Carbon electrode with multi-layer echelon cracks and preparation method thereof
The carbon electrode preparation method with multi-layer ladder cracks solves the problem of insufficient hydrophobicity of fuel cell electrodes, achieves high hydrophobicity and good mechanical properties, improves the stability of fuel cells and is suitable for industrial applications.
Patent Information
- Application Number
- CN202410790165.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
AI Technical Summary
The hydrophobic performance of existing fuel cell electrodes is insufficient, resulting in water flooding and a reduction in electrochemical active area, which hinders the industrial application of fuel cells.
A carbon electrode preparation method with multi-layer ladder cracks is used to form a carbon electrode with excellent hydrophobic properties and good mechanical properties by changing the mass ratio and type of polytetrafluoroethylene and commercial carbon black, including ultrasonic dispersion, ultrasonic stirring and high-temperature drying and other steps to form a micron-scale crack structure.
It achieves high hydrophobicity, bending resistance and pressure resistance of the electrode, improves the stability and mechanical properties of the fuel cell, and has a simple preparation process, making it suitable for industrial applications.
Smart Images

Figure CN118825291A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fuel cells, and in particular to a carbon electrode with multi-layered stepped cracks and a preparation method thereof. Background Art
[0002] Fuel cells have the advantages of high efficiency, low pollution, low radiation, high reliability, and easy construction, so they have a wide range of applications. Fuel cells mainly include proton exchange membrane (PEM), catalyst layer (CL), microporous layer (MPL), gas diffusion layer (GDL) and bipolar plate (BP). Among them, the catalyst layer of the electrode is a fine and uniform crack structure visible to the naked eye. In the gas-liquid-solid three-phase reaction system in the fuel cell, if the electrode hydrophobicity is insufficient, water flooding will occur, resulting in a large amount of water blocking the pores of the electrode catalyst layer and the porous transport layer, resulting in a decrease in the electrochemical active area. This series of adverse effects will cause the performance of the fuel cell to decline or even stop working completely. In short, the underwater wettability adjustment of the electrode (with hydrophobicity as the goal) is the key to the overall performance of the battery, especially at the high current density involved in industrial applications. The lack of the necessary anti-electrowetting ability will cause the electrolyte solution to infiltrate the electrode, resulting in the gas channel being blocked and the catalyst active sites being shielded, which will greatly reduce the performance of the fuel cell. This is also an important reason that hinders the industrial application of fuel cells. Therefore, increasing the stability of the fuel cell by improving the hydrophobicity of the electrode is one of the current research focuses.
[0003] An ordered stepped porous carbon electrode and its preparation method with publication number CN117543024A discloses the formation of ordered stepped macropores and randomly distributed small pores inside the electrode, and the formation of gas-liquid separation channels inside the electrode under the action of capillary force, which effectively improves the material transfer efficiency inside the electrode. At the same time, the invention can also adjust the balance of liquid water inside the electrode through ordered stepped macropores, retain liquid water under low pressure conditions to meet the hydration of the proton exchange membrane, and effectively remove excess liquid water under high pressure conditions to prevent flooding inside the battery, thereby improving the electrochemical performance of the battery. However, the preparation process of this solution is complicated, and the mechanical properties such as poor bending resistance and poor compression resistance are poor, which is not conducive to industrial application.
[0004] In the literature Optimizing the hydrophobicity of GDL to improve the fuel cell performance, Zhou Ke et al. prepared a GDL with dual MPL. By rationally distributing the content of polytetrafluoroethylene (PTFE) and carbon black, the GDL was subjected to gradient hydrophobic treatment, which can improve the electrode hydrophobicity to a certain extent and obtain better water management capabilities. However, it has the disadvantages of unclear stratification of the catalyst layer structure and limited improvement in hydrophobicity.
[0005] The document Anti-electrowetting carbon film electrode with self-sustained aeration for industrial H2O2 electrosynthesis, Lele Cui et al., demonstrated the concept of an anti-electrowetting carbon film electrode, which exhibits good underwater hydrophobicity by structurally discontinuously destroying the traditional planar electrocatalyst membrane. However, the invention is limited by its single-layer structure. In order to form a specific crack structure, the PTFE doping amount of its catalyst layer is almost unadjustable. Excessive use of PTFE not only improves the hydrophobicity of the electrode, but also has the risk of blocking the active sites of the catalyst carbon.
