown in Table 1.
[0139] Table 1: Mechanical properties of TC4 titanium alloy residual powder during the preparation of substrate
[0140]
[0141]
[0142] Embodiment 2:
[0143] This embodiment provides a method for recycling Inconel718 nickel-based high-temperature alloy powder remaining from 3D printing to prepare a 3D printing substrate, comprising the following steps:
[0144] S1. The remaining Inconel718 nickel-based high-temperature alloy powder from 3D printing is divided into four particle size segments by sieving;
[0145] Specifically, three sieves are prepared with apertures of 150μm, 106μm, and 53μm, respectively; a sieving machine that can be used to sieve metal powder is prepared, and the remaining Inconel718 alloy powder from 3D printing is evenly distributed on the sieve with an aperture of 150μm in the sieving machine, and the sieving machine is started to allow the powder to pass through the sieves with apertures of 150μm, 106μm, and 53μm in turn, and powders of four particle size segments are collected from the three sieves and a receiving container, namely, the first particle size segment: D1>150μm; the second particle size segment: 106μm<D2≤150μm; the third particle size segment: 53μm<D3≤106μm; the fourth particle size segment: D4<15μm.
[0146] S2, mixing the powders of the four particle size segments evenly according to the proportions;
[0147] According to the total mass M0 of the expected mixed powder and the mass ratio of the four required particle size segments, the required mass of the powder of each particle size segment is calculated; wherein, M0 = 100Kg; the first particle size segment accounts for 13.5%, the second particle size segment accounts for 26.5%, the third particle size segment accounts for 34%, and the fourth particle size segment accounts for 26%; specifically,
[0148] The mass of the powder in the first particle size range is m1 = M0 × 13.5% = 100 kg × 13.5% = 13.5 kg;
[0149] The mass of the powder in the second particle size range is m2 = M0 × 26.5% = 100 kg × 26.5% = 26.5 kg;
[0150] The mass of the powder in the third particle size range is m3=M0×34%=100Kg×34%=34.0Kg;
[0151] The mass of the powder in the fourth particle size segment is m4=M0×26%=100Kg×26%=26.0Kg;
[0152] Furthermore, corresponding masses of powders were weighed from the powders of the four particle size segments obtained by sieving in step S1 and loaded into a three-dimensional mixer. The mixer was evacuated to -0.1 MPa, high-purity argon was filled into the mixer, the mixer was started, the mixer speed was set to 16 r / min, and the mixing time was 4.5 h, so that the powders of each particle size segment were evenly mixed.
[0153] S3, putting the evenly mixed powder into the bag and compacting it;
[0154] The package material is stainless steel, and the shape is designed to be a square package with a size of 20cm×20cm×40cm. It is sealed into a cavity by argon arc welding, and the inside is cleaned with alcohol and compressed air;
[0155] According to the packing density of the powder (ρ f) and theoretical density (ρ t ), and the volume of the package (V), calculate the mass M of powder that needs to be loaded into the package b ; Theoretical density of Inconel718 nickel-based powder ρ t 8.24g / cm 3 , the volume of the package V = 20cm × 20cm × 40cm = 16000cm 3 , M b =ρ fmin ×V=68%×ρ t ×V=68%×8.24g / cm 3 ×16000cm 3 =89651g, 90Kg of powder needs to be weighed;
[0156] Weigh 90 kg of powder from the uniformly mixed powder in step S2, place the bag on a vibration table, turn on the vibration table, and vibrate while filling the powder until all 90 kg of powder is filled into the bag. At this time, the powder packing density ρ f At least reach ρ fmin =68%×ρ t After the powder is filled, the upper cover of the package is welded closed.
[0157] S4, vacuum degassing and sealing the bag filled with powder;
[0158] The package filled with powder and sealed with an upper cover is placed in a degassing furnace, and the vacuum hole on the package is connected to the vacuum device in the degassing furnace through a vacuum tube;
[0159] Start the heating system of the degassing furnace and raise the temperature to 450°C;
[0160] Start the vacuum device in the degassing furnace and evacuate until the pressure inside the bag reaches 1×10 -3 Pa, maintained for 5 hours;
[0161] After the vacuum degassing is completed, the exhaust holes on the package are sealed and welded to ensure that the inside of the package is in a high vacuum state.
