Light emitting diode with improved preparation efficiency and preparation method thereof

By forming a passivation layer on the epitaxial structure and etching the photoresist layer to form through holes, the pad preparation process of the light-emitting diode is simplified, the problem of low preparation efficiency in the existing technology is solved, and a more efficient preparation process is achieved .

CN118825152APending Publication Date: 2024-10-22HC SEMITEK (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410808228.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing manufacturing process of light-emitting diodes, the pad preparation process is complicated and requires multiple times of photoresist formation and etching to form holes, resulting in low preparation efficiency.

Method used

A passivation layer is formed on the epitaxial structure, and the first through-hole and the second through-hole are formed through one photoresist layer etching. These through-holes are used to form bonding pads on the epitaxial structure, which simplifies the use of photoresist.

Benefits of technology

It effectively simplifies the preparation process of the light-emitting diode, improves the preparation efficiency, reduces the repeated steps of forming the photoresist layer and etching holes, and improves the production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825152A_ABST
    Figure CN118825152A_ABST
Patent Text Reader

Abstract

The invention provides a light emitting diode with improved preparation efficiency and a preparation method thereof, and belongs to the technical field of photoelectron manufacturing. The preparation method of the light-emitting diode comprises the following steps: forming a passivation layer on an epitaxial structure; a photoresist layer is formed on the surface of the passivation layer, the photoresist layer is etched, and the surface of the photoresist layer is provided with a first through hole exposing the passivation layer; corroding the passivation layer through the first through hole, and forming a second through hole exposing the epitaxial structure on the surface of the passivation layer; and forming a bonding pad on the surface of the epitaxial structure through the first through hole and the second through hole in sequence. The embodiment of the invention can simplify the preparation process of the light-emitting diode and improve the preparation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of optoelectronic manufacturing technology, and in particular to a light emitting diode with improved manufacturing efficiency and a manufacturing method thereof. Background Art

[0002] Light Emitting Diode (LED) is a very influential new product in the optoelectronics industry. It has the characteristics of small size, long service life, rich colors and low energy consumption. It is widely used in lighting, display screens, signal lights, backlight sources, toys and other fields.

[0003] In the related art, a light emitting diode includes: an epitaxial layer, a passivation layer and a pad, wherein the passivation layer is located on the surface of the epitaxial layer and has a through hole exposing the epitaxial layer, and the pad is located on the surface of the passivation layer and connected to the epitaxial layer through the through hole.

[0004] In the process of preparing the pad, it is necessary to first form a photoresist on the surface of the passivation layer, use the photoresist to etch a through hole on the passivation layer, and remove the photoresist; then, form another layer of photoresist on the surface of the passivation layer, etch the photoresist to form a through hole that exposes the through hole of the passivation layer, and evaporate metal on the photoresist layer to form a pad on the surface of the passivation layer and in the through hole of the passivation layer. Since it is necessary to form photoresist multiple times and etch holes on the photoresist in the process of preparing the pad, the preparation process is complicated, which reduces the preparation efficiency of the light-emitting diode. Summary of the invention

[0005] The embodiment of the present disclosure provides a light emitting diode with improved manufacturing efficiency and a manufacturing method thereof, which can simplify the manufacturing process of the light emitting diode and improve the manufacturing efficiency. The technical solution is as follows:

[0006] On the one hand, an embodiment of the present disclosure provides a method for preparing a light-emitting diode, the method comprising: forming a passivation layer on an epitaxial structure; forming a photoresist layer on the surface of the passivation layer, and etching the photoresist layer, wherein the surface of the photoresist layer has a first through hole exposing the passivation layer; corroding the passivation layer through the first through hole, forming a second through hole exposing the epitaxial structure on the surface of the passivation layer; and forming a pad on the surface of the epitaxial structure through the first through hole and the second through hole in sequence.

[0007] Optionally, etching the passivation layer through the first through hole includes: wet etching the passivation layer so that the width of the formed second through hole is greater than the width of the first through hole.

[0008] Optionally, wet etching the passivation layer includes: using a buffered oxide etchant to etch the passivation layer, controlling the etching rate of the buffered oxide etchant to be 40 angstroms / second to 50 angstroms / second, controlling the etching time to be 250s to 350s, and the ratio of HF to NH4F in the buffered oxide etchant to be 15 to 22.

[0009] Optionally, the cross-sectional shape of the axial cross-section of the second through hole is an inverted trapezoid, and the inclination angle of the hole wall of the second through hole is less than or equal to 60 degrees.

[0010] Optionally, forming a photoresist layer on the surface of the passivation layer includes: forming the photoresist layer on the surface of the passivation layer, and controlling the sum of the thickness of the photoresist layer and the thickness of the passivation layer to be greater than or equal to the thickness of the pad.

[0011] Optionally, the cross-sectional shape of the axial cross-section of the first through hole is a regular trapezoid, and the inclination angle of the hole wall of the first through hole is less than or equal to 60 degrees.

