Perovskite precursor solution, cell, preparation method, photovoltaic module and system
By adding thiol chelating agents and other compounds to the perovskite precursor solution, the internal defects of the perovskite film are deeply passivated, which solves the problem that the interface passivation material cannot penetrate deeply and improves the photoelectric conversion efficiency of the perovskite solar cell.
Patent Information
- Application Number
- CN202411229314.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-10-22
AI Technical Summary
The interface passivation material in existing perovskite solar cells cannot penetrate deep into the internal defects of the passivation film, causing carrier transmission to be blocked and affecting photoelectric conversion efficiency.
Add thiol chelating agents and compounds containing carbon-oxygen or phosphorus-oxygen double bonds as additives to the perovskite precursor solution to deeply passivate the internal defects of the perovskite film and avoid the formation of a two-dimensional structure on the surface. A specific chromatographic structure and Process for preparing perovskite solar cells.
It achieves deep passivation of the perovskite film, avoids carrier transmission obstruction, and significantly improves photoelectric conversion efficiency and solar cell performance.
Smart Images

Figure CN118829338A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a perovskite precursor solution, a perovskite solar cell and a preparation method thereof, a photovoltaic module, and a photovoltaic system. Background Art
[0002] Due to their excellent photoelectric properties, perovskite materials can be used to prepare perovskite films and applied in perovskite solar cells.
[0003] The perovskite film in conventional perovskite solar cells needs to be passivated using interface passivation materials. However, the interface passivation materials cannot penetrate into the defects inside the passivation film, and the surface interface passivation materials easily form a two-dimensional structure on the surface of the perovskite film, causing the perovskite solar cell to have problems with hindering carrier transport, thereby affecting the improvement of photoelectric conversion efficiency.
[0004] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention
[0005] The embodiments of the present application provide a perovskite precursor solution, a perovskite solar cell and a method for preparing the same, a photovoltaic module, and a photovoltaic system to solve or alleviate one or more of the technical problems raised above.
[0006] A first aspect of an embodiment of the present application provides a perovskite precursor solution, comprising:
[0007] Perovskite material, perovskite material is ABX 3 structure;
[0008] Organic solvents;
[0009] The additives include a mercapto chelating agent, and the mercapto chelating agent is used to passivate the perovskite material.
[0010] Optionally, the thiol chelating agent is a small molecule thiol chelating agent; wherein the molecular weight of the small molecule thiol chelating agent is 47-274.
[0011] Optionally, the small molecule mercapto chelating agent includes one or more of thioglycolic acid, mercaptosuccinic acid, dimercaptosuccinic acid, dimercaptopropanol or sodium dimercaptopropane sulfonate.
[0012] Optionally, the additive further includes: one or both of a compound containing a carbon-oxygen double bond and a compound containing a phosphorus-oxygen double bond.
[0013] Optionally, the compound containing a carbon-oxygen double bond includes one or more of acetylacetone, diacetyl methane and phenethyl dione;
[0014] The compound containing a phosphorus-oxygen double bond includes one or both of ethylenediaminephosphonic acid and oxadiazolephosphonic acid.
[0015] Optionally, the molar concentration ratio of the additive to the perovskite material is 1:10 5 ~1:10.
[0016] Optionally, A is a monovalent cation, including a mixture of one or several monovalent cations selected from cesium, rubidium, methylamine, and methylamidine; B is a divalent cation, including a mixture of one or several divalent cations selected from lead, copper, zinc, gallium, tin, and calcium; and X is a monovalent anion, including a mixture of one or several monovalent anions selected from iodine, bromine, chlorine, fluorine, and thiocyanate.
[0017] Optionally, the organic solvent includes one or more of acetonitrile, 2-methoxyethanol, dimethylacetamide, and N,N'-dimethylpropyleneurea.
[0018] In a second aspect, an embodiment of the present application provides a method for preparing a perovskite solar cell, comprising:
[0019] providing a conductive substrate;
[0020] forming a hole transport layer on the upper surface of the conductive substrate;
[0021] Placing a perovskite precursor solution as provided in the previous embodiment on the upper surface of the hole transport layer to form a perovskite light absorbing layer;
[0022] An electron transport layer and an electrode are sequentially formed on the upper surface of the perovskite light absorbing layer.
[0023] In a third aspect, an embodiment of the present application provides a perovskite solar cell, comprising a conductive substrate, a hole transport layer, a perovskite light absorbing layer, an electron transport layer, a modification layer and an electrode stacked in sequence; the perovskite light absorbing layer is prepared from the perovskite precursor solution of any implementation aspect of the above embodiments.
[0024] In a fourth aspect, an embodiment of the present application provides a photovoltaic module, comprising: at least one battery string, the battery string comprising at least two perovskite solar cells of any one of the above items.
[0025] In a fifth aspect, an embodiment of the present application provides a photovoltaic system, comprising the above-mentioned photovoltaic assembly.