[0162] S5, hot isostatic pressing: put the vacuum degassed and sealed package into the hot isostatic pressing equipment, set the hot isostatic pressing temperature to 1170°C, and the pressure to 140Mpa. After the temperature and pressure reach the set values, keep them for 3.5 hours, and perform hot isostatic pressing to obtain an ingot with a package;
[0163] S6, forging and machining to obtain an Inconel718 nickel-based high-temperature alloy substrate for 3D printing;
[0164] Forging: the ingot with the jacket after hot isostatic pressing is placed in a heating furnace, heated to 1170°C, and kept warm for 3 hours. The ingot is then taken out and forged by free forging in an atmospheric environment. The forging speed is set to 7 m / s and the forging ratio is 2.0 to obtain a rectangular blank with a size of 450 mm × 450 mm × 40 mm.
[0165] Processing: The forged blank is processed into an Inconel718 nickel-based high-temperature alloy substrate of 421mm×421mm×30mm as required, and put into 3D printing equipment for use as a printing substrate.
[0166] In the method provided in this embodiment, the relative density of the Inconel718 ingot after hot isostatic pressing is greater than 99%, the microstructure is uniform, the grains in the structure are fine, and there are no defects such as cracks and holes. Figure 3 As shown; the Inconel718 ingot with uniform microstructure exhibits similar mechanical and physical properties at different locations, which helps to ensure the stability and consistency of the quality of each batch of final products while improving thermal stability.
[0167] In the method provided in this embodiment, the mechanical properties of the Inconel718 ingot after hot isostatic pressing are already good. After further forging strengthening, the mechanical properties of the final substrate product reach a level comparable to that of the newly purchased Inconel718 nickel-based alloy substrate, as shown in Table 2.
[0168] Table 2: Mechanical properties of Inconel718 nickel-based high-temperature alloy residual powder during the preparation of substrates
[0169]
[0170] Embodiment 3:
[0171] This embodiment provides a method for recycling 6061 aluminum alloy powder remaining from 3D printing to prepare a 3D printing substrate, comprising the following steps:
[0172] S1. The remaining 6061 aluminum alloy powder from 3D printing is divided into four particle size segments by sieving;
[0173] Specifically, three sieves are prepared with apertures of 150μm, 106μm, and 53μm, respectively; a sieving machine that can be used to sieving metal powder is prepared, and the remaining 6061 aluminum alloy powder from 3D printing is evenly distributed on the sieve with an aperture of 150μm in the sieving machine, and the sieving machine is started to allow the powder to pass through the sieves with apertures of 150μm, 106μm, and 53μm in turn, and powders of four particle size segments are collected from the three sieves and a receiving container, namely, the first particle size segment: D1>150μm; the second particle size segment: 106μm<D2≤150μm; the third particle size segment: 53μm<D3≤106μm; the fourth particle size segment: D4<15μm.
[0174] S2, mixing the powders of the four particle size segments evenly according to the proportions;
[0175] According to the total mass M0 of the expected mixed powder and the mass ratio of the four required particle size segments, the required mass of the powder of each particle size segment is calculated; wherein, M0 = 100 kg; the first particle size segment accounts for 10%, the second particle size segment accounts for 30%, the third particle size segment accounts for 34%, and the fourth particle size segment accounts for 26%;
[0176] The mass of the powder in the first particle size segment m1 = M0 × 10% = 100 Kg × 10% = 10.0 Kg;
[0177] The mass of the powder in the second particle size range is m2 = M0 × 30% = 100 kg × 30% = 30.0 kg;
[0178] The mass of the powder in the third particle size range is m3=M0×34%=100Kg×34%=34.0Kg;
[0179] The mass of the powder in the fourth particle size segment is m4=M0×26%=100Kg×26%=26.0Kg;
[0180] Furthermore, the corresponding mass of powder is weighed from the powders of the four particle size segments obtained by sieving in step S1 and loaded into a double-cone mixer. The mixer is evacuated to -0.1 MPa, high-purity argon gas is filled into the mixer, the mixer is started, the mixer speed is set to 13 r / min, and the mixing time is 3.0 h, so that the powders of each particle size segment are evenly mixed.
