Anti-aging elastomer and preparation method thereof

By using polystyrene, butylene-octene copolymer and other materials combined with specific additives, aging-resistant elastomers are prepared, which solves the problem of easy aging of existing elastomers and significantly improves their performance and use under high temperature conditions. life.

CN118812972APending Publication Date: 2024-10-22陕西振铭时代科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411021746.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing elastomers are prone to aging during long-term use, which affects their service life in fields such as high-end shoe materials, automobile parts, and medical catheters.

Method used

Using materials such as polystyrene, butene-octene copolymer, polyethylene resin, hydrogenated nitrile rubber, and adding N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxy phenyl) propionyl), pentaerythritol Ingredients such as tetrakis (3-laurylthiopropionate) and butylhydroxyanisole are combined with plasticizers, inorganic fillers, heat stabilizers and flame retardants to prepare aging-resistant elastomers, which are extruded through twin-screw extruders. Granules are obtained through out-of-machine granulation process.

Benefits of technology

It significantly improves the aging resistance of the elastomer, extends its service life, and shows excellent surface condition and performance in high-temperature aging tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967477410000091
    Figure BDA0004967477410000091
Patent Text Reader

Abstract

The invention relates to an anti-aging elastomer and a preparation method thereof, and the anti-aging elastomer comprises the following substances in parts by weight: 80-100 parts of polystyrene, 60-80 parts of a butylene-octene copolymer, 60-80 parts of polyethylene resin, 80-100 parts of hydrogenated nitrile rubber, 4-8 parts of N, N '-bis-(3-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexamethylenediamine and 3-5 parts of pentaerythritol tetra (3-lauryl thiopropionate). The flame-retardant plastic is prepared from the following components in parts by weight: 3-5 parts of butyl hydroxy anisd, 5-15 parts of white oil, 3-5 parts of a lubricant, 4-8 parts of a plasticizer, 6-10 parts of inorganic filler, 3-5 parts of a heat stabilizer and 2-4 parts of a flame retardant. The polystyrene, the butene-octylene copolymer, the polyethylene resin and the hydrogenated butadiene-acrylonitrile rubber are used as main substances of the elastomer, the properties of the substances are excellent, and the elastomer prepared by mixing the substances is more excellent; meanwhile, through combined use of N, N '-bis-(3-(3, 5-di-tert-butyl-4-hydroxyphenyl) propionyl), pentaerythritol tetra (3-lauryl thiopropionate) and butylated hydroxyanisole, the aging resistance of the prepared elastomer can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of elastomer production, in particular to an aging-resistant elastomer and a preparation method thereof. Background Art

[0002] Elastomer is one of the important raw materials in current chemical production. Due to its excellent performance, elastomer is increasingly widely used in the production of advanced shoe materials, auto parts, medical catheters, silencer gears, elastic fibers, and smart wearables. However, due to the problem of its own material, the current elastomer is prone to aging during long-term use, thus affecting the service life of the finished product made with it as raw material. Summary of the invention

[0003] The invention provides an aging-resistant elastomer and a preparation method thereof, which are used to solve the defects in the prior art.

[0004] The present invention is achieved through the following technical solutions:

[0005] An aging-resistant elastomer comprises the following substances in parts by weight: 80-100 parts of polystyrene, 60-80 parts of butene-octene copolymer, 60-80 parts of polyethylene resin, 80-100 parts of hydrogenated nitrile rubber, 4-8 parts of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, 3-5 parts of pentaerythritol tetrakis(3-laurylthiopropionate), 3-5 parts of butylated hydroxyanisole, 5-15 parts of white oil, 3-5 parts of lubricant, 4-8 parts of plasticizer, 6-10 parts of inorganic filler, 3-5 parts of heat stabilizer and 2-4 parts of flame retardant.

[0006] In the above-mentioned aging-resistant elastomer, the molecular weight of the polystyrene is 100,000-120,000.

[0007] In the above-mentioned aging-resistant elastomer, the molecular weight of the butene-octene copolymer is 50,000-80,000.

[0008] In the above-mentioned aging-resistant elastomer, the molecular weight of the polyethylene resin is 100,000-200,000.

[0009] In the above-mentioned aging-resistant elastomer, the kinematic viscosity (40° C.) of the white oil is 30-40 m2 / s.

[0010] In the above-mentioned aging-resistant elastomer, the lubricant is any one of ethyl stearate, potassium stearate, magnesium stearate, solid paraffin and ethylenebisricinoleamide, or a mixture of any two or more of them in any proportion.