[0006] Therefore, there is an urgent need for a carbon electrode with the advantages of simple preparation process, good mechanical properties and excellent electrode hydrophobicity. Summary of the invention
[0007] The purpose of the present invention is to provide a carbon electrode with multi-layer stepped cracks and a preparation method thereof, which can ensure excellent electrode hydrophobicity, have a large controllable range of the air flow channel, and a simple preparation process. The obtained carbon electrode has good mechanical properties and a micron-level crack structure, and also improves the stability of the fuel cell.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] A method for preparing a carbon electrode having multi-layer stepped cracks comprises the following steps:
[0010] S1, ultrasonically dispersing polytetrafluoroethylene in a solvent to obtain a mixed suspension;
[0011] S2, mixing the mixed suspension obtained in step S1 and commercial carbon black with ultrasonic stirring to obtain a coating slurry 1;
[0012] S3, coating the coating slurry 1 on the support layer, and drying at high temperature to obtain a carbon electrode with a layer of cracks;
[0013] S4, changing the mass ratio of polytetrafluoroethylene to commercial carbon black or changing the type of commercial carbon black n times, repeating steps S1-S2, to obtain coating slurry n+1, where n is a natural number greater than or equal to 1;
[0014] S5, coating the coating slurry n+1 on the carbon electrode having n layers of cracks, and drying at high temperature to obtain a carbon electrode having n+1 layers of stepped cracks.
[0015] Furthermore, the solvent includes ethanol and dimethylacetamide.
[0016] Furthermore, the support layer is selected from any one of commercial carbon paper, commercial carbon cloth, and steel mesh.
[0017] Furthermore, the coating adopts any one of gravure coating, reverse roller coating, knife roller coating, metering rod coating, slot die coating, dipping, curtain coating, and air knife coating processes.
[0018] Furthermore, the coating slurry 1 or n has a thickness of 0.1 mm to 1.5 mm.
[0019] Furthermore, the amount of the solvent used is 2 ml to 10 ml per 100 mg of carbon black.
[0020] Furthermore, the ultrasonic stirring temperature range is 30°C-70°C, and the rotation speed is 100r / min-500r / min.
[0021] Furthermore, the high temperature drying temperature is 150°C-500°C, and the drying time is 0.5h-12h.
[0022] Furthermore, the carbon black is commercial carbon black, and the commercial carbon black includes any one of Cabot carbon black EC300JD, Cabot carbon black XC-72R, XC-72, Ketjen black carbon powder ECP600J, Ketjen black EC300J, graphene, multi-walled carbon nanotubes, and amino multi-walled carbon nanotubes.
[0023] The present invention also provides a carbon electrode with multiple layers of stepped cracks, which is prepared by the method for preparing the carbon electrode with multiple layers of stepped cracks.
[0024] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects: the carbon electrode with multi-layer ladder cracks provided by the present invention and the preparation method thereof, by changing the mass ratio of carbon black to PTFE, the type of carbon black, the type of solvent, etc., a carbon electrode with a multi-layer crack structure is obtained, which not only increases the roughness of the electrode surface, but also forms an ordered ladder large crack layer and a small crack layer inside the electrode, thereby obtaining excellent hydrophobic properties. Moreover, the obtained carbon electrode has good mechanical properties such as bending resistance and compression resistance, good anti-electrowetting ability, and good battery stability. The electrode crack width obtained by the present invention can be adjusted in the range of 10μm-260μm, which is a micron-level crack structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0026] Figure 1 This is an optical photograph of a double-layer cracked carbon electrode having a two-layer crack structure in Example 1 of the present invention;
[0027] Figure 2 This is a SEM photo of a double-layer cracked carbon electrode having a two-layer crack structure in Example 1 of the present invention;
[0028] Figure 3 This is a photograph of the static hydrophobic angle θ1 of the double-layer crack carbon electrode with a two-layer crack structure in Example 1 of the present invention;
[0029] Figure 4 This is an optical photograph of a carbon electrode with three layers of graded cracks prepared in Example 2 of the present invention;
[0030] Figure 5 This is a SEM photo of a carbon electrode with three layers of stepped cracks prepared in Example 2 of the present invention;
[0031] Figure 6 This is a cross-sectional SEM photograph of a carbon electrode having three layers of stepped cracks prepared in Example 2 of the present invention;