[0181] S3, putting the evenly mixed powder into the bag and compacting it;
[0182] The package material is aluminum alloy, and the shape is designed to be a square package with a size of 30cm×30cm×36cm. It is sealed into a cavity by argon arc welding, and the inside is cleaned with alcohol and compressed air;
[0183] According to the packing density of the powder (ρ f ) and theoretical density (ρ t), and the volume of the package (V), calculate the mass M of powder loaded into the package b ; 6061 powder theoretical density ρ t 2.68g / cm 3 , V = 30 × 30 × 36 cm = 32400 cm 3 , M b =ρ fmin ×V=70%×ρ t ×V=70%×2.68g / cm 3×32400cm 3 =60782g, 61Kg of powder needs to be weighed;
[0184] Weigh 61 kg of powder from the uniformly mixed powder in step S2, place the bag on a vibration table, turn on the vibration table, and vibrate while filling the powder until all 61 kg of powder is filled into the bag. At this time, the packing density of the powder is f At least reach ρ fmin =70%×ρ t After the powder is filled, the upper cover of the package is welded closed.
[0185] S4, vacuum degassing and sealing the bag filled with powder;
[0186] The package filled with powder and sealed with an upper cover is placed in a degassing furnace, and the vacuum hole on the package is connected to the vacuum device in the degassing furnace through a vacuum tube;
[0187] Start the heating system of the degassing furnace and raise the temperature to 370°C;
[0188] Start the vacuum device in the degassing furnace and evacuate until the pressure inside the bag reaches 1×10 -3 Pa, maintained for 5.5h;
[0189] After the vacuum degassing is completed, the exhaust holes on the package are sealed and welded to ensure that the inside of the package is in a high vacuum state.
[0190] S5. Hot isostatic pressing: put the vacuum degassed and sealed package into the hot isostatic pressing equipment, set the hot isostatic pressing temperature to 500°C and the pressure to 130 MPa. After the temperature and pressure reach the set values, keep them for 2.5 hours and perform hot isostatic pressing to obtain an ingot with a package;
[0191] S6, forging and machining to obtain a 6061 aluminum alloy substrate for 3D printing;
[0192] Forging: the ingot with the jacket after hot isostatic pressing was placed in a heating furnace, heated to 420°C, and kept warm for 4 hours. The ingot was then taken out and forged by free forging in an atmospheric environment. The forging speed was set to 6 m / s, and the forging ratio was 4.0 to obtain a rectangular blank with a size of 450 mm × 450 mm × 40 mm.
[0193] Processing: The forged blank is processed into a 6061 aluminum alloy substrate of 421mm×421mm×30mm as required, and put into 3D printing equipment for use as a printing substrate.
[0194] In the method provided in this embodiment, the relative density of the 6061 ingot after hot isostatic pressing is greater than 99%, the microstructure is uniform, the grains in the structure are fine, and there are no defects such as cracks and holes; the 6061 ingot with uniform microstructure exhibits similar mechanical properties and physical properties at different positions, which helps to ensure the quality stability and consistency of each batch of final products, while improving thermal stability.
[0195] In the method provided in this embodiment, the mechanical properties of the 6061 ingot after hot isostatic pressing are already good, and after further forging strengthening and heat treatment, the mechanical properties of the final substrate product reach a level comparable to that of the newly purchased 6061 aluminum alloy substrate, as shown in Table 3. The heat treatment can adopt the heat treatment process applicable to aluminum alloys (such as 6061 aluminum alloy) in the prior art, for example, T6 (solution heat treatment followed by artificial aging), firstly performing solution heat treatment: the temperature is 500°C, maintained for 1 hour; rapidly cooling to room temperature; and then performing artificial aging treatment: the temperature is 160°C, maintained for 7 hours.
[0196] Table 3: Mechanical properties of 6061 aluminum alloy residual powder during the preparation of substrate
[0197]
[0198] Comparative Example 1:
[0199] The difference between this comparative example and Example 1 is that in step S2, the first particle size segment accounts for 8%, the second particle size segment accounts for 37%, the third particle size segment accounts for 33%, and the fourth particle size segment accounts for 22%;
[0200] The remaining steps and parameters are the same as those in Example 1.
[0201] Since this comparative example does not adopt the preferred particle size distribution and ratio provided by the present invention (the first particle size segment accounts for 10% to 20%), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 830 MPa, a yield strength of 736 MPa, and an elongation of 8%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0202] Comparative Example 2:
[0203] The difference between this comparative example and Example 1 is that in step S2, the first particle size segment accounts for 20%, the second particle size segment accounts for 18%, the third particle size segment accounts for 37%, and the fourth particle size segment accounts for 25%;
[0204] The remaining steps and parameters are the same as those in Example 1.
