Steel spade production process

Through continuous stamping and multi-step heat treatment, the problems of cumbersome processes and difficult shape control in the production of steel shovels are solved, production efficiency and product quality are improved, and the performance of the steel shovels is enhanced.

CN118809095APending Publication Date: 2024-10-22TANGSHAN TENGFEI HARDWARE TOOLS MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411069439.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The production process of steel shovels is cumbersome and the shape of the blank is difficult to control, resulting in low production efficiency and reduced quality requirements.

Method used

The manganese steel plate is stamped into a blank using a continuous stamping machine mold, and then subjected to high-temperature quenching treatment, stamped into the shovel body and handle tube structures respectively, followed by cooling, tempering and pickling, and finally the handle and handle tube are fixedly connected. , forming the finished steel shovel.

Benefits of technology

It reduces the phenomenon of multiple forging presses, improves processing efficiency, enhances the hardness and toughness of the steel shovel, reduces internal stress, removes oxide films and rust, and improves performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809095A_ABST
    Figure CN118809095A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of steel spade production, and particularly discloses a steel spade production process which comprises the following steps: (1) uncoiling and leveling a manganese steel coil; (2) the leveled manganese steel is subjected to punch forming to form a blank piece; (3) sharpening the circumferential edge of the shovel body of the blank; (4) the blanks are sequentially put into a quenching furnace to be subjected to high-temperature heating treatment; (5) carrying out punch forming on the shovel body; (6) carrying out punch forming treatment on the handle tube to form a finished product of the steel spade; (7) the finished steel spade is rapidly cooled; (8) the cooled finished steel spade is subjected to tempering treatment; and (9) the finished steel spade cooled in the step (8) is put into an acid pickling solution to be treated. According to the steel spade machining process, the phenomenon of tedious procedures during steel spade machining is avoided, the machining quality requirement and the use performance can be guaranteed, and therefore the machining efficiency of the process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel shovel production, and in particular to a steel shovel production process. Background Art

[0002] Steel shovel is also called iron shovel. It is a farm tool that can be used for tilling land and shoveling soil. Its long handle is mostly made of wood, and the head is made of iron. It can also be used in the military. At present, the production process of steel shovel is usually to first stamp the steel plate into a T-shaped structure, and then heat the T-shaped structure at high temperature. After heating, it is repeatedly forged into the shape of a blank on the corresponding forging machine, and then the two ends of the blank are stamped into the structure of the shovel body and the handle tube, and finally the pre-processed handle and the handle tube are fixedly connected.

[0003] The above-mentioned operation production process has complicated procedures, the shape of the blank is difficult to control during the forging process, and deformation is prone to occur. The production efficiency is low and the labor intensity is high, which reduces the production efficiency and quality requirements for the steel shovel. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the above technical defects and propose a steel shovel production process that can improve production efficiency and product quality.

[0005] In order to solve the above problem, the technical solution of the present invention is: a steel shovel production process, which includes the following steps: (1) placing a manganese steel coil on a support frame of an uncoiling machine, uncoiling it, and then passing the uncoiling manganese steel end through a flattening machine for flattening;

[0006] (2) placing the flattened end of the manganese steel into a continuous stamping machine die, and stamping the manganese steel into a plurality of blanks;

[0007] (3) sharpening the circumferential edge of the shovel body of each blank, and then punching rivet holes at designated positions on the handle tube;

[0008] (4) placing the plurality of blanks processed in step (3) in turn into a quenching furnace with a conveying function for high-temperature heating treatment;

[0009] (5) Then, the heated blank is placed into a shovel body stamping machine through a special fixture, and the shovel body of the blank is stamped and formed;

[0010] (6) placing the blank processed in step (5) into a handle tube stamping machine through a special fixture, and performing stamping and forming on the handle tube of the blank to form it into a finished steel shovel;

[0011] (7) placing the finished steel shovel after the treatment in step (6) into a cooling device for cooling;

[0012] (8) After cooling, the finished steel shovel is placed in a tempering furnace for low-temperature heating treatment, and then cooled again after heating treatment;

[0013] (9) placing the finished steel shovel after cooling in step (8) into a pickling solution for immersion treatment, and after the treatment is completed, taking it out for drying;

[0014] (10) The finished steel shovel after drying is fixedly connected through the handle tube and the pre-processed handle.