[0012] Optionally, when preparing the passivation layer, the thickness of the passivation layer is controlled to be smaller than the thickness of the pad.

[0013] Optionally, preparing the epitaxial structure includes: forming an epitaxial layer on a substrate; forming a transparent conductive layer on a surface of the epitaxial layer; forming a first insulating layer on the surface of the epitaxial layer, so that the first insulating layer covers the transparent conductive layer, and the surface of the first insulating layer has a first via hole exposing the transparent conductive layer; forming a metal reflective layer on the surface of the first insulating layer, so that the metal reflective layer is connected to the transparent conductive layer through the first via hole; forming a metal protective layer on the surface of the first insulating layer, so that the metal protective layer covers the metal reflective layer; forming a second insulating layer on the surface of the first insulating layer, so that the second insulating layer covers the metal protective layer, and the second insulating layer has a second via hole exposing the metal protective layer; forming an electrode on the surface of the second insulating layer, so that the electrode is connected to the metal protective layer through the second via hole; forming a passivation layer on the epitaxial structure includes: forming the passivation layer on the surface of the second insulating layer, so that the passivation layer covers the electrode, and the second through hole exposes the electrode.

[0014] On the other hand, an embodiment of the present disclosure provides a light-emitting diode, which is prepared by the preparation method as described above, including: an epitaxial structure, a passivation layer and a solder pad, the passivation layer is located on the surface of the epitaxial structure, and the passivation layer has a second through hole exposing the epitaxial structure; the orthographic projection of the solder pad on the bottom surface of the epitaxial structure is located within the orthographic projection of the second through hole on the bottom surface of the epitaxial structure.

[0015] Optionally, the thickness of the passivation layer is smaller than the thickness of the pad.

[0016] The beneficial effects brought by the technical solution provided by the embodiments of the present disclosure include at least:

[0017] In the method for preparing a light-emitting diode provided in an embodiment of the present disclosure, a passivation layer is first formed on the epitaxial structure, and then a photoresist layer is formed on the passivation layer, and a first through hole exposing the passivation layer is formed by etching on the photoresist layer, and then the passivation layer is corroded through the first through hole to form a second through hole on the passivation layer, and finally a pad can be formed on the epitaxial structure through the first through hole and the second through hole.

[0018] Compared with the related art, the preparation method only needs to form a photoresist layer on the passivation layer once when preparing the pad. The photoresist layer is first used as a mask to etch and form a second through hole on the passivation layer, and the photoresist layer is also used as a mask to form the pad. Therefore, there is no need to repeatedly form a photoresist layer and etch holes on the photoresist layer, which effectively simplifies the preparation process of the light-emitting diode and improves the preparation efficiency of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0020] Figure 1 It is a flow chart of a method for preparing a light-emitting diode provided in an embodiment of the present disclosure;

[0021] Figure 2 is a diagram of a preparation state of a light emitting diode provided by an embodiment of the present disclosure;

[0022] Figure 3 is a diagram of a preparation state of a light emitting diode provided by an embodiment of the present disclosure;

[0023] Figure 4 is a diagram of a preparation state of a light emitting diode provided by an embodiment of the present disclosure;

[0024] Figure 5 It is a structural schematic diagram of a light emitting diode provided by the present disclosure.

[0025] The descriptions of the marks in the figure are as follows:

[0026] 10. Substrate;

[0027] 20. Epitaxial structure;

[0028] 21. epitaxial layer; 22. transparent conductive layer; 23. first insulating layer; 24. metal reflective layer; 25. metal protective layer; 26. second insulating layer; 27. electrode;

[0029] 30. passivation layer; 31. second through hole;

[0030] 40. photoresist layer; 41. first through hole;

[0031] 50. Soldering pad. DETAILED DESCRIPTION

[0032] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.

[0033] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. The words "first", "second", "third" and similar words used in the patent application specification and claims of the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantity limitation, but indicate the existence of at least one. Words such as "include" or "comprise" and similar words mean that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. Words such as "connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right", "top", "bottom" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0034] Figure 1 FIG. 1 is a flow chart of a method for preparing a light-emitting diode provided in an embodiment of the present disclosure. Figure 1 As shown, the preparation method comprises:

[0035] Step 101 : forming a passivation layer 30 on the epitaxial structure 20 .

[0036] Step 102 : forming a photoresist layer 40 on the surface of the passivation layer 30 , and etching the photoresist layer 40 .

[0037] The surface of the photoresist layer 40 has a first through hole 41 exposing the passivation layer 30 .

[0038] Step 103 : etching the passivation layer 30 through the first through hole 41 to form a second through hole 31 on the surface of the passivation layer 30 to expose the epitaxial structure 20 .

[0039] Step 104 : forming a pad 50 on the surface of the epitaxial structure 20 through the first through hole 41 and the second through hole 31 in sequence.