[0205] Since this comparative example does not adopt the preferred particle size distribution and ratio provided by the present invention (the second particle size segment does not adopt 20% to 40%), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 825 MPa, a yield strength of 742 MPa, and an elongation of 9%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0206] Comparative Example 3:
[0207] The difference between this comparative example and Example 1 is that in step S2, the first particle size segment accounts for 13%, the second particle size segment accounts for 20%, the third particle size segment accounts for 42%, and the fourth particle size segment accounts for 25%;
[0208] The remaining steps and parameters are the same as those in Example 1.
[0209] Since this comparative example does not adopt the preferred particle size distribution and ratio provided by the present invention (the third particle size segment does not adopt 20% to 40%), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 837 MPa, a yield strength of 745 MPa, and an elongation of 8.5%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0210] Comparative Example 4:
[0211] The difference between this comparative example and Example 1 is that in step S2, the first particle size segment accounts for 13%, the second particle size segment accounts for 20%, the third particle size segment accounts for 35%, and the fourth particle size segment accounts for 32%;
[0212] The remaining steps and parameters are the same as those in Example 1.
[0213] Since this comparative example does not adopt the preferred particle size distribution and ratio provided by the present invention (the fourth particle size segment does not adopt 20% to 30%), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 839 MPa, a yield strength of 748 MPa, and an elongation of 10%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0214] Comparative Example 5:
[0215] The difference between this comparative example and Example 1 is that in step S2, the first particle size segment accounts for 14%, the second particle size segment accounts for 35%, the third particle size segment accounts for 30%, and the fourth particle size segment accounts for 21%;
[0216] The remaining steps and parameters are the same as those in Example 1.
[0217] Since this comparative example does not adopt the more preferred particle size distribution and ratio for titanium alloy powder provided by the present invention (i.e., the first particle size segment accounts for 10% to 12%, the second particle size segment accounts for 35% to 40%, the third particle size segment accounts for 30% to 35%, and the fourth particle size segment accounts for 20% to 25%), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 850 MPa, a yield strength of 752 MPa, and an elongation of 11.5%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0218] Comparative Example 6:
[0219] The difference between this comparative example and Example 2 is that in step S2, the first particle size segment accounts for 12%, the second particle size segment accounts for 22%, the third particle size segment accounts for 40%, and the fourth particle size segment accounts for 26%;
[0220] The remaining steps and parameters are the same as those in Example 2.
[0221] Since this comparative example does not adopt the more preferred particle size distribution and ratio for high-temperature alloy powder provided by the present invention (i.e., the first particle size segment accounts for 12% to 15%, the second particle size segment accounts for 24% to 30%, the third particle size segment accounts for 34% to 40%, and the fourth particle size segment accounts for 24% to 30%), the tensile strength of the Inconel718 alloy substrate obtained in this comparative example is 1242 MPa, the yield strength is 950 MPa, and the elongation is 11%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 2 of the present invention.
[0222] Comparative Example 7:
[0223] The difference between this comparative example and Example 3 is that in step S2, the first particle size segment accounts for 12%, the second particle size segment accounts for 28%, the third particle size segment accounts for 34%, and the fourth particle size segment accounts for 26%;
[0224] The remaining steps and parameters are the same as those in Example 3.
[0225] Since this comparative example does not adopt the more preferred particle size distribution and ratio for aluminum alloy powder provided by the present invention (i.e., the first particle size segment accounts for 10% to 14%, the second particle size segment accounts for 30% to 34%, the third particle size segment accounts for 34% to 38%, and the fourth particle size segment accounts for 22% to 26%), the aluminum alloy substrate obtained in this comparative example has a tensile strength of 310 MPa, a yield strength of 240 MPa, and an elongation of 12%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 3 of the present invention.
[0226] Comparative Example 8:
[0227] The difference between this comparative example and Example 1 is that in step S3, the mass of powder to be loaded into the bag is M b =ρ fmin ×V=55%×ρ t ×V=55%×4.51g / cm 3 ×54000cm 3 = 133947 g, weigh 134 kg of powder from the powder mixed in step S2, place the bag on a vibration table, turn on the vibration table, fill the powder while vibrating until all 134 kg of powder is filled into the bag, stop vibrating, and the powder packing density ρ f =55%×ρ t ;
[0228] The remaining steps and parameters are the same as those in Example 1.