[0015] Furthermore, in step (4), the temperature at which the blank is heated is 900-1100°C.

[0016] Furthermore, in step (8), the temperature at which the finished steel shovel is heated is 500-600°C.

[0017] Furthermore, in step (9), the finished steel shovel is immersed in the acid solution for 15-25 minutes.

[0018] After adopting the above process, the present invention has the following advantages: first, a continuous stamping machine mold is used to stamp the steel plate into a blank, and then the blank is subjected to high-temperature quenching treatment, and then the two ends of the heated blank are respectively stamped into the structure of a shovel body and a handle tube to form it into a finished steel shovel, and then it is cooled, and then the finished steel shovel is tempered and cooled, and finally the finished steel shovel is placed in a pickling solution for treatment; through the process of stamping the steel plate into a blank at one time, not only the phenomenon of repeated forging of steel parts and the cumbersomeness of processing are reduced, but also the quality requirements of the steel plate shape can be guaranteed, thereby improving the processing efficiency of the present process, the hardness and toughness of the finished steel shovel can be improved through quenching treatment, the internal stress generated during quenching can be reduced through tempering treatment, and the requirements for flexibility and elasticity can be improved, and the oxide film and rust on the surface of the finished steel shovel can be removed through pickling treatment, thereby improving the performance requirements of the present process. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a structural diagram of the blank in the present invention. DETAILED DESCRIPTION

[0020] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0021] Embodiment 1

[0022] like Figure 1 As shown, a steel shovel production process includes the following steps: (1) placing a manganese steel coil on a support frame of an uncoiling machine, uncoiling it, and then passing the uncoiling manganese steel end through a flattening machine for flattening;

[0023] (2) placing the flattened end of the manganese steel into a continuous stamping machine die, and stamping the manganese steel into a plurality of blanks;

[0024] (3) sharpening the circumferential edge of the shovel body of each blank, and then punching rivet holes at designated positions on the handle tube;

[0025] (4) placing the plurality of blanks processed in step (3) in turn into a quenching furnace with a conveying function for high-temperature heating treatment;

[0026] (5) Then, the heated blank is placed into a shovel body stamping machine through a special fixture, and the shovel body of the blank is stamped and formed;

[0027] (6) placing the blank processed in step (5) into a handle tube stamping machine through a special fixture, and performing stamping and forming on the handle tube of the blank to form it into a finished steel shovel;

[0028] (7) placing the finished steel shovel after the treatment in step (6) into a cooling device for cooling;

[0029] (8) After cooling, the finished steel shovel is placed in a tempering furnace for low-temperature heating treatment, and then cooled again after heating treatment;

[0030] (9) placing the finished steel shovel after cooling in step (8) into a pickling solution for immersion treatment, and after the treatment is completed, taking it out for drying;

[0031] (10) The finished steel shovel after drying is fixedly connected through the handle tube and the pre-processed handle.

[0032] In this embodiment, the temperature at which the blank is heated in step (4) is 900°C.

[0033] In this embodiment, the temperature at which the finished steel shovel is heated in step (8) is 500°C.

[0034] In this embodiment, the finished steel shovel is immersed in the acid solution for 15 minutes in step (9).

[0035] Embodiment 2

[0036] like Figure 1 As shown, a steel shovel production process includes the following steps: (1) placing a manganese steel coil on a support frame of an uncoiling machine, uncoiling it, and then passing the uncoiling manganese steel end through a flattening machine for flattening;

[0037] (2) placing the flattened end of the manganese steel into a continuous stamping machine die, and stamping the manganese steel into a plurality of blanks;

[0038] (3) sharpening the circumferential edge of the shovel body of each blank, and then punching rivet holes at designated positions on the handle tube;

[0039] (4) placing the plurality of blanks processed in step (3) in turn into a quenching furnace with a conveying function for high-temperature heating treatment;

[0040] (5) Then, the heated blank is placed into a shovel body stamping machine through a special fixture, and the shovel body of the blank is stamped and formed;

[0041] (6) placing the blank processed in step (5) into a handle tube stamping machine through a special fixture, and performing stamping and forming on the handle tube of the blank to form it into a finished steel shovel;

[0042] (7) placing the finished steel shovel after the treatment in step (6) into a cooling device for cooling;

[0043] (8) After cooling, the finished steel shovel is placed in a tempering furnace for low-temperature heating treatment, and then cooled again after heating treatment;

[0044] (9) placing the finished steel shovel after cooling in step (8) into a pickling solution for immersion treatment, and after the treatment is completed, taking it out for drying;

[0045] (10) The finished steel shovel after drying is fixedly connected through the handle tube and the pre-processed handle.