[0032] Figure 7 This is an optical photograph of a double-layer cracked carbon electrode with the same crack structure prepared in Example 3 of the present invention;
[0033] Figure 8 This is a SEM photo of a double-layer cracked carbon electrode with the same crack structure prepared in Example 3 of the present invention;
[0034] Fig. 9 A photograph of the static hydrophobic angle θ2 of the double-layer cracked carbon electrode with the same crack structure prepared in Example 3 of the present invention;
[0035] Fig.10 This is an optical photograph of a single-layer cracked carbon electrode having a first-layer crack structure prepared in Comparative Example 1 of the present invention;
[0036] Fig.11 This is a SEM photograph of a single-layer cracked carbon electrode having a first-layer crack structure prepared in Comparative Example 1 of the present invention;
[0037] Fig.12 This is a photograph of the static hydrophobic angle θ3 of the single-layer crack carbon electrode having only the first layer of crack structure prepared in Comparative Example 1 of the present invention;
[0038] Fig.13 This is an optical photograph of a single-layer cracked carbon electrode having only a second layer of crack structure prepared in Comparative Example 2 of the present invention;
[0039] Fig.14This is a SEM photograph of a single-layer cracked carbon electrode having only a second layer of crack structure prepared in Comparative Example 2 of the present invention;
[0040] Fig.15 This is a photograph of the static hydrophobic angle θ4 of the single-layer crack carbon electrode having only the second layer of crack structure prepared in Comparative Example 2 of the present invention;
[0041] Fig.16 This is a surface morphology diagram of the electrode after bending and shearing according to an embodiment of the present invention;
[0042] Fig.17 This is a photograph of the static hydrophobic angle θ5 of the carbon electrode with three layers of stepped cracks prepared in Example 2 of the present invention;
[0043] Fig.18 The present invention is a flow chart of a method for preparing a carbon electrode having multi-layer stepped cracks. DETAILED DESCRIPTION
[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] The purpose of the present invention is to provide a carbon electrode with multi-layer stepped cracks and a preparation method thereof. Under the premise of ensuring excellent electrode hydrophobicity, the air flow channel has a large controllable range and a simple preparation process. The obtained carbon electrode has good mechanical properties and a micron-level crack structure, which also improves the stability of the fuel cell.
[0046] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0047] like Fig.18 As shown, a method for preparing a carbon electrode with multi-layered stepped cracks provided by an embodiment of the present invention comprises the following steps:
[0048] S1, ultrasonically dispersing polytetrafluoroethylene in a solvent to obtain a mixed suspension;
[0049] S2, mixing the mixed suspension obtained in step S1 and commercial carbon black with ultrasonic stirring to obtain a coating slurry 1;
[0050] S3, coating the coating slurry 1 on the support layer, and drying at high temperature to obtain a carbon electrode with a layer of cracks;
[0051] S4, changing the mass ratio of polytetrafluoroethylene to commercial carbon black or changing the type of commercial carbon black n times, repeating steps S1-S2, to obtain coating slurry n+1, where n is a natural number greater than or equal to 1;
[0052] S5, coating the coating slurry n+1 on the carbon electrode having n layers of cracks, and drying at high temperature to obtain a carbon electrode having n+1 layers of stepped cracks.
[0053] In this embodiment, the solvent includes alcohol solvents such as methanol, ethanol, propanol, as well as water, tetrahydrofuran, dimethylacetamide, etc. The solvent needs to meet the following conditions: 1. It has good dispersibility for carbon black. Generally speaking, polar solvents are more conducive to the dispersion of carbon black; 2. It is miscible with water; 3. The pH is neutral or weakly alkaline (between pH 7-9).
[0054] In this embodiment, the support layer is selected from any one of commercial carbon paper, commercial carbon cloth, and steel mesh.
[0055] In this embodiment, the coating process can be any one of gravure coating, reverse roller coating, knife roller coating, metering rod coating, slot die coating, dipping, curtain coating, and air knife coating.
[0056] In this embodiment, the thickness of the coating slurry 1 or n is 0.1 mm-1.5 mm.
[0057] In this embodiment, the amount of the solvent used is 2 ml to 10 ml per 100 mg of carbon black.
[0058] In this embodiment, the ultrasonic stirring temperature ranges from 30°C to 70°C, and the rotation speed ranges from 100r / min to 500r / min.