[0011] In the aging-resistant elastomer as described above, the plasticizer is any one of diisobutyl phthalate, diphenyl phosphate, dioctyl epoxytetrahydrophthalate, dioctyl sebacate and trihexyl trimellitate, or a mixture of any two or more thereof in any proportion.

[0012] In the above-mentioned aging-resistant elastomer, the inorganic filler is any one of kaolin, talcum powder, silicon dioxide, calcium carbonate and quartz glass fiber, or a mixture of any two or more of them in any proportion.

[0013] In the above-mentioned aging-resistant elastomer, the heat stabilizer is any one of zinc carboxylate, barium laurate and dibutyltin maleate, or a mixture of any two or more of them in any proportion.

[0014] In the above-mentioned aging-resistant elastomer, the flame retardant is any one of decabromodiphenyl ether, triphenyl phosphate, hexachlorocyclopentadiene and triphenyl phosphite, or a mixture of any two or more of them in any proportion.

[0015] A method for preparing an aging-resistant elastomer comprises the following steps:

[0016] Step 1: Weigh polystyrene, butene-octene copolymer, polyethylene resin, hydrogenated nitrile rubber, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl), pentaerythritol tetrakis(3-laurylthiopropionate), butylated hydroxyanisole, white oil, lubricant, plasticizer, inorganic filler, heat stabilizer, and flame retardant according to the ratio;

[0017] Step 2: Add the weighed material in step 1 into a sealed mixer, heat to 180-200°C, and melt mix at a stirring speed of 150-170 r / min for 2-3 hours;

[0018] Step 3: sending the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation, and cooling the granulation by water to obtain aging-resistant elastomer particles.

[0019] In the method for preparing an aging-resistant elastomer as described above, the temperature of the feeding section of the twin-screw extruder is controlled at 165-185°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 120-140°C.

[0020] The advantages of the present invention are as follows: the present invention uses polystyrene, butene-octene copolymer, polyethylene resin and hydrogenated nitrile rubber as main substances of the elastomer, the above substances have excellent performance and the elastomer prepared after being mixed is more excellent, and at the same time, the molecular weights of polystyrene, butene-octene copolymer and polyethylene resin are relatively large, so they have good aging resistance; at the same time, the aging resistance of the prepared elastomer can be effectively improved by using N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl), pentaerythritol tetrakis(3-laurylthiopropionate) and butylated hydroxyanisole in combination; at the same time, the plasticizer, inorganic filler, heat stabilizer and flame retardant can improve the performance of the prepared elastomer and further increase the aging resistance of the elastomer. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] Step 1: According to the ratio, weigh 8kg of polystyrene with a molecular weight of 100000-110000, 6kg of butene-octene copolymer with a molecular weight of 50000-60000, 6kg of polyethylene resin with a molecular weight of 100000-120000, 8kg of hydrogenated nitrile rubber, 0.4kg of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, 0.3kg of pentaerythritol tetrakis(3-laurylthiopropionate), 0.3kg of butylated hydroxyanisole, 0.5kg of white oil (kinematic viscosity (40°C) is 30-40㎡ / s), 0.3kg of ethyl stearate, 0.4kg of dioctyl epoxytetrahydrophthalate, 0.6kg of silicon dioxide, 0.3kg of dibutyltin maleate, and 0.2kg of decabromodiphenyl ether;

[0024] Step 2: Add the material weighed in step 1 into a sealed mixer, heat to 180°C, and melt mix at a stirring speed of 150 r / min for 3 hours;

[0025] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 165°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 120°C. After granulation, water cooling is used for cooling to obtain aging-resistant elastomer particles.

[0026] Example 2

[0027] Step 1: According to the proportion, weigh 10 kg of polystyrene with a molecular weight of 110,000-120,000, 8 kg of butene-octene copolymer with a molecular weight of 70,000-80,000, 8 kg of polyethylene resin with a molecular weight of 170,000-200,000, 10 kg of hydrogenated nitrile rubber, 0.8 kg of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, 0.5 kg of pentaerythritol tetrakis(3-laurylthiopropionate), 0.5 kg of butylated hydroxyanisole, and white oil (kinematic viscosity (40°C) is 30-40㎡ / s) 1.5kg, ethyl stearate 0.1kg, magnesium stearate 0.2kg, solid paraffin 0.2kg, diisobutyl phthalate 0.2kg, diphenyl phosphate toluene 0.2kg, dioctyl epoxytetrahydrophthalate 0.2kg, trihexyl trimellitate 0.2kg, kaolin 0.5kg, talc 0.2kg, quartz glass fiber 0.3kg, zinc carboxylate 0.3kg, dibutyltin maleate 0.2kg, decabromodiphenyl ether 0.1kg, hexachlorocyclopentadiene 0.1kg, triphenyl phosphite 0.2kg;

[0028] Step 2: Add the weighed material in step 1 into a sealed mixer, heat to 200°C, and melt mix at a stirring speed of 170 r / min for 2 hours;

[0029] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 185°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 140°C. After granulation is completed, water cooling is used for cooling to obtain aging-resistant elastomer particles.