[0229] Since this comparative example does not adopt the preferred packing density conditions provided by the present invention (i.e., packing density ρ f Satisfy: ρ f ≥60%×ρ t , ρ t is the theoretical density of the powder), therefore, the tensile strength of the TC4 titanium alloy substrate obtained in this comparative example is 829 MPa, the yield strength is 738 MPa, and the elongation is 12%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0230] Comparative Example 9:
[0231] The difference between this comparative example and Example 1 is that in step S2, the mixing time is 3.5 h;
[0232] The remaining steps and parameters are the same as those in Example 1.
[0233] Since this comparative example does not adopt the preferred mixing time in S2 provided by the present invention (i.e., the mixing time is 4h to 6h), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 838Mpa, a yield strength of 740Mpa, and an elongation of 11%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0234] Comparative Example 10:
[0235] The difference between this comparative example and Example 1 is that in step S2, the mixer speed is set to 9 r / min;
[0236] The remaining steps and parameters are the same as those in Example 1.
[0237] Since this comparative example does not adopt the preferred mixer speed in S2 provided by the present invention (i.e., the mixer speed is 12r / min to 20r / min), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 845Mpa, a yield strength of 750Mpa, and an elongation of 13%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0238] Comparative Example 11:
[0239] The difference between this comparative example and Example 1 is that in step S4, the heating system of the degassing furnace is started and the temperature is raised to 250°C;
[0240] The remaining steps and parameters are the same as those in Example 1.
[0241] Since this comparative example does not adopt the preferred vacuum degassing temperature in step S4 provided by the present invention (that is, during the vacuum degassing process in S4: the temperature is set to 300°C ~ 500°C), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 837 MPa, a yield strength of 740 MPa, and an elongation of 9%. The mechanical properties of the substrate obtained in this comparative example are not as good as the mechanical properties of the substrate in Example 1 of the present invention.
[0242] Comparative Example 12:
[0243] The difference between this comparative example and Example 1 is that in step S4, the vacuuming device in the degassing furnace is started to evacuate the bag until the pressure inside the bag reaches 2×10 -3 Pa, maintain for 1h;
[0244] The remaining steps and parameters are the same as those in Example 1.
[0245] Since this comparative example does not adopt the preferred vacuum degassing time in step S4 provided by the present invention (i.e., during the vacuum degassing process described in S4: maintaining for 2h to 6h), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 827Mpa, a yield strength of 734Mpa, and an elongation of 8%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0246] Comparative Example 13:
[0247] The difference between this comparative example and Example 1 is that in step S6, the forging speed is set to 4 m / s;
[0248] The remaining steps and parameters are the same as those in Example 1.
[0249] Since this comparative example does not adopt the preferred forging speed in step S6 provided by the present invention (that is, in S6, during the forging process, the forging speed is set to 5m / s to 8m / s), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 858Mpa, a yield strength of 752Mpa, and an elongation of 12%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0250] Comparative Example 14:
[0251] The difference between this comparative example and Example 1 is that in step S6, the forging speed is set to 10 m / s;
[0252] The remaining steps and parameters are the same as those in Example 1.
[0253] Since this comparative example does not adopt the preferred forging speed in step S6 provided by the present invention (that is, in S6, during the forging process, the forging speed is set to 5m / s to 8m / s), the TC4 titanium alloy substrate obtained in this comparative example has a tensile strength of 825Mpa, a yield strength of 751Mpa, and an elongation of 11.5%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0254] Comparative Example 15:
[0255] The difference between this comparative example and Example 1 is that in step S6, the forging ratio is 1.3, and a rectangular blank with a size of 620 mm×620 mm×108 mm is obtained;
[0256] The remaining steps and parameters are the same as those in Example 1.
[0257] Since this comparative example does not adopt the preferred forging ratio in step S6 provided by the present invention (that is, in S6, during the forging process, the forging ratio is 1.5-4), the TC4 titanium alloy substrate obtained by forging in this comparative example has a tensile strength of 821 MPa, a yield strength of 747 MPa, and an elongation of 11%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 1 of the present invention.
[0258] Comparative Example 16:
[0259] The difference between this comparative example and Example 3 is that in step S6, the forging ratio is 4.5, and a rectangular blank with a size of 441 mm×441 mm×37 mm is obtained;
[0260] The remaining steps and parameters are the same as those in Example 3.
[0261] Since this comparative example does not adopt the preferred forging ratio in step S6 provided by the present invention (that is, in S6, during the forging process, the forging ratio is 1.5-4), the aluminum alloy substrate obtained by forging in this comparative example has a tensile strength of 321 MPa, a yield strength of 264 MPa, and an elongation of 13%. The mechanical properties of the substrate obtained in this comparative example are not as good as those of the substrate in Example 3 of the present invention.