[0059] In this embodiment, the high temperature drying temperature is 150° C.-500° C., and the drying time is 0.5 h-12 h.
[0060] In this embodiment, the carbon black is commercial carbon black, and the commercial carbon black includes any one of Cabot carbon black EC300JD, Cabot carbon black XC-72R, XC-72, Ketjen black carbon powder ECP600J, Ketjen black EC300J, graphene, multi-walled carbon nanotubes, and amino multi-walled carbon nanotubes.
[0061] The embodiment of the present invention further provides a carbon electrode with multiple layers of stepped cracks, which is prepared by the method for preparing the carbon electrode with multiple layers of stepped cracks.
[0062] Example 1
[0063] In this embodiment, when n is 1, the method for preparing the carbon electrode having multiple layers of stepped cracks specifically includes:
[0064] Step 1, weigh 1.2 g PTFE (60% wt) and add it to 70 ml anhydrous ethanol, place it in an ultrasonic cleaning machine and continue ultrasonication for 20 min to obtain a uniformly dispersed milky white suspension;
[0065] Step 2: Mix the solution obtained in step 1 and 1 g of commercial carbon black, place in an ultrasonic cleaning machine, and set mechanical stirring, that is, continue ultrasonic stirring for 120 minutes at a temperature of 50° C. and a speed of 300 r / min to obtain a uniformly dispersed solution, that is, coating slurry 1;
[0066] Step 3: Use an automatic coating machine to evenly coat the coating slurry 1 obtained in step 2 on a 3 cm×4 cm carbon paper (Kawamori). Set the coating height to 1 mm.
[0067] Step 4: Immediately transfer the electrode coated in step 3 to a muffle furnace and dry it at 300° C. for 120 min to obtain a single-layer cracked carbon electrode with a single-layer crack structure.
[0068] Step 5, weigh 0.6 g PTFE (60% wt) and add it to 60 ml anhydrous ethanol, place it in an ultrasonic cleaning machine and continue ultrasonication for 20 minutes to obtain a uniformly dispersed milky white suspension;
[0069] Step 6: Mix the milky white suspension obtained in step 5 with 1 g of commercial carbon black, place in an ultrasonic cleaning machine, and set mechanical stirring, that is, stirring temperature 30° C., speed 500 r / min, and continue ultrasonic stirring for 180 min to obtain a uniformly dispersed solution, that is, coating slurry 2;
[0070] Step 7, using an automatic coating machine, setting the coating height to 0.3 mm, and evenly coating the coating slurry 2 on the single-layer cracked carbon electrode in step 4;
[0071] Step 8: Immediately transfer the electrode coated in step 7 to a muffle furnace and dry it at 150° C. for 60 min to obtain a double-layer cracked carbon electrode with a two-layer crack structure.
[0072] In the double-layer cracked carbon electrode having both the first layer and the second layer crack structure prepared in Example 1, the first layer crack width ranges from 50 to 100, and the second layer crack width ranges from 10 to 20. The optical photograph of the electrode is as follows: Figure 1 , SEM photos are shown in Figure 2 , the static hydrophobic angle θ1 is shown in the following figure Figure 3 It can be seen that the present invention can obtain an upper and lower double-layer crack carbon electrode with different structures, and the upper crack can cover the lower crack.