[0030] Example 3

[0031] Step 1: According to the ratio, weigh 9kg of polystyrene with a molecular weight of 110000-115000, 7kg of butene-octene copolymer with a molecular weight of 60000-70000, 7kg of polyethylene resin with a molecular weight of 120000-170000, 9kg of hydrogenated nitrile rubber, 0.6kg of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, 0.4kg of pentaerythritol tetra(3-laurylthiopropionate), 0.4kg of butylated hydroxyanisole, 1kg of white oil (kinematic viscosity (40°C) is 30-40㎡ / s), 0.1kg of ethyl stearate, 0.05kg of potassium stearate, and 0.6kg of magnesium stearate. .05kg, solid paraffin 0.1kg, ethylene bis ricinoleamide 0.1kg, diisobutyl phthalate 0.1kg, diphenyl methyl phosphate 0.1kg, dioctyl epoxide tetrahydrophthalate 0.2kg, dioctyl phthalate 0.1kg, trihexyl trimellitate 0.1kg, kaolin 0.1kg, talc 0.2kg, silicon dioxide 0.1kg, calcium carbonate 0.1kg, quartz glass fiber 0.3kg, zinc carboxylate 0.1kg, barium laurate 0.2kg, dibutyl tin maleate 0.1kg, decabromodiphenyl ether 0.05kg, triphenyl phosphate 0.1kg, hexachlorocyclopentadiene 0.05kg, triphenyl phosphite 0.1kg;

[0032] Step 2: Add the material weighed in step 1 into a sealed mixer, heat to 190°C, and melt mix at a stirring speed of 160 r / min for 2.5 hours;

[0033] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 175°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 130°C. After granulation, water cooling is used for cooling to obtain aging-resistant elastomer particles.

[0034] Example 4

[0035] Step 1: According to the proportion, weigh 10kg of polystyrene with a molecular weight of 100000-110000, 6kg of butene-octene copolymer with a molecular weight of 50000-70000, 7kg of polyethylene resin with a molecular weight of 150000-180000, 8kg of hydrogenated nitrile rubber, 0.7kg of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, 0.4kg of pentaerythritol tetrakis(3-laurylthiopropionate), 0.5kg of butylated hydroxyanisole, and white oil (kinematic viscosity (40°C) is 30-40㎡ / s) 0.8kg, ethyl stearate 0.1kg, 0.1kg, solid paraffin 0.1kg, ethylene bis ricinoleamide 0.1kg, diisobutyl phthalate 0.4kg, dioctyl epoxide tetrahydrophthalate 0.1kg, trihexyl trimellitate 0.2kg, kaolin 0.2kg, talc 0.2kg, silicon dioxide 0.2kg, calcium carbonate 0.2kg, quartz glass fiber 0.2kg, barium laurate 0.2kg, dibutyltin maleate 0.2kg, triphenyl phosphate 0.1kg, hexachlorocyclopentadiene 0.1kg, triphenyl phosphite 0.1kg;

[0036] Step 2: Add the material weighed in step 1 into a sealed mixer, heat to 185°C, and melt mix at a stirring speed of 170 r / min for 2.7 hours;

[0037] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 180°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 125°C. After granulation, water cooling is used for cooling to obtain aging-resistant elastomer particles.

[0038] Comparative Example 1

[0039] Step 1: According to the ratio, weigh 8kg of polystyrene with a molecular weight of 100000-110000, 6kg of butene-octene copolymer with a molecular weight of 50000-60000, 6kg of polyethylene resin with a molecular weight of 100000-120000, 8kg of hydrogenated nitrile rubber, 0.5kg of white oil (kinematic viscosity (40°C) is 30-40㎡ / s), 0.3kg of ethyl stearate, 0.4kg of dioctyl epoxytetrahydrophthalate, 0.6kg of silicon dioxide, 0.3kg of dibutyltin maleate, and 0.2kg of decabromodiphenyl ether;

[0040] Step 2: Add the material weighed in step 1 into a sealed mixer, heat to 180°C, and melt mix at a stirring speed of 150 r / min for 3 hours;

[0041] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 165°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 120°C. After granulation, the elastomer particles are obtained by cooling with water.

[0042] Comparative Example 2

[0043] Step 1: According to the proportion, weigh 10kg of polystyrene with a molecular weight of 110000-120000, 8kg of butene-octene copolymer with a molecular weight of 70000-80000, 8kg of polyethylene resin with a molecular weight of 170000-200000, 10kg of hydrogenated nitrile rubber, 1.5kg of white oil (kinematic viscosity (40℃) is 30-40㎡ / s), 0.1kg of ethyl stearate, 0.2kg of magnesium stearate, and solid Paraffin 0.2kg, diisobutyl phthalate 0.2kg, diphenyl methyl phosphate 0.2kg, dioctyl epoxide tetrahydrophthalate 0.2kg, trihexyl trimellitate 0.2kg, kaolin 0.5kg, talc 0.2kg, quartz glass fiber 0.3kg, zinc carboxylate 0.3kg, dibutyltin maleate 0.2kg, decabromodiphenyl ether 0.1kg, hexachlorocyclopentadiene 0.1kg, triphenyl phosphite 0.2kg;

[0044] Step 2: Add the weighed material in step 1 into a sealed mixer, heat to 200°C, and melt mix at a stirring speed of 170 r / min for 2 hours;

[0045] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 185°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 140°C. After granulation, the elastomer particles are obtained by cooling with water.

[0046] Comparative Example 3

[0047] Step 1: According to the proportion, weigh 9kg of polystyrene with a molecular weight of 110000-115000, 7kg of butene-octene copolymer with a molecular weight of 60000-70000, 7kg of polyethylene resin with a molecular weight of 120000-170000, 9kg of hydrogenated nitrile rubber, 1kg of white oil (kinematic viscosity (40℃) is 30-40㎡ / s), 0.1kg of ethyl stearate, 0.05kg of potassium stearate, 0.05kg of magnesium stearate, 0.1kg of solid paraffin, 0.1kg of ethylenebisricinoleamide, and 1,2-diisophthalic acid. 0.1kg of phthalate, 0.1kg of toluene diphenyl phosphate, 0.2kg of dioctyl epoxytetrahydrophthalate, 0.1kg of dioctyl phthalate, 0.1kg of trihexyl trimellitate, 0.1kg of kaolin, 0.2kg of talc, 0.1kg of silicon dioxide, 0.1kg of calcium carbonate, 0.3kg of quartz glass fiber, 0.1kg of zinc carboxylate, 0.2kg of barium laurate, 0.1kg of dibutyltin maleate, 0.05kg of decabromodiphenyl ether, 0.1kg of triphenyl phosphate, 0.05kg of hexachlorocyclopentadiene, and 0.1kg of triphenyl phosphite;

[0048] Step 2: Add the material weighed in step 1 into a sealed mixer, heat to 190°C, and melt mix at a stirring speed of 160 r / min for 2.5 hours;

[0049] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 175°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 130°C. After granulation, water cooling is used for cooling to obtain elastomer particles.

[0050] Comparative Example 4

[0051] Step 1: According to the proportion, weigh 10kg of polystyrene with a molecular weight of 100000-110000, 6kg of butene-octene copolymer with a molecular weight of 50000-70000, 7kg of polyethylene resin with a molecular weight of 150000-180000, 8kg of hydrogenated nitrile rubber, 0.8kg of white oil (kinematic viscosity (40℃) is 30-40㎡ / s), 0.1kg of ethyl stearate, 0.1kg of solid paraffin, and 0.1kg of ethylene dicastate. 0.1kg of amine phthalate, 0.4kg of diisobutyl phthalate, 0.1kg of dioctyl epoxide tetrahydrophthalate, 0.2kg of trihexyl trimellitate, 0.2kg of kaolin, 0.2kg of talc, 0.2kg of silicon dioxide, 0.2kg of calcium carbonate, 0.2kg of quartz glass fiber, 0.2kg of barium laurate, 0.2kg of dibutyltin maleate, 0.1kg of triphenyl phosphate, 0.1kg of hexachlorocyclopentadiene, and 0.1kg of triphenyl phosphite;

[0052] Step 2: Add the material weighed in step 1 into a sealed mixer, heat to 185°C, and melt mix at a stirring speed of 170 r / min for 2.7 hours;

[0053] Step 3: Feed the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation. The temperature of the feeding section of the twin-screw extruder is controlled at 180°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 125°C. After granulation, the elastomer particles are obtained by cooling with water.

[0054] Verification test

[0055] The 50mm*50mm*5mm plates prepared in Examples 1-4 and Comparative Examples 1-4 were placed in the same aging box and the temperature was raised to 100°C for a high-temperature aging test for 48 hours (for specific operations, see GB / T 3512-2014). The heating device of the aging box was then turned off. After cooling to room temperature, the plates were taken out to observe the surface conditions and perform a performance test. The results are shown in Table 1.

[0056]

[0057] Table 1

[0058] It can be seen from the data in Table 1 that the plates prepared from the elastomers produced in Examples 1-4 of the present invention have good surface conditions after the high-temperature aging test in the aging box. Except for slight deformation in Example 1 and Example 4, deformation occurred in Example 2 and Example 3, and obvious deformation occurred in Comparative Examples 1-4. Moreover, the plates prepared from the elastomers produced in Examples 1-4 of the present invention still have excellent performance after the high-temperature aging test, while the performance of Comparative Examples 1-4 is poor after the high-temperature aging test. Therefore, the elastomer prepared in the present invention has excellent anti-aging performance.

[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An aging-resistant elastomer, characterized in that: The invention comprises the following substances in parts by weight: 80-100 parts of polystyrene, 60-80 parts of butene-octene copolymer, 60-80 parts of polyethylene resin, 80-100 parts of hydrogenated nitrile rubber, 4-8 parts of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, 3-5 parts of pentaerythritol tetrakis(3-laurylthiopropionate), 3-5 parts of butylated hydroxyanisole, 5-15 parts of white oil, 3-5 parts of lubricant, 4-8 parts of plasticizer, 6-10 parts of inorganic filler, 3-5 parts of heat stabilizer and 2-4 parts of flame retardant.

2. The aging-resistant elastomer according to claim 1, characterized in that: The molecular weight of the polystyrene is 100000-120000; The molecular weight of the butene-octene copolymer is 50,000-80,000; The molecular weight of the polyethylene resin is 100,000-200,000.

3. The aging-resistant elastomer according to claim 1, characterized in that: The kinematic viscosity (40° C.) of the white oil is 30-40 m2 / s.

4. The aging-resistant elastomer according to claim 1, characterized in that: The lubricant is any one of ethyl stearate, potassium stearate, magnesium stearate, solid paraffin and ethylenebisricinoleamide or a mixture of any two or more of them in any proportion.

5. The aging-resistant elastomer according to claim 1, characterized in that: The plasticizer is any one of diisobutyl phthalate, diphenyl methyl ester phosphate, dioctyl epoxytetrahydrophthalate, dioctyl sebacate and trihexyl trimellitate, or a mixture of any two or more of them in any proportion.

6. The aging-resistant elastomer according to claim 1, characterized in that: The inorganic filler is any one of kaolin, talcum powder, silicon dioxide, calcium carbonate and quartz glass fiber or a mixture of any two or more of them in any proportion.

7. The aging-resistant elastomer according to claim 1, characterized in that: The heat stabilizer is any one of zinc carboxylate, barium laurate and dibutyltin maleate or a mixture of any two or more of them in any proportion.

8. The aging-resistant elastomer according to claim 1, characterized in that: The flame retardant is any one of decabromodiphenyl ether, triphenyl phosphate, hexachlorocyclopentadiene and triphenyl phosphite, or a mixture of any two or more of them in any proportion.

9. A method for preparing an aging-resistant elastomer, characterized in that: The steps include: Step 1: Weigh polystyrene, butene-octene copolymer, polyethylene resin, hydrogenated nitrile rubber, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl), pentaerythritol tetrakis(3-laurylthiopropionate), butylated hydroxyanisole, white oil, lubricant, plasticizer, inorganic filler, heat stabilizer, and flame retardant according to the ratio; Step 2: Add the weighed material in step 1 into a sealed mixer, heat to 180-200°C, and melt mix at a stirring speed of 150-170 r / min for 2-3 hours; Step 3: sending the molten material obtained in the mixer of step 2 into a twin-screw extruder for extrusion granulation, and cooling the granulation by water to obtain aging-resistant elastomer particles.

10. The method for preparing an aging-resistant elastomer according to claim 9, characterized in that: The temperature of the feeding section of the twin-screw extruder is controlled at 165-185°C, and the temperature of the extrusion end of the twin-screw extruder is controlled at 120-140°C.