[0262] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for recycling 3D printing waste powder to prepare a 3D printing substrate, characterized in that: The following steps are involved: S1. The remaining powder from 3D printing is divided into four particle size segments by sieving; The first particle size segment: D1>150μm; The second particle size range: 106μm<D2≤150μm; the third particle size range: 53μm<D3≤106μm; the fourth particle size range: D4<15μm; D1, D2, D3, D4 are the powder particle sizes from the first particle size range to the fourth particle size range respectively; S2, mixing the powders of the four particle size segments uniformly according to the proportions, wherein the proportions calculated by mass percentage are as follows: the first particle size segment accounts for 10% to 20%, the second particle size segment accounts for 20% to 40%, the third particle size segment accounts for 20% to 40%, and the fourth particle size segment accounts for 20% to 30%; S3. Put the evenly mixed powder into the bag and compact it to make the packing density ρ f Satisfy: ρ f ≥60%×ρ t , ρ t is the theoretical density of the powder; S4, vacuum degassing and sealing the bag filled with powder; S5, placing the vacuum degassed and sealed package into a hot isostatic pressing device for hot isostatic pressing to obtain an ingot with a package; S6. Forging the ingot with the sheath to obtain a blank, and machining the blank to obtain a 3D printing substrate.
2. The method according to claim 1, characterized in that When the powder is titanium alloy powder, in S2, the first particle size segment accounts for 10% to 12%, the second particle size segment accounts for 35% to 40%, the third particle size segment accounts for 30% to 35%, and the fourth particle size segment accounts for 20% to 25%.
3. The method according to claim 1, characterized in that When the powder is a high temperature alloy powder, in S2, the first particle size segment accounts for 12% to 15%, the second particle size segment accounts for 24% to 30%, the third particle size segment accounts for 34% to 40%, and the fourth particle size segment accounts for 24% to 30%.
4. The method according to claim 1, characterized in that: When the powder is aluminum alloy powder, in S2, the first particle size segment accounts for 10% to 14%, the second particle size segment accounts for 30% to 34%, the third particle size segment accounts for 34% to 38%, and the fourth particle size segment accounts for 22% to 26%.
5. The method according to claim 1, characterized in that The main steps of S2 include: weighing powders of four particle size segments according to the ratio and loading them into the mixer, evacuating the mixture, filling with argon, controlling the mixing time to 4h to 6h, and the mixer speed to 12r / min to 20r / min, so that the powders are mixed evenly and prevent oxidation.
6. The method according to claim 1, characterized in that During the vacuum degassing process described in S4: the temperature is set to 300° C. to 500° C. and maintained for 2 h to 6 h.
7. The method according to claim 6, characterized in that During the vacuum degassing process described in S4: When the powder is titanium alloy powder, the temperature is set to 400°C to 450°C and maintained for 2h to 3h; or, When the powder is a high temperature alloy powder, the temperature is set to 400°C to 500°C and maintained for 4h to 6h; or, When the powder is aluminum alloy powder, the temperature is set to 350° C. to 400° C. and maintained for 5 h to 6 h.
8. The method according to claim 1, characterized in that When the powder is titanium alloy powder, in S5, the temperature of the hot isostatic pressing treatment is 900°C to 950°C, the pressure is maintained at 120 MPa or more, and the time is 2h to 3h; in S6, the forging temperature is 980°C to 1020°C; or, When the powder is a high temperature alloy powder, in S5, the temperature of the hot isostatic pressing treatment is 1150°C to 1200°C, the pressure is maintained at 140 MPa or more, and the time is 3h to 4h; in S6, the temperature of the forging is 1150°C to 1200°C; or, When the powder is aluminum alloy powder, in S5, the temperature of the hot isostatic pressing treatment is 480°C to 520°C, the pressure is maintained at more than 130 MPa, and the time is 2h to 3h; in S6, the forging temperature is 400°C to 450°C.
9. The method according to claim 1, characterized in that: In S6, during the forging process, the forging speed is set to 5 m / s to 8 m / s, and the forging ratio is set to 1.5 to 4.
10. The method according to claim 1, characterized in that In S6, before the forging, the ingot with the jacket is heated to the forging temperature and then kept at the temperature for 2 hours to 5 hours.
Citation Information
Cited By
Method for recycling and reusing 3D printing substrate at low cost
CN120828136A