[0040] In the method for preparing a light-emitting diode provided in the embodiment of the present disclosure, a passivation layer 30 is first formed on the epitaxial structure 20, and then a photoresist layer 40 is formed on the passivation layer 30, and a first through hole 41 exposing the passivation layer 30 is formed by etching on the photoresist layer 40, and then the passivation layer 30 is corroded through the first through hole 41 to form a second through hole 31 on the passivation layer 30, and finally a pad 50 can be formed on the epitaxial structure 20 through the first through hole 41 and the second through hole 31.

[0041] Compared with the related art, the preparation method only needs to form a photoresist layer 40 on the passivation layer 30 once when preparing the pad 50. The photoresist layer 40 is first used as a mask to etch and form the second through hole 31 on the passivation layer 30, and the photoresist layer 40 is also used as a mask to form the pad 50. Therefore, there is no need to repeatedly form the photoresist layer 40 and etch holes on the photoresist layer 40, which effectively simplifies the preparation process of the light-emitting diode and improves the preparation efficiency of the light-emitting diode.

[0042] Before step 101, preparing the epitaxial structure 20 may include the following steps:

[0043] In the first step, an epitaxial layer 21 is formed on a substrate.

[0044] The substrate is a sapphire substrate, a silicon substrate or a silicon carbide substrate. The substrate can be a flat substrate or a patterned substrate.

[0045] As an example, in the embodiment of the present disclosure, the substrate is a sapphire substrate. The sapphire substrate is a commonly used substrate with mature technology and low cost. Specifically, it can be a patterned sapphire substrate or a sapphire flat sheet substrate.

[0046] The sapphire substrate may be pre-treated, placed in a MOCVD (Metal-organic Chemical Vapor Deposition) reaction chamber, and baked for 12 to 18 minutes. As an example, in the embodiment of the present disclosure, the sapphire substrate is baked for 15 minutes.

[0047] Specifically, the baking temperature may be 1000° C. to 1200° C., and the pressure in the MOCVD reaction chamber during baking may be 100 mbar to 200 mbar.

[0048] Growing the epitaxial layer 21 on the substrate may include: sequentially forming a first semiconductor layer, a multi-quantum well layer, and a second semiconductor layer on the sapphire substrate by using MOCVD technology.

[0049] The first semiconductor layer is an n-type layer, and the second semiconductor layer is a p-type layer.

[0050] Optionally, the first semiconductor layer is a silicon-doped n-type GaN layer, and the thickness of the n-type GaN layer may be 0.5 μm to 3 μm.

[0051] The growth temperature of the n-type GaN layer may be 1000° C. to 1100° C., and the growth pressure of the n-type GaN layer may be 100 torr to 300 torr.

[0052] Optionally, the multi-quantum well layer includes alternately grown InGaN quantum well layers and GaN quantum barrier layers. Wherein, the multi-quantum well layer may include 3 to 8 periods of alternately stacked InGaN quantum well layers and GaN quantum barrier layers.

[0053] When growing multi-quantum well layers, the pressure of the MOCVD reaction chamber is controlled at 200 torr. When growing InGaN quantum well layers, the temperature of the reaction chamber is 760°C to 780°C. When growing GaN quantum barrier layers, the temperature of the reaction chamber is 860°C to 890°C.

[0054] As an example, in the embodiment of the present disclosure, the multi-quantum well layer includes five periods of alternately stacked InGaN quantum well layers and GaN quantum barrier layers.

[0055] Optionally, the thickness of the multi-quantum well layer may be 150 nm to 200 nm.

[0056] Optionally, the second semiconductor layer is a magnesium-doped p-type GaN layer. The thickness of the p-type GaN layer may be 0.5 μm to 3 μm.

[0057] When growing the p-type GaN layer, the growth pressure of the p-type GaN layer may be 200 Torr to 600 Torr, and the growth temperature of the p-type GaN layer may be 800° C. to 1000° C.

[0058] After forming the epitaxial layer 21 , the preparation method further includes: etching the second semiconductor layer to form a groove exposing the first semiconductor layer.

[0059] In the second step, a transparent conductive layer 22 is formed on the surface of the epitaxial layer 21 .

[0060] Specifically, it may include: sputtering a transparent conductive layer 22 on the epitaxial layer 21 .

[0061] Exemplarily, the transparent conductive layer 22 may be an indium tin oxide (ITO) layer or an indium zinc oxide (IZO) layer.

[0062] Exemplarily, the transparent conductive layer 22 is an indium tin oxide layer. The indium tin oxide layer has good transmittance and low resistivity. The indium tin oxide layer has low resistivity, facilitates carrier conduction, and improves injection efficiency.

[0063] Exemplarily, the transparent conductive layer 22 is an indium zinc oxide layer. The indium zinc oxide layer has good transmittance and low resistivity. The indium zinc oxide layer has low resistivity, facilitates carrier conduction, and improves injection efficiency.

[0064] Exemplarily, the thickness of the transparent conductive layer 22 is 100 angstroms to 300 angstroms. For example, the thickness of the transparent conductive layer 22 is 200 angstroms.

[0065] In the above implementation, by disposing the transparent conductive layer 22 between the metal reflective layer 24 and the epitaxial layer 21 , the current conduction efficiency between the metal reflective layer 24 and the epitaxial layer 21 can be improved.

[0066] In the third step, a first insulating layer 23 is formed on the surface of the epitaxial layer 21 , so that the first insulating layer 23 covers the transparent conductive layer 22 .

[0067] The surface of the first insulating layer 23 has a first via hole exposing the transparent conductive layer 22 .

[0068] Exemplarily, the first insulating layer 23 may be a silicon oxide layer.

[0069] As an example, in the implementation of the present disclosure, the thickness of the silicon oxide layer is 7000 angstroms to 12000 angstroms.

[0070] In the fourth step, a metal reflective layer 24 is formed on the surface of the first insulating layer 23 , so that the metal reflective layer 24 is connected to the transparent conductive layer 22 through the first via hole.

[0071] The metal reflective layer 24 is connected to the transparent conductive layer 22 through the first through hole 41. The metal reflective layer 24 includes an Ag layer, a Ni layer and a TiW layer stacked in sequence.

[0072] Exemplarily, the thickness of the Ag layer is 1400 angstroms to 1700 angstroms. For example, the thickness of the Ag layer is 1500 angstroms.

[0073] Exemplarily, the thickness of the Ni layer is 100 angstroms to 300 angstroms. For example, the thickness of the Ni layer is 200 angstroms.

[0074] Exemplarily, the thickness of the TiW layer is 700 angstroms to 1000 angstroms. For example, the thickness of the TiW layer is 800 angstroms.

[0075] In the fifth step, a metal protection layer 25 is formed on the surface of the first insulating layer 23 , so that the metal protection layer 25 covers the metal reflective layer 24 .

[0076] The metal protection layer 25 includes a Cr layer, an Al layer, a Ti layer, an Al layer, a Ti layer, an Al layer, a Cr layer, a Pt layer and a Ti layer stacked in sequence, and the thickness of each metal layer is 30 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 500 angstroms, 2000 angstroms and 500 angstroms respectively.

[0077] In the sixth step, a second insulating layer 26 is formed on the surface of the first insulating layer 23 , so that the second insulating layer 26 covers the metal protection layer 25 .

[0078] The second insulating layer 26 has a second via hole exposing the metal protection layer 25 .

[0079] The second insulating layer 26 is a distributed Bragg reflector (DBR) layer, and the DBR layer includes a plurality of SiO2 layers and TiO2 layers that are periodically and alternately stacked, and the thickness of the DBR layer is 3 μm to 4 μm.

[0080] Exemplarily, the number of periods of the DBR layer may be between 20 and 50. For example, the number of periods of the DBR layer is 32.

[0081] The thickness of the SiO2 layer in the DBR layer may be 800 angstroms to 1200 angstroms, and the thickness of the TiO2 layer may be 500 angstroms to 900 angstroms.

[0082] In the seventh step, an electrode 27 is formed on the surface of the second insulating layer 26 , so that the electrode 27 is connected to the metal protection layer 25 through a second via hole.

[0083] For example, the electrode 27 may include a Cr layer, an Al layer, a Ti layer, an Al layer, a Ti layer, an Al layer, a Cr layer, a Pt layer, and a Ti layer stacked in sequence, and the thickness of each metal layer is 30 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 500 angstroms, 2000 angstroms, and 500 angstroms, respectively.

[0084] Exemplarily, the electrode 27 includes two mutually insulated parts, one part of the electrode 27 is connected to the first semiconductor layer of the epitaxial layer 21, and the other part of the electrode 27 is connected to the metal protective layer 25 through a through hole, thereby achieving the purpose of electrically connecting the electrode 27 to the second semiconductor layer of the epitaxial layer 21.

[0085] Step 101 may include: forming a passivation layer 30 on the surface of the second insulating layer 26 , so that the passivation layer 30 covers the electrode 27 .

[0086] Exemplarily, the passivation layer 30 may be a silicon oxide layer.

[0087] In the embodiment of the present disclosure, when preparing the passivation layer 30 , the thickness of the passivation layer 30 is controlled to be smaller than the thickness of the pad 50 .

[0088] By making the thickness of the passivation layer 30 smaller than the thickness of the pad 50 , the formed pad 50 can protrude from the passivation layer 30 , which is beneficial for the pad 50 to be electrically connected to an external power source.

[0089] The thickness of the passivation layer 30 may be 10000 angstroms to 15000 angstroms. For example, the thickness of the passivation layer 30 may be 12000 angstroms.

[0090] Step 102 may include the following steps:

[0091] First, a photoresist layer 40 is formed on the surface of the passivation layer 30 , and the sum of the thickness of the photoresist layer 40 and the thickness of the passivation layer 30 is controlled to be greater than or equal to the thickness of the pad 50 .

[0092] Figure 2 FIG. 1 is a diagram showing the preparation state of a light emitting diode provided by an embodiment of the present disclosure. Figure 2 As shown, the passivation layer 30 is located on the epitaxial structure 20 , and a photoresist layer 40 is formed on the surface of the passivation layer 30 .