[0073] Example 2
[0074] In this embodiment, when n=2, the method for preparing the carbon electrode with multi-layered stepped cracks specifically includes:
[0075] Step 1, ultrasonically disperse 1.2 g PTFE (60% wt) in 60 ml anhydrous ethanol, place in an ultrasonic cleaning machine and continue ultrasonication for 20 min to obtain a uniformly dispersed milky white suspension;
[0076] Step 2, placing the milky white mixed solution obtained in step 1 and 1 g of commercial carbon black in an ultrasonic cleaning machine, and setting mechanical stirring, that is, continuously ultrasonically stirring for 120 min at a temperature of 50° C. and a rotation speed of 300 r / min to obtain a uniformly dispersed solution, that is, coating slurry 1;
[0077] Step 3: The coating slurry 1 obtained in step 2 is evenly coated on a 3 cm × 4 cm carbon paper (Hesen) using an automatic coating machine with a coating height of 1 mm;
[0078] Step 4, immediately transferring the electrode coated in step 3 to a muffle furnace and drying at 300° C. for 120 min to obtain a single-layer cracked carbon electrode having a crack structure;
[0079] Step 5, weigh 0.6 g PTFE (60% wt) and add it to 30 ml anhydrous ethanol, place it in an ultrasonic cleaning machine and continue ultrasonication for 20 min to obtain a uniformly dispersed milky white suspension;
[0080] Step 6: Mix the milky white suspension obtained in step 5 with 1 g of commercial carbon black, place in an ultrasonic cleaning machine, and set mechanical stirring, that is, stirring temperature 50° C., speed 500 r / min, and continue ultrasonic stirring for 180 min to obtain a uniformly dispersed solution, that is, coating slurry 2;
[0081] Step 7, using an automatic coating machine, setting the coating height to 0.6 mm, and evenly coating the coating slurry 2 on the single-layer cracked carbon electrode in step 4;
[0082] Step 8, immediately transfer the electrode coated in step 7 to a muffle furnace and dry at 150° C. for 60 min to obtain a carbon electrode with two layers of stepped cracks;
[0083] Step 9, weigh 0.3 g PTFE (60% wt) and add it to 15 ml anhydrous ethanol, place it in an ultrasonic cleaning machine and continue ultrasonication for 20 minutes to obtain a uniformly dispersed milky white suspension;
[0084] Step 10, the milky white suspension obtained in step 5 and 1 g of commercial carbon black are mixed, placed in an ultrasonic cleaning machine, and set to mechanical stirring, that is, the stirring temperature is 50° C. and the speed is 500 r / min for continuous ultrasonic stirring for 180 min to obtain a uniformly dispersed solution, that is, coating slurry 3;
[0085] Step 11, coating the coating slurry 3 on the two-layer cracked carbon electrode obtained in step 8, and then immediately transferring it to a muffle furnace and drying it at a high temperature of 150°C for 60 minutes to obtain a carbon electrode with three layers of graded cracks, the optical photograph of which is as follows: Figure 4 , surface SEM photos are as follows Figure 5 , cross-sectional SEM photos are shown in Figure 6 , static hydrophobic angle photo θ5 as Fig.17 It can be seen that the carbon electrode with three layers of cracks obtained in this example has a clearly visible hierarchical multi-layer structure with different crack widths.
[0086] Example 3
[0087] This embodiment is still a method for preparing a carbon electrode with multi-layered graded cracks when n=1, and adopts the same steps 1 to 4 as in Embodiment 1. The difference from Embodiment 1 is that after Step 4, the following steps are further included:
[0088] Step 5, using an automatic coating machine, setting the coating height to 1.0 mm, and uniformly coating the coating slurry 1 in step 2 of Example 1 on the single-layer crack electrode in step 4;
[0089] Step 6: Immediately transfer the electrode coated in step 5 to a muffle furnace and dry it at 300° C. for 120 min to obtain a double-layer crack carbon electrode with a two-layer crack structure.
[0090] In the double-layer cracked carbon electrode having both the first layer and the second layer crack structure prepared in Example 3, the first layer crack width ranges from 50 to 150, and the second layer crack width ranges from 50 to 150. The optical photograph of the electrode is as follows: Figure 7 , SEM photos are shown in Figure 8 , the static hydrophobic angle θ2 is shown in the following figure Fig. 9 It can be seen that the present invention can obtain a double-layer cracked carbon electrode with the same structure, and the upper crack can cover the lower crack without affecting the structure of the lower crack.
[0091] Comparative Example 1
[0092] The difference between this comparative example 1 and example 1 is that the steps of preparing and coating the second layer of catalyst are omitted, that is, the difference is:
[0093] Step A1, using an automatic coating machine, setting the coating height to 0.6 mm, and evenly coating the coating slurry 1 obtained in step 2 of Example 1 on a 3 cm×4 cm carbon paper (Hesen);
[0094] Step A2, immediately transferring the electrode coated in step A1 to a muffle furnace, and drying at 300° C. for 120 min to obtain a single-layer cracked carbon electrode having only the first layer of crack structure;
[0095] In the first layer of the single-layer crack electrode prepared in Comparative Example 1, the single-layer crack carbon electrode having only the first layer of crack structure prepared in Comparative Example 1 has a crack width ranging from 50 to 150. The optical photograph of the electrode is as follows: Fig.10 , SEM photos are shown in Fig.11 , the static hydrophobic angle θ3 is shown in the following figure Fig.12 .
[0096] Comparative Example 2
[0097] The difference between this comparative example 2 and example 1 is that this comparative example 2 does not use steps 1-4 in example 1, but only uses the coating slurry 2 obtained in step 6 to obtain a single-layer cracked carbon electrode - a single-layer cracked carbon electrode having only a second layer of crack structure, that is, the preparation steps of this comparative example 2 are:
[0098] Step B1, weigh 0.6 g PTFE (60% wt) and add it to 60 ml anhydrous ethanol, place it in an ultrasonic cleaning machine and continue ultrasonication for 20 min to obtain a uniformly dispersed milky white suspension;
[0099] Step B2, the milky white suspension obtained in step 5 and 1 g of commercial carbon black are mixed, placed in an ultrasonic cleaning machine, and mechanical stirring is set, that is, the stirring temperature is 30° C. and the speed is 500 r / min, and continuous ultrasonic stirring is performed for 180 min to obtain a uniformly dispersed solution, that is, coating slurry 2;
[0100] Step B3, using an automatic coating machine, setting the coating height to 0.3 mm, the coating slurry 2 obtained in step 6 of Example 1 is evenly coated on a 3 cm×4 cm carbon paper (Hesen);
[0101] Step B4, immediately transferring the electrode coated in step B3 to a muffle furnace and drying at 150° C. for 60 min to obtain a single-layer cracked carbon electrode having only a second layer of crack structure;
[0102] In the single-layer crack carbon electrode with only the second crack structure prepared in Comparative Example 2, the crack width ranges from 10 to 30. The optical photograph of the electrode is as follows: Fig.13 , SEM photos are shown in Fig.14 , the static hydrophobic angle θ4 is shown in the following figure Fig.15 .
[0103] pass Figure 1 , Fig.10 , Fig.13 It can be seen that the double-layer cracked carbon electrode obtained in Example 1 retains the crack structure of the first single-layer cracked electrode and the second single-layer cracked electrode. Figure 2 , Fig.11 , Fig.14 It can be seen that the width range of the lower crack of the double-layer crack electrode obtained in Example 1 is basically consistent with that of the corresponding single-layer crack electrode. Figure 3 , Fig.12 , Fig.15 It can be seen that the hydrophobicity of the double-layer crack electrode obtained in Example 1 is better than that of the first single-layer crack electrode obtained in Comparative Example 1 and the second single-layer crack electrode obtained in Comparative Example 2.
[0104] pass Figure 7 , Fig.10 It can be seen that the upper crack structure and the lower crack structure of the double-layer crack electrode obtained in Example 3 are similar to the crack structure of the single-layer crack electrode in Comparative Example 2. Figure 8 , Fig.11 It can be seen that the width range of the cracks in the upper and lower layers of the double-layer crack electrode is basically consistent with that of the single-layer crack electrode in Comparative Example 2. Fig. 9 , Fig.12 It can be seen that the hydrophobicity of the double-layer crack electrode obtained in Example 1 is similar to that of the single-layer crack electrode obtained in Comparative Example 1. In short, while doubling the amount of catalyst loaded on the electrode, the structure and hydrophobicity of the crack electrode can be kept unchanged.
[0105] Reliability verification of carbon electrodes with multi-layer stepped cracks: Figure 4 , Figure 5 , Figure 6 It can be seen that in the three-layer crack electrode obtained in Example 2, the first layer crack structure, the second layer crack structure and the third layer crack structure are clearly visible, and the layers are obvious, presenting a hierarchical arrangement structure.
[0106] pass Figure 3 , Fig. 9 , Fig.12 , Fig.15 , Fig.17 It can be seen that multilayer crack electrodes with different hydrophobic properties can be obtained by adjusting the crack structure of each layer.
[0107] In summary, the method for preparing a carbon electrode with multi-layered tiered cracks provided by the present invention obtains a carbon electrode with a double-layer or more-layered crack structure by changing the mass ratio of carbon black to PTFE, the type of carbon black, the type of solvent, etc., so that the catalyst crack distribution obtained is a tiered multi-layer structure with large cracks in the lower layer and small cracks in the upper layer. The present invention not only has the advantages of good mechanical properties such as strong hydrophobicity, resistance to bending and compression, but also has the characteristics of flexible and changeable controllability. In practical applications, not only can the preparation parameters and target performance of the first layer catalyst and the second layer catalyst be designed separately according to actual use requirements, but also the third layer catalyst or even more multi-layer structures can be combined, and the preparation process is very simple, which is not available in similar products at present, and is convenient for industrial application. The present invention solves the problems existing in the prior art well:
[0108] 1. The present invention not only has a simple preparation method, but also has good bending and compression resistance (through Fig.16 It can be seen that after bending and shearing, the surface structure of the electrode does not change significantly), and it can even be sheared arbitrarily without affecting its multilayer structure and the morphology of the crack surface.
[0109] 2. The catalyst layer obtained by the present invention not only has a multi-layer structure with clear boundaries, but also has better hydrophobicity, and the airflow channel obtained through the cracks has a wider controllable range (up to 260 microns and down to 10 microns, that is, a micron-level crack structure is obtained).
[0110] 3. By setting up a multi-layered stepped crack structure, even if the amount of surface catalyst PTFE is reduced, the hydrophobicity of the electrode will not be reduced. Even within a certain range, the carbon black loading amount and type of carbon black of catalysts at different levels can be adjusted, which can be more widely used in industrial applications.
[0111] The remaining technical features in this embodiment can be flexibly selected by those skilled in the art according to actual conditions to meet different specific practical needs. However, it is obvious to those skilled in the art that it is not necessary to adopt these specific details to implement the present invention. In other examples, in order to avoid confusing the present invention, the well-known components, structures or parts are not specifically described, which are all within the technical protection scope defined by the technical solution claimed for protection in the claims of the present invention.
[0112] Modifications and changes made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the scope of protection of the claims attached to the present invention. In the above description, a large number of specific details are set forth in order to provide a thorough understanding of the present invention. However, it is obvious to those of ordinary skill in the art that these specific details are not necessary to practice the present invention. In other examples, in order to avoid confusing the present invention, well-known technologies, such as specific construction details, operating conditions and other technical conditions, are not described in detail.
[0113] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing a carbon electrode having multi-layered stepped cracks, characterized in that: The following steps are involved: S1, ultrasonically dispersing polytetrafluoroethylene in a solvent to obtain a mixed suspension; S2, mixing the mixed suspension obtained in step S1 and carbon black with ultrasonic stirring to obtain a coating slurry 1; S3, coating the coating slurry 1 on the support layer, and drying at high temperature to obtain a carbon electrode with a layer of cracks; S4, changing the mass ratio of polytetrafluoroethylene to commercial carbon black or changing the type of carbon black n times, repeating steps S1-S2, to obtain coating slurry n+1, where n is a natural number greater than or equal to 1; S5, coating the coating slurry n+1 on the carbon electrode having n layers of cracks, and drying at high temperature to obtain a carbon electrode having n+1 layers of stepped cracks.
2. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The solvent includes ethanol and dimethylacetamide.
3. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The support layer can be selected from any one of commercial carbon paper, commercial carbon cloth and steel mesh.
4. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The coating is carried out by any one of gravure coating, reverse roller coating, knife roller coating, metering rod coating, slot die coating, dipping, curtain coating and air knife coating processes.
5. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The thickness of the coating slurry 1 or n is 0.1 mm-1.5 mm.
6. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The amount of the solvent used is 2 ml to 10 ml of the corresponding amount of solvent per 100 mg of carbon black.
7. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The ultrasonic stirring temperature range is 30°C-70°C, and the rotation speed is 100r / min-500r / min.
8. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The temperature of high temperature drying is 150℃-500℃, and the drying time is 0.5h-12h.
9. The method for preparing a carbon electrode having multi-layered stepped cracks according to claim 1, characterized in that: The carbon black is commercial carbon black, which includes any one of Cabot carbon black EC300JD, Cabot carbon black XC-72R, XC-72, Ketjen black carbon powder ECP600J, Ketjen black EC300J, graphene, multi-walled carbon nanotubes, and amino multi-walled carbon nanotubes.
10. A carbon electrode having multi-layered stepped cracks, characterized in that: The carbon electrode is prepared by the method for preparing a carbon electrode having multi-layer stepped cracks as described in any one of claims 1-9.
Citation Information
Patent Citations
Ordered stepped porous carbon electrode and preparation method thereof
CN117543024A