[0026] The above technical solution adopted in the embodiment of the present application may have the following advantages:
[0027] The technical solution of the embodiment of the present application prepares a perovskite film by adding a passivation material to a perovskite precursor solution, which can achieve deep passivation of internal defects of the perovskite film and will not form a two-dimensional structure on the surface of the perovskite film, thereby avoiding the situation of hindering carrier transmission, improving the photoelectric conversion efficiency, and thus improving the performance of perovskite solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0029] Figure 1 A flow chart schematically shows a method for preparing a perovskite solar cell provided in an embodiment of the present application;
[0030] Figure 2 The structural diagram of the perovskite solar cell provided in the embodiment of the present application is schematically shown. DETAILED DESCRIPTION
[0031] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0032] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.
[0033] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0034] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0035] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.
[0036] The embodiment of the present application provides a perovskite precursor solution. The perovskite precursor solution can be used to prepare a perovskite film, and the perovskite film can be used as a light-absorbing layer in a perovskite solar cell to convert light energy into electrical energy.
[0037] The perovskite precursor solution comprises: a perovskite material, an organic solvent and an additive.
[0038] (1) Perovskite materials:
[0039] Perovskite materials have a wide light absorption spectrum, can absorb most of the solar spectrum, have high photoelectric conversion efficiency, and are low in cost, so they can be used to prepare solar cells.
[0040] In one example, the perovskite material may include one or more of cesium bromide, lead iodide, and lead bromide.
[0041] Specifically, the perovskite material is ABX 3 Structure, which is a crystal structure with high symmetry, good adjustability and stability. Among them, A is a monovalent cation, including one or a mixture of monovalent cations of cesium, rubidium, methylamine, and methylamidine; B is a divalent cation, including one or a mixture of divalent cations of lead, copper, zinc, gallium, tin, and calcium; X is a monovalent anion, including one or a mixture of monovalent anions of iodine, bromine, chlorine, fluorine, and thiocyanate.
[0042] (2) Organic solvents:
[0043] Organic solvent, the organic solvent is used to dissolve the perovskite material.
[0044] In one example, the organic solvent may include one or more of acetonitrile, 2-methoxyethanol, dimethylacetamide, and N,N′-dimethylpropyleneurea.
[0045] (3) Additives:
[0046] The additive may include a mercapto chelating agent, which is used to passivate the perovskite material. A chelating agent is an organic compound that can form a stable complex with metal ions, and a mercapto chelating agent specifically refers to a chelating agent containing a mercapto (-SH) functional group.
[0047] There are some structural defects inside the perovskite material, including insufficient lead coordination, which leads to the distortion of the perovskite crystal structure. Specifically, in the structure of the perovskite material, the lead atom is coordinated with six halogen atoms (which can be iodine atoms) to form an octahedral structure. However, due to various reasons, such as iodine vacancies, insufficient lead coordination may occur. Insufficient lead coordination may destroy the lattice structure of the perovskite material, resulting in lattice distortion, making the perovskite material more susceptible to environmental factors such as light, temperature, and humidity, resulting in a decrease in material performance and a shortened battery life.
[0048] The embodiment of the present application uses a mercapto chelating agent to passivate the perovskite material. This is because the mercapto group has a strong complexing property and can coordinate with the lead in the perovskite material, thereby alleviating the problem of lattice distortion caused by insufficient lead coordination as mentioned above. Therefore, it can be used to passivate the perovskite material. In addition, the mercapto chelating agent can passivate the internal defects of the perovskite material without forming a passivation layer on the surface of the perovskite film. Therefore, a two-dimensional structure will not be formed on the surface of the perovskite film, thereby avoiding the situation of hindering carrier transmission and improving the photoelectric conversion efficiency.
[0049] In one example, the thiol chelating agent is a small molecule thiol chelating agent, which is easily dissolved in the perovskite precursor solution. The molecular weight of the small molecule thiol chelating agent is 47 to 274. For example, the molecular weight of the small molecule thiol chelating agent can be 47, 76, 150, 182 or 274.
[0050] In one example, the small molecule mercapto chelating agent may include one or more of thioglycolic acid, thiosuccinic acid, dimercaptosuccinic acid, dimercaptopropanol, or sodium dimercaptopropane sulfonate.
[0051] In this embodiment, a small molecule thiol chelating agent is added as a passivation material to the perovskite precursor solution to prepare a perovskite film, which can achieve deep passivation of internal defects of the perovskite film without forming a two-dimensional structure on the surface of the perovskite film, further alleviating the situation of hindering carrier transport and improving the photoelectric conversion efficiency.
[0052] In one example, the additive in the perovskite precursor solution may also include one or both of a compound containing a carbon-oxygen double bond and a compound containing a phosphorus-oxygen double bond. Since the compound containing a carbon-oxygen double bond and the compound containing a phosphorus-oxygen double bond can both produce strong coordination with the lead ions in the perovskite material, the problem of insufficient coordination of lead ions can be further alleviated, and therefore, they can also be added to the perovskite precursor solution as an additive to passivate the perovskite material.
[0053] In one example, the compound containing a carbon-oxygen double bond may include one or more of acetylacetone, diacetyl methane, and phenethyl dione.
[0054] In one example, the compound containing a phosphorus-oxygen double bond may include one or more of ethylenediaminephosphonic acid and oxadiazolephosphonic acid.
[0055] In this embodiment, a compound containing a carbon-oxygen double bond and / or a compound containing a phosphorus-oxygen double bond is added as an additive to a perovskite precursor solution to prepare a perovskite film, which can passivate the internal defects of the perovskite material without forming a passivation layer on the surface of the perovskite film. Therefore, a two-dimensional structure will not be formed on the surface of the perovskite film, further alleviating the situation of hindering carrier transmission and improving the photoelectric conversion efficiency.
[0056] In one example, the molar concentration ratio of the additive to the perovskite material is 1:10. 5 ~1:10. Exemplarily, the molar concentration ratio of the additive to the perovskite material is 1:10 5 、 1:10 4 , 1:10 3 , 1:10 2 Or 1:50, 1:10.
[0057] In this embodiment, the molar concentration in the above ratio can better passivate the defects in the perovskite material.
[0058] See also Figure 1 The present application embodiment may also provide a method for preparing a perovskite solar cell, comprising:
[0059] Step S100: providing a conductive substrate.
[0060] In the embodiment of the present application, the conductive substrate can be divided into a substrate layer and a conductive layer. The material of the substrate layer may include glass, plastic, etc. to provide mechanical support. The conductive layer may include indium tin oxide, tin fluoride oxide, etc. to transmit photogenerated loads. The photogenerated loads refer to free electrons and holes generated under light irradiation.
[0061] In one example, the conductive substrate may be pre-treated.
[0062] In one example, the pretreatment may include: using any one of deionized water, isopropyl alcohol or ethanol to clean the conductive substrate by ultrasonic cleaning technology, and the cleaning time may be 10 minutes to 60 minutes.
[0063] In one example, the pretreatment may further include: ultraviolet ozone treatment, and the treatment time may be 10 minutes to 60 minutes.
[0064] Step S200: forming a hole transport layer on the upper surface of the conductive substrate.
[0065] In the embodiment of the present application, the hole transport layer is used to collect photogenerated holes and effectively transport them to the external electrodes of the battery.
[0066] In one example, a method of forming a hole transport layer may include: dropping a solution including a hole transport material on a conductive substrate and spin coating the solution, and then performing an annealing process to form the hole transport layer.
[0067] In one example, the hole transport material may include one or more of poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonate), [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz).
[0068] In one example, the rotation speed of the spin coating may be 2000 rpm to 7000 rpm. The annealing temperature may be 100° C. to 180° C., and the annealing time may be 10 min to 40 min.
[0069] Step S300: placing the perovskite precursor solution described in any one of the embodiments of the present application on the upper surface of the hole transport layer to form a perovskite light absorbing layer. The perovskite light absorbing layer can be used to absorb photons in sunlight and convert the photons into photogenerated loads (electrons and holes).
[0070] In one example, forming the perovskite light absorbing layer may include: dropping a perovskite precursor solution onto the upper surface of the hole transport layer and spin coating the solution, and dropping an anti-solvent during the spin coating process.
[0071] Antisolvents can be used to remove some of the solvent residues in the perovskite precursor solution, making the perovskite film denser and more uniform, thereby increasing the film filling rate, reducing defects, and thus improving the efficiency and stability of the battery.
[0072] In one example, the spin coating speed of the spin coating of the perovskite precursor solution may be 2000 rpm to 7000 rpm, the anti-solvent added during the spin coating process may include toluene, and the amount of the anti-solvent added may be 100 μL to 1000 μL.
[0073] In one example, forming the perovskite light absorbing layer may further include annealing treatment, which may promote recrystallization of the perovskite crystals and growth of grains, and improve the crystallinity and orderliness of the crystals, thereby improving the performance of the photoelectric conversion device.
[0074] In one example, the annealing temperature may be 70° C. to 180° C., and the annealing time may be 5 min to 30 min.
[0075] An additive containing a passivation component is added to the perovskite precursor solution, so that an interface passivation layer does not need to be formed on the surface of the perovskite light-absorbing layer.
[0076] Step S400: forming an electron transport layer and an electrode in sequence on the upper surface of the perovskite light absorbing layer.
[0077] The electron transport layer can serve as a channel for electron transport, promoting the migration of photogenerated electrons generated in the perovskite light-absorbing layer to the electrode, thereby forming a current. The electrode divides and transmits the photogenerated electrons to the external circuit, thereby outputting current.
[0078] In one example, the material of the electron transport layer may include C 60 , titanium dioxide and zinc oxide, