ZrB2 particles are generated in aluminum alloys through in-situ reaction methods to form ceramic particles/aluminum composite materials, which solves the problem of reduced mechanical properties of aluminum alloys at high temperatures, achieves high-temperature performance improvement and process simplification, and is suitable for large-scale applications.
Patent Information
- Application Number
- CN202410937029.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-22
AI Technical Summary
The high-temperature mechanical properties of aluminum alloys decrease due to the growth of crystal grains and precipitated phases in high-temperature environments. Existing methods such as microalloying and powder metallurgy are costly or complex, making them difficult to apply on a large scale.
ZrB2/Al-12Si-4Cu-2Ni-0.8Mg heat-resistant aluminum-silicon alloy is prepared using an in-situ reaction method. Potassium fluoroborate and potassium fluorozirconate are added to the aluminum melt for mechanical stirring to generate ZrB2 particles, which are combined with aluminum, copper, and Raw materials such as aluminum-magnesium and aluminum-silicon alloy react in situ to form ceramic particles/aluminum composite materials.
It improves the room temperature and high temperature tensile strength of the material, reduces the high temperature creep rate, and extends the creep life. The process is simple, the cost is low, it is suitable for industrial production, and it has good high temperature resistance.
Smart Images

Figure CN118814031A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of alloy materials, and in particular to a heat-resistant aluminum-silicon alloy and a preparation method thereof. Background Art
[0002] Aluminum Matrix Composites have been widely used in various industries due to their advantages of high specific strength, high specific stiffness, low density, good thermal stability, and high temperature creep resistance. However, the high temperature mechanical properties of aluminum alloy parts often decrease significantly due to the growth of their grains and precipitates at high temperatures, making the parts unable to continue to be used in high temperature environments. For example, as one of the key components in the engine combustion chamber, the piston of an automobile engine needs to withstand the thermal mechanical fatigue of 25 to 300 ° C and be used for a long time in an environment of 350 to 400 ° C. At present, researchers have adopted many methods to improve the high temperature mechanical properties of aluminum alloys, such as: adding trace amounts of rare earth elements to aluminum using the microalloying method. These rare earth elements can form thermally stable dispersed nano-precipitates in aluminum. These precipitates can pin dislocations at grain boundaries, thereby improving the high temperature mechanical properties of the material. However, the microalloying method increases the cost of the material, which limits its large-scale application to a certain extent; the preparation of ceramic particles / aluminum composites by powder metallurgy can well improve the high temperature mechanical properties of the material, but the powder metallurgy method always faces the dilemma of high cost and complex process. In contrast, the preparation of ceramic particles / aluminum composite materials by in-situ reaction method to enhance the high temperature creep performance of aluminum matrix has the advantages of small in-situ particle size, close and clean ceramic particle-aluminum interface, and simple preparation process. In view of the above problems, the present invention proposes a preparation method of ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg heat-resistant aluminum-silicon alloy by in-situ reaction method. Summary of the invention
[0003] The purpose of the present invention is to provide a heat-resistant aluminum-silicon alloy and a preparation method thereof to solve the problems raised in the above background technology.
[0004] To achieve the above-mentioned purpose, the present invention provides a heat-resistant aluminum-silicon alloy, including an Al-12Si-4Cu-2Ni-0.8Mg matrix alloy and ZrB2 particles; in terms of mass percentage, the ZrB2 particles are 0wt.% to 4wt.%, and the Al-12Si-4Cu-2Ni-0.8Mg alloy is 96wt.% to 100wt.%.
[0005] The present invention also provides a method for preparing the above-mentioned heat-resistant aluminum-silicon alloy, comprising the following steps:
[0006] S1: Cutting block industrial pure aluminum, aluminum-copper alloy, aluminum-magnesium alloy, aluminum-silicon alloy, and aluminum-nickel alloy into small pieces in a machine tool, and then drying them for standby use;
[0007] S2: Put industrial pure aluminum into a graphite crucible, place it in an electromagnetic induction furnace to heat and melt, take potassium fluoroborate and potassium fluorozirconate mixed salt powder and add it to the melt, and perform in-situ reaction by electromagnetic and mechanical stirring;
[0008] S3: After adjusting the temperature, aluminum-copper alloy, aluminum-silicon alloy, and aluminum-nickel alloy are added as raw materials to the melt obtained in S2, and then a covering agent is added. After standing and keeping warm, the mixture is stirred and slag is removed;
[0009] S4: After adjusting the temperature, the aluminum-magnesium alloy is pressed into the bottom of the melt obtained in S3, and a refining agent is added after heat preservation. After all the raw materials are melted, the slag is skimmed to obtain a ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material melt;
[0010] S5: injecting the ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material melt into a mold, and demolding after air cooling to obtain an ingot of the ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material.
[0011] Preferably, in S1, the drying conditions are: drying in an electric constant temperature blast drying oven at 200°C for 0.5h, wherein the heating rate of the drying oven is 5-10°C / min.
[0012] Preferably, in S2, the temperature of the electromagnetic induction furnace is 870° C., and the in-situ reaction time is 30 min.
[0013] Preferably, in S3, the temperature is adjusted to 800° C., the covering agent is a NaCl / KCl mixed material with a mass ratio of 1:1, and the standing and heat preservation time is 10 minutes.
[0014] Preferably, in S4, the temperature is adjusted to 680-700° C. and kept warm for 5 minutes.
[0015] Preferably, in S4, the refining agent is hexachloroethane.
[0016] Preferably, in S5, after the mold is coated with a sodium silicate / zinc oxide mixed coating in a mass ratio of 1:3, it is placed in a muffle furnace and preheated to 200° C., and air-cooled for ≥40 min.
[0017] Therefore, the present invention provides a heat-resistant aluminum-silicon alloy and a preparation method thereof, and the specific beneficial effects are as follows:
[0018] (1) The present invention uses industrial pure aluminum, aluminum-copper alloy, aluminum-magnesium alloy, aluminum-silicon alloy, aluminum-nickel alloy, potassium borofluoride and potassium zirconate as raw materials, and adopts mechanical stirring and electromagnetic stirring methods to react in situ in aluminum melt to generate ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite materials with different mass fractions. ZrB2 particles serve as a strengthening phase to improve the room temperature tensile strength and high temperature tensile strength of the matrix alloy, thus overcoming the defects of the casting performance of conventional Al-Si alloys. The preparation process is relatively simple, the smelting and cooling time is short, the preparation cost is low, and industrial production is easy to achieve. The composite material has great application prospects in the fields of new material development and excellent high temperature resistant alloys.
[0019] (2) The room temperature tensile strength of ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material increases with the increase of ZrB2 content, reaching the maximum when adding 4wt.%, and the room temperature tensile strength increases from 253.79MPa to 322.65MPa, an increase of 27.13%. The high temperature tensile strength of ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material increases with the increase of ZrB2 content, reaching the maximum when adding 4wt.%, and the high temperature tensile strength increases from 100.84MPa to 127.65MPa, an increase of 26.59%.
[0020] (3) The addition of ZrB2 improves the high temperature creep strength of the matrix alloy. When the mass fraction of the particles increases to 4wt.%, the steady-state creep rate of the composite material is further reduced to 7.27×10 -8 s -1 , than the base alloy (1.73×10 - 7 s -1 ) is 2.38 times lower. The creep life of the 4wt.% composite material is about 76.6 hours, which is almost 130% longer than that of the matrix alloy (33.5 hours). At 300°C and 50MPa, the steady-state creep rate of the composite material of the present invention is 7.27×10 -8 s -1 , which is lower than the high temperature creep rate of many creep-resistant aluminum alloys reported in recent years, indicating that the composite material developed by the present invention has the potential for application above 300°C.
[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 XRD line graphs of T5 and T6 state ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite materials;
[0023] Figure 2 It is the room temperature tensile curve of T6 state ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material;
[0024] Figure 3 This is the high temperature tensile curve of T6 state ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material.
[0025] Figure 4 This is the high temperature creep tensile strain-time diagram of T5 state ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific drawings and embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.
[0027] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0028] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0029] Unless otherwise specified in the present invention, the reagents, instruments, equipment, etc. used are the reagents, instruments, and equipment commonly used by technicians in this field. The raw materials used in the present invention are industrial pure aluminum and aluminum-copper 50 alloy provided by Suzhou Guangyuan Metal Materials Co., Ltd., aluminum-magnesium 20, aluminum-silicon 50, and aluminum-nickel 20 alloys provided by Suzhou Xinghai E-commerce Co., Ltd., and potassium fluoroborate and potassium fluorozirconate purchased from the Aladdin website.
[0030] Example 1
[0031] This embodiment provides a method for preparing a 0wt.% ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material, comprising the following steps:
[0032] S1: Cut the block of industrial pure aluminum, aluminum-copper alloy, aluminum-magnesium alloy, aluminum-silicon alloy, and aluminum-nickel alloy into small pieces in a machine tool, and then place them in an electric constant temperature blast drying oven at 200°C to dry for 0.5h for use.
[0033] S2: Place 540g of pure aluminum ingot in a graphite crucible and put it into an electromagnetic induction furnace and heat it to 800℃. After the aluminum block is completely melted, add 80g of aluminum-copper 50 alloy, 240g of aluminum-silicon 50 alloy, and 100g of aluminum-nickel 20 alloy in sequence. While ensuring the alloy composition, add 8g of covering agent (NaCl:KCl, mass ratio of 1:1) to isolate the air and reduce oxidation. After standing and keeping warm for 10 minutes, stir and skim the slag.
[0034] S3: Adjust the power and when the furnace temperature drops to 700°C, quickly press 40g of Al-20Mg master alloy into the bottom of the melt. After keeping warm for 5 minutes, add 15g of hexachloroethane as a refining agent. After all the raw materials are melted, skim the slag again to obtain a 0wt.% ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material melt.
[0035] S4: Carry out mechanical stirring at 710°C for 2 minutes, maintain the furnace temperature at 720°C to skim off the slag, maintain the temperature and take out the crucible, and finally pour the above aluminum melt into a mold that has been pre-coated with a sodium silicate / zinc oxide mixed coating with a mass ratio of 1:3 and fully preheated at 200°C to obtain the target material.
[0036] As attached Figure 1 , 2 As shown in Figures 3 and 4, when x=0, the diffraction results of the Al-12Si-4Cu-2Ni-0.8Mg matrix alloy prepared in this embodiment show that the main phase components in the matrix alloy are Al phase, Si phase, Al3CuNi phase, and Al2Cu phase, and the room temperature tensile strength of the matrix alloy is 253.79MPa; the tensile strength of the Al-12Si-4Cu-2Ni-0.8Mg alloy material at 350°C is 100.84MPa. Under the conditions of 300°C and 50MPa, the steady-state creep rate of the Al-12Si-4Cu-2Ni-0.8Mg alloy material is 1.73×10 -7 s -1 , the creep life is about 35.5 hours.
[0037] Example 2
[0038] This embodiment provides a method for preparing a 4wt.% ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material, comprising the following steps:
[0039] S1: Cut the block of industrial pure aluminum, aluminum-copper alloy, aluminum-magnesium alloy, aluminum-silicon alloy, and aluminum-nickel alloy into small pieces in a machine tool, and then place them in an electric constant temperature blast drying oven at 200°C to dry for 0.5h for use.
[0040] S2: Put 500g pure aluminum ingot and graphite crucible into an electromagnetic induction furnace and heat it to 870°C. After the aluminum block is completely melted, add 89g potassium fluoroborate and 100g potassium fluorozirconate mixed salt powder, turn on electromagnetic stirring and mechanical stirring to ensure that the in-situ reaction is fully carried out for 30 minutes.
[0041] S3: Adjust the power and wait for the furnace temperature to reach 800°C, then add 80g of aluminum-copper 50 alloy, 240g of aluminum-silicon 50 alloy, and 100g of aluminum-nickel 20 alloy in sequence. While ensuring the alloy composition, add 8g of covering agent (NaCl:KCl, mass ratio is 1:1) to isolate the air and reduce oxidation. After standing and keeping warm for 10 minutes, stir and remove the slag.
[0042] S4: Adjust the power and when the furnace temperature drops to 700°C, quickly press 40g of Al-20Mg master alloy into the bottom of the melt. After keeping warm for 5 minutes, add 15g of hexachloroethane as a refining agent. After all the raw materials are melted, skim the slag again to obtain a 4wt.% ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material melt.
[0043] S5: Carry out mechanical stirring at 710°C for 2 minutes, maintain the furnace temperature at 720°C to skim off the slag, maintain the temperature and take out the crucible, and finally pour the above aluminum melt into a mold that has been pre-coated with a sodium silicate / zinc oxide mixed coating with a mass ratio of 1:3 and fully preheated at 200°C to obtain the target material.
[0044] As attached Figure 1 , 2As shown in Figures 3 and 4, the diffraction results of the 4wt.% ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material prepared in this embodiment show that the main phase components in the composite material are Al phase, Si phase, ZrB2 phase, Al3CuNi phase, and Al2Cu phase. The room temperature tensile strength of the composite material is 322.65MPa, and the room temperature tensile strength of the Al-12Si-4Cu-2Ni-0.8Mg matrix alloy is 253.79MPa; the tensile strength of the 4wt.% ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material at 350°C is 127.65MPa, and the tensile strength of the Al-12Si-4Cu-2Ni-0.8Mg alloy material at 350°C is 100.84MPa. At 300℃ and 50MPa, the steady-state creep rate of Al-12Si-4Cu-2Ni-0.8Mg alloy is 7.27×10 -8 s -1 , the creep life is about 76.6 hours.
[0045] By comparing the test results of ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg materials with different mass fractions prepared from the above two embodiments, it can be seen that the room temperature tensile strength and high temperature tensile strength of the ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material are higher than those of the matrix alloy.
[0046] Depend on Figure 2 It can be seen that the room temperature tensile strength increased from 253.79MPa to 322.65MPa, an increase of 27.13%; the high temperature tensile strength increased from 100.84MPa to 127.65MPa, an increase of 26.59%.
[0047] Depend on Figure 3 It can be seen that at a high temperature of 350°C, the maximum tensile strength of the composite material of the present invention reaches 127.65MPa, which exceeds the high-temperature tensile strength of many heat-resistant aluminum alloys reported in recent years, indicating that the composite material developed by the present invention has the potential for application above 300°C, and at the same time provides a reference for the development of aluminum alloys with excellent high-temperature resistance.
[0048] Depend on Figure 4 It can be seen that the addition of ZrB2 improves the high temperature creep strength of the matrix alloy. When the mass fraction of the particles increases to 4wt.%, the steady-state creep rate of the composite material decreases to 7.27×10 -8 s -1 , than the base alloy (1.73×10 -7 s -1) is 2.38 times lower. The creep life of the 4wt.% composite material is about 76.6 hours, which is almost 130% longer than that of the matrix alloy (33.5 hours). At 300°C and 50MPa, the steady-state creep rate of the composite material of the present invention is 7.27×10 -8 s -1 , which is lower than the high temperature creep rate of many creep-resistant aluminum alloys reported in recent years, indicating that the composite material developed by the present invention has the potential for application above 300°C.
[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A heat-resistant aluminum-silicon alloy, characterized in that: It includes Al-12Si-4Cu-2Ni-0.8Mg matrix alloy and ZrB2 particles; in terms of mass percentage, the ZrB2 particles account for 0wt.% to 4wt.%, and the Al-12Si-4Cu-2Ni-0.8Mg alloy accounts for 96wt.% to 100wt.%.
2. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 1, characterized in that: The following steps are involved: S1: Cutting block industrial pure aluminum, aluminum-copper alloy, aluminum-magnesium alloy, aluminum-silicon alloy, and aluminum-nickel alloy into small pieces in a machine tool, and then drying them for standby use; S2: Put industrial pure aluminum into a graphite crucible, place it in an electromagnetic induction furnace to heat and melt, take potassium fluoroborate and potassium fluorozirconate mixed salt powder and add it to the melt, and perform in-situ reaction by electromagnetic and mechanical stirring; S3: After adjusting the temperature, aluminum-copper alloy, aluminum-silicon alloy, and aluminum-nickel alloy are added as raw materials to the melt obtained in S2, and then a covering agent is added. After standing and keeping warm, the mixture is stirred and slag is removed; S4: After adjusting the temperature, the aluminum-magnesium alloy is pressed into the bottom of the melt obtained in S3, and a refining agent is added after heat preservation. After all the raw materials are melted, the slag is skimmed to obtain a ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material melt; S5: injecting the ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material melt into a mold, and demolding after air cooling to obtain an ingot of the ZrB2 / Al-12Si-4Cu-2Ni-0.8Mg composite material.
3. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 2, characterized in that: In S1, the drying condition is: drying in an electric constant temperature blast drying oven at 200°C for 0.5h, wherein the heating rate of the drying oven is 5-10°C / min.
4. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 2, characterized in that: In S2, the temperature of the electromagnetic induction furnace is 870° C., and the in-situ reaction time is 30 min.
5. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 2, characterized in that: In S3, the temperature is adjusted to 800°C, the covering agent is a NaCl / KCl mixed material with a mass ratio of 1:1, and the static insulation time is 10 minutes.
6. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 2, characterized in that: In S4, the temperature is adjusted to 680-700° C. and kept at this temperature for 5 minutes.
7. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 2, characterized in that: In the above-mentioned S4, the refining agent is hexachloroethane.
8. The method for preparing a heat-resistant aluminum-silicon alloy according to claim 2, characterized in that: In S5, after the mold is coated with a sodium silicate / zinc oxide mixed coating in a mass ratio of 1:3, it is placed in a muffle furnace and preheated to 200° C., and air-cooled for ≥40 min.