[0093] By controlling the sum of the thickness of the photoresist layer 40 and the thickness of the passivation layer 30 to be not less than the thickness of the pad 50, when the pad 50 is evaporated through the photoresist layer 40, the metal evaporated on the surface of the photoresist layer 40 and the metal in the first through hole 41 and the second through hole 31 will be torn off, thereby preventing the pad 50 from being evaporated to other areas except the second through hole 31.

[0094] Then, the photoresist layer 40 is etched to form a first through hole 41 exposing the passivation layer 30 in the photoresist layer 40 .

[0095] like Figure 2 As shown, the cross-sectional shape of the axial cross-section of the first through hole 41 is a regular trapezoid.

[0096] By setting the first through hole 41 etched by the photoresist layer 40 to be a regular trapezoid, the shape of the subsequently deposited pad 50 is also a regular trapezoid. In this way, the bottom surface of the pad 50 has a large enough area to contact the epitaxial structure 20, thereby improving the connection reliability between the pad 50 and the epitaxial structure 20.

[0097] Furthermore, the opening position of the first through hole 41 in a regular trapezoidal shape is in a sharp angle, which is conducive to tearing off the deposited metal material so that the pad 50 is only deposited in the first through hole 41 .

[0098] Exemplarily, the inclination angle of the hole wall of the first through hole 41 is less than or equal to 60 degrees. For example, the inclination angle of the hole wall of the first through hole 41 is 60 degrees.

[0099] Step 103 may include: wet etching the passivation layer 30 , so that the width of the formed second through hole 31 is greater than the width of the first through hole 41 .

[0100] The width of the first through hole and the width of the second through hole may refer to the maximum length in a direction parallel to the surface of the passivation layer.

[0101] Exemplarily, when the first through hole is a circular hole, the width of the first through hole refers to the diameter of the circular hole.

[0102] Exemplarily, when the first through hole is a rectangular hole, the width of the first through hole refers to the diagonal length of the rectangular hole.

[0103] Specifically, the method may include: using a buffered oxide etchant to etch the passivation layer 30 , wherein the ratio of HF to NH 4 F in the buffered oxide etchant is 15 to 22.

[0104] For example, the ratio of HF to NH4F in the buffered oxide etchant is 20.

[0105] When the passivation layer 30 is wet-etched by a buffered oxide method, the passivation layer 30 will be longitudinally and transversely etched. After the transverse etching, the width of the second through hole 31 of the passivation layer 30 will naturally be greater than the width of the first through hole 41 of the photoresist layer 40 .

[0106] The passivation layer 30 is formed into a second through hole 31 with a larger width by etching, so that the deposited metal can be transferred laterally in the second through hole 31 after passing through the first through hole 41, thereby increasing the size of the pad 50 and making the contact area between the pad 50 and the epitaxial structure 20 larger, which is beneficial for the pad 50 to transfer current to the epitaxial structure 20.

[0107] Optionally, during the process of etching the passivation layer 30 , the etching rate of the buffered oxide etching solution is controlled to be 40 angstroms / second to 50 angstroms / second, and the etching time is controlled to be 250 seconds to 350 seconds.

[0108] For example, in the embodiment of the present disclosure, the thickness of the passivation layer 30 is 13000 angstroms, so the etching rate of the buffered oxide etchant can be controlled to be 45 angstroms / second, and the etching time is 300 seconds. Such an etching rate and etching time can ensure that the passivation layer 30 can be completely etched through to expose the epitaxial structure 20.

[0109] Figure 3 FIG. 1 is a diagram showing the preparation state of a light emitting diode provided by an embodiment of the present disclosure. Figure 3 As shown, the cross-sectional shape of the axial cross-section of the second through hole 31 is an inverted trapezoid.

[0110] By setting the cross-sectional shape of the second through hole 31 to an inverted trapezoid, that is, making the maximum diameter of the second through hole 31 connected to the first through hole 41, when the metal is deposited from the first through hole 41 to the second through hole 31, the lateral space is immediately expanded, which is conducive to the free lateral expansion of the metal, thereby making it easier to prepare a larger pad 50.

[0111] Exemplarily, the inclination angle of the hole wall of the second through hole 31 is less than or equal to 60 degrees. For example, the inclination angle of the hole wall of the second through hole 31 is 60 degrees.

[0112] Figure 4 FIG. 1 is a diagram showing the preparation state of a light emitting diode provided by an embodiment of the present disclosure. Figure 4 As shown, the cross section of the pad prepared by the photoresist layer is formed into a regular trapezoid.

[0113] The pad prepared in step 104 may include at least one of a Ti layer, an Al layer, a Pt layer, a Ni layer, and an Au layer.

[0114] The above metal material has good heat dissipation performance. Therefore, the pad 50 made of the above material also has good heat dissipation performance, which can improve the heat dissipation effect of the light emitting diode.

[0115] Optionally, each of the pads 50 includes a first Ti layer, an Al layer, a second Ti layer, a Pt layer, a Ni layer, and an Au layer stacked in sequence.

[0116] Exemplarily, the thickness of the first Ti layer is 20 angstroms to 100 angstroms. For example, the thickness of the first Ti layer is 50 angstroms.

[0117] Exemplarily, the thickness of the Al layer is 10000 angstroms to 20000 angstroms. For example, the thickness of the Al layer is 15000 angstroms.

[0118] Exemplarily, the thickness of the second Ti layer is 500 angstroms to 1500 angstroms. For example, the thickness of the second Ti layer is 1000 angstroms.

[0119] Exemplarily, the thickness of the Pt layer is 500 angstroms to 1500 angstroms. For example, the thickness of the Pt layer is 1000 angstroms.

[0120] Exemplarily, the thickness of the Ni layer is 60,000 angstroms to 80,000 angstroms. For example, the thickness of the Ni layer is 70,000 angstroms.

[0121] Exemplarily, the thickness of the Au layer is 1500 angstroms to 2500 angstroms. For example, the thickness of the Au layer is 2000 angstroms.

[0122] The embodiment of the present disclosure provides a light emitting diode, which is prepared by the preparation method described above.

[0123] Figure 5 Schematic diagram of a light emitting diode provided by the present disclosure. Figure 5 As shown, the light emitting diode comprises: an epitaxial structure 20 , a passivation layer 30 and a pad 50 . The passivation layer 30 is located on the surface of the epitaxial structure 20 . The passivation layer 30 has a second through hole 31 exposing the epitaxial structure 20 .

[0124] The orthographic projection of the pad 50 on the bottom surface of the epitaxial structure 20 is located within the orthographic projection of the second through hole 31 on the bottom surface of the epitaxial structure 20 .

[0125] Compared with the related art, the light-emitting diode prepared by the preparation method described above only needs to form a photoresist layer 40 once on the passivation layer 30 when preparing the pad 50. The photoresist layer 40 is first used as a mask to etch and form the second through hole 31 on the passivation layer 30, and the photoresist layer 40 is also used as a mask to form the pad 50. Therefore, there is no need to repeatedly form the photoresist layer 40 and etch the holes on the photoresist layer 40, which effectively simplifies the preparation process of the light-emitting diode and improves the preparation efficiency of the light-emitting diode.

[0126] Furthermore, since the prepared pad 50 is not overlapped outside the passivation layer 30 and there is no height difference in the area where the pad 50 is deposited, the formed pad 50 is more flat.

[0127] Alternatively, if Figure 5 As shown, the thickness of the passivation layer 30 is smaller than that of the pad 50. By making the thickness of the passivation layer 30 smaller than that of the pad 50, the formed pad 50 can protrude from the passivation layer 30, which is beneficial for the pad 50 to be electrically connected to an external power source.

[0128] Alternatively, if Figure 5 As shown, the light emitting diode further includes: a substrate, an epitaxial layer 21 , a transparent conductive layer 22 , a first insulating layer 23 , a metal reflective layer 24 , a metal protective layer 25 , a second insulating layer 26 and an electrode 27 .

[0129] like Figure 5 As shown, the epitaxial layer 21 is located on the substrate, the transparent conductive layer 22 is located on the surface of the epitaxial layer 21, the first insulating layer 23 is located on the surface of the transparent conductive layer 22, the first insulating layer 23 covers the transparent conductive layer 22, and the surface of the first insulating layer 23 has a first via hole exposing the transparent conductive layer 22.

[0130] like Figure 5 As shown, the metal reflective layer 24 is located on the surface of the first insulating layer 23 , and the metal reflective layer 24 is connected to the transparent conductive layer 22 through the first via hole. The metal protective layer 25 is located on the surface of the first insulating layer 23 , and the metal protective layer 25 covers the metal reflective layer 24 .

[0131] like Figure 5 As shown, the second insulating layer 26 is located on the surface of the first insulating layer 23 , and the second insulating layer 26 covers the metal protection layer 25 . The second insulating layer 26 has a second via hole exposing the metal protection layer 25 .

[0132] like Figure 5 As shown, the electrode 27 is located on the surface of the second insulating layer 26 and is connected to the metal protection layer 25 through the second via hole. The passivation layer 30 is located on the surface of the second insulating layer 26 and covers the electrode 27 . The second through hole 31 exposes the electrode 27 .

[0133] Exemplarily, the substrate is a sapphire substrate. The sapphire substrate has a relatively high light transmittance, that is, the substrate is a transparent substrate. In addition, the sapphire material is relatively hard and has relatively stable chemical properties, so that the light-emitting diode has good light-emitting effect and stability.

[0134] In the disclosed embodiment, the epitaxial layer 21 includes a first semiconductor layer, a multi-quantum well layer, and a second semiconductor layer sequentially stacked on a substrate, and a surface of the second semiconductor layer has a groove exposing the first semiconductor layer.

[0135] In the embodiment of the present disclosure, one of the first semiconductor layer and the second semiconductor layer is a p-type layer, and the other of the first semiconductor layer and the second semiconductor layer is an n-type layer.