[0046] In this embodiment, the temperature at which the blank is heated in step (4) is 1100°C.

[0047] In this embodiment, the temperature at which the finished steel shovel is heated in step (8) is 600°C.

[0048] In this embodiment, the finished steel shovel is immersed in the acid solution for 25 minutes in step (9).

[0049] The working principle of the present invention is as follows: first, a continuous stamping machine mold is used to continuously stamp the steel plate into multiple blanks, and then the multiple blanks are distributedly subjected to high-temperature quenching treatment, and then the two ends of the heated blank are respectively stamped into the structure of a shovel body and a handle tube to form it into a finished steel shovel, and then a cooling treatment is performed, and then the cooled finished steel shovel is subjected to low-temperature tempering and cooling treatment, and finally the finished steel shovel is placed in a pickling solution for treatment; through the process of stamping the steel plate into a blank at one time, not only the phenomenon of repeated forging of steel parts and the cumbersomeness of processing are reduced, but also the quality requirements of the shape of the steel plate can be guaranteed, thereby improving the processing efficiency of the present process, the hardness and toughness of the finished steel shovel can be improved through quenching treatment, the internal stress generated during quenching can be reduced through tempering treatment, and the requirements for flexibility and elasticity can be improved, and the oxide film and rust on the surface of the finished steel shovel can be removed through pickling treatment, thereby improving the performance requirements of the present process.

[0050] The present invention and its implementation methods are described above, and such description is not restrictive, and the actual structure is not limited thereto. In general, if a person skilled in the art is inspired by it, and does not deviate from the purpose of the invention, and does not creatively design a structure and implementation method similar to the technical solution, they should all fall within the protection scope of the present invention.

Claims

1. A steel shovel production process, characterized in that: It includes the following steps: (1) Place the manganese steel coil on the support frame of the uncoiler and perform uncoil operation on it, and then pass the uncoiled manganese steel end through the flattening machine for flattening; (2) placing the flattened end of the manganese steel into a continuous stamping machine die, and stamping the manganese steel into a plurality of blanks; (3) sharpening the circumferential edge of the shovel body of each blank, and then punching rivet holes at designated positions on the handle tube; (4) placing the plurality of blanks processed in step (3) in turn into a quenching furnace with a conveying function for high-temperature heating treatment; (5) Then, the heated blank is placed into a shovel body stamping machine through a special fixture, and the shovel body of the blank is stamped and formed; (6) placing the blank processed in step (5) into a handle tube stamping machine through a special fixture, and performing stamping and forming on the handle tube of the blank to form it into a finished steel shovel; (7) placing the finished steel shovel after the treatment in step (6) into a cooling device for cooling; (8) After cooling, the finished steel shovel is placed in a tempering furnace for low-temperature heating treatment, and then cooled again after heating treatment; (9) placing the finished steel shovel after cooling in step (8) into a pickling solution for immersion treatment, and after the treatment is completed, taking it out for drying; (10) The finished steel shovel after drying is fixedly connected through the handle tube and the pre-processed handle.

2. A steel shovel production process according to claim 1, characterized in that: In step (4), the temperature at which the blank is heated is 900-1100°C.

3. A steel shovel production process according to claim 1, characterized in that: The temperature at which the finished steel shovel is heated in step (8) is 500-600°C.

4. A steel shovel production process according to claim 1, characterized in that: In step (9), the finished steel shovel is immersed in the acid solution for 15-25 minutes.

Citation Information

Patent Citations

  • Technology for manufacturing steel spade based on continuous cold-punched die

    CN108994205A

  • Production process of non-oxidation steel spade

    CN114453843A

  • Technique of manufacturing steel spade in environment protechion type

    CN1518856A

  • Stainless steel material and manufacturing method therefor

    WO2013159669A1