[0136] Exemplarily, the first semiconductor layer is an n-type layer, and the second semiconductor layer is a p-type layer.

[0137] Optionally, the first semiconductor layer is a silicon-doped n-type GaN layer, and the thickness of the n-type GaN layer may be 0.5 μm to 3 μm.

[0138] Optionally, the multi-quantum well layer includes alternately grown InGaN quantum well layers and GaN quantum barrier layers. Wherein, the multi-quantum well layer may include 3 to 8 periods of alternately stacked InGaN quantum well layers and GaN quantum barrier layers.

[0139] As an example, in the embodiment of the present disclosure, the multi-quantum well layer includes five periods of alternately stacked InGaN quantum well layers and GaN quantum barrier layers.

[0140] Optionally, the thickness of the multi-quantum well layer may be 150 nm to 200 nm.

[0141] Optionally, the second semiconductor layer is a magnesium-doped p-type GaN layer. The thickness of the p-type GaN layer may be 0.5 μm to 3 μm.

[0142] Optionally, the metal reflective layer 24 includes an Ag layer, a Ni layer, and a TiW layer stacked in sequence.

[0143] Since Ag has a good reflective effect, providing an Ag layer in the reflective layer can enhance the reflection of light by the reflective layer and improve the light emitting brightness of the light emitting surface of the light emitting diode.

[0144] The Ni layer has good corrosion resistance and wear resistance, and the TiW layer can be successfully deposited on other films as an adhesion layer without peeling or cracking. The alternating stacked Ni and TiW layers can act as a barrier layer to protect the silver mirror.

[0145] Exemplarily, the thickness of the Ag layer is 1400 angstroms to 1700 angstroms. For example, the thickness of the Ag layer is 1500 angstroms.

[0146] Exemplarily, the thickness of the Ni layer is 100 angstroms to 300 angstroms. For example, the thickness of the Ni layer is 200 angstroms.

[0147] Exemplarily, the thickness of the TiW layer is 700 angstroms to 1000 angstroms. For example, the thickness of the TiW layer is 800 angstroms.

[0148] Optionally, the metal protection layer 25 includes a Cr layer, an Al layer, a Ti layer, an Al layer, a Ti layer, an Al layer, a Cr layer, a Pt layer and a Ti layer stacked in sequence, and the thickness of each metal layer is 30 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 500 angstroms, 2000 angstroms and 500 angstroms respectively.

[0149] For example, the electrode 27 may include a Cr layer, an Al layer, a Ti layer, an Al layer, a Ti layer, an Al layer, a Cr layer, a Pt layer, and a Ti layer stacked in sequence, and the thickness of each metal layer is 30 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 1000 angstroms, 2000 angstroms, 500 angstroms, 2000 angstroms, and 500 angstroms, respectively.

[0150] Optionally, the pad 50 includes at least one of a Ti layer, an Al layer, a Pt layer, a Ni layer, and an Au layer.

[0151] The above metal material has good heat dissipation performance. Therefore, the pad 50 made of the above material also has good heat dissipation performance, which can improve the heat dissipation effect of the light emitting diode.

[0152] Alternatively, the pad 50 includes a first Ti layer, an Al layer, a second Ti layer, a Pt layer, a Ni layer, and an Au layer stacked in sequence.

[0153] Exemplarily, the thickness of the first Ti layer is 20 angstroms to 100 angstroms. For example, the thickness of the first Ti layer is 50 angstroms.

[0154] Exemplarily, the thickness of the Al layer is 10000 angstroms to 20000 angstroms. For example, the thickness of the Al layer is 15000 angstroms.

[0155] Exemplarily, the thickness of the second Ti layer is 500 angstroms to 1500 angstroms. For example, the thickness of the second Ti layer is 1000 angstroms.

[0156] Exemplarily, the thickness of the Pt layer is 500 angstroms to 1500 angstroms. For example, the thickness of the Pt layer is 1000 angstroms.

[0157] Exemplarily, the thickness of the Ni layer is 60,000 angstroms to 80,000 angstroms. For example, the thickness of the Ni layer is 70,000 angstroms.

[0158] Exemplarily, the thickness of the Au layer is 1500 angstroms to 2500 angstroms. For example, the thickness of the Au layer is 2000 angstroms.

[0159] Optionally, the first insulating layer 23 and the second insulating layer 26 both include silicon oxide layers, and the thickness of the silicon oxide layers is 3000 angstroms to 5000 angstroms.

[0160] The silicon oxide material has a good barrier effect on the active metal in the metal reflective layer 24, which can prevent the generated metal particles from damaging the silicon oxide layer and forming cracks on the silicon oxide layer, thereby preventing the light emitting diode from having leakage failure.

[0161] Optionally, the first insulating layer 23 and the second insulating layer 26 each include a plurality of silicon oxide layers and a plurality of titanium oxide layers alternately stacked.

[0162] Among them, multiple periodically alternately stacked SiO2 layers and TiO2 layers can form a DBR layer.

[0163] Exemplarily, the number of periods of the DBR layer may be between 20 and 50. For example, the number of periods of the DBR layer is 32.

[0164] The thickness of the SiO2 layer in the DBR layer may be 800 angstroms to 1200 angstroms, and the thickness of the TiO2 layer may be 500 angstroms to 900 angstroms.

[0165] In addition to the passivation effect, the DBR layer is also used to reflect the light emitted from the multi-quantum well layer to the DBR layer to the substrate, thereby improving the light extraction effect.

[0166] Optionally, the passivation layer 30 is a silicon oxide layer, wherein the thickness of the passivation layer 30 may be 10000 angstroms to 15000 angstroms. For example, the thickness of the passivation layer 30 may be 12000 angstroms.

[0167] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a light emitting diode, characterized in that: The preparation method comprises: forming a passivation layer (30) on the epitaxial structure (20); forming a photoresist layer (40) on the surface of the passivation layer (30), and etching the photoresist layer (40), wherein the surface of the photoresist layer (40) has a first through hole (41) exposing the passivation layer (30); Etching the passivation layer (30) through the first through hole (41) to form a second through hole (31) on the surface of the passivation layer (30) that exposes the epitaxial structure (20); A pad (50) is formed on the surface of the epitaxial structure (20) through the first through hole (41) and the second through hole (31) in sequence.

2. The preparation method according to claim 1, characterized in that: Etching the passivation layer (30) through the first through hole (41) comprises: The passivation layer (30) is wet-etched so that the width of the formed second through hole (31) is greater than the width of the first through hole (41).

3. The preparation method according to claim 2, characterized in that: Wet etching the passivation layer (30) comprises: The passivation layer (30) is etched with a buffered oxide etchant, the etching rate of the buffered oxide etchant is controlled to be 40 angstroms / second to 50 angstroms / second, the etching time is controlled to be 250 seconds to 350 seconds, and the ratio of HF to NH4F in the buffered oxide etchant is 15 to 22.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The cross-sectional shape of the axial cross-section of the second through hole (31) is an inverted trapezoid, and the inclination angle of the hole wall of the second through hole (31) is less than or equal to 60 degrees.

5. The preparation method according to any one of claims 1 to 3, characterized in that: Forming a photoresist layer (40) on the surface of the passivation layer (30) comprises: The photoresist layer (40) is formed on the surface of the passivation layer (30), and the sum of the thickness of the photoresist layer (40) and the thickness of the passivation layer (30) is controlled to be greater than or equal to the thickness of the pad (50).

6. The preparation method according to any one of claims 1 to 3, characterized in that: The cross-sectional shape of the axial cross-section of the first through hole (41) is a regular trapezoid, and the inclination angle of the hole wall of the first through hole (41) is less than or equal to 60 degrees.

7. The preparation method according to any one of claims 1 to 3, characterized in that: When preparing the passivation layer (30), the thickness of the passivation layer (30) is controlled to be smaller than the thickness of the pad (50).

8. The preparation method according to any one of claims 1 to 3, characterized in that: The preparation of the epitaxial structure (20) comprises: forming an epitaxial layer (21) on a substrate; forming a transparent conductive layer (22) on the surface of the epitaxial layer (21); forming a first insulating layer (23) on the surface of the epitaxial layer (21), so that the first insulating layer (23) covers the transparent conductive layer (22), and the surface of the first insulating layer (23) has a first via hole exposing the transparent conductive layer (22); forming a metal reflective layer (24) on the surface of the first insulating layer (23), so that the metal reflective layer (24) is connected to the transparent conductive layer (22) through the first via hole; forming a metal protective layer (25) on the surface of the first insulating layer (23), so that the metal protective layer (25) covers the metal reflective layer (24); forming a second insulating layer (26) on the surface of the first insulating layer (23), so that the second insulating layer (26) covers the metal protective layer (25), and the second insulating layer (26) has a second via hole exposing the metal protective layer (25); forming an electrode (27) on the surface of the second insulating layer (26), so that the electrode (27) is connected to the metal protection layer (25) through the second via hole; Forming a passivation layer (30) on the epitaxial structure (20) includes: The passivation layer (30) is formed on the surface of the second insulating layer (26), so that the passivation layer (30) covers the electrode (27), and the second through hole (31) exposes the electrode (27).

9. A light emitting diode, characterized in that: The light emitting diode is manufactured by the manufacturing method according to any one of claims 1 to 7, comprising: an epitaxial structure (20), a passivation layer (30) and a pad (50), wherein the passivation layer (30) is located on the surface of the epitaxial structure (20), and the passivation layer (30) has a second through hole (31) exposing the epitaxial structure (20); The orthographic projection of the solder pad (50) on the bottom surface of the epitaxial structure (20) is located within the orthographic projection of the second through hole (31) on the bottom surface of the epitaxial structure (20).

10. The light emitting diode according to claim 9, characterized in that: The thickness of the passivation layer (30) is smaller than the thickness of the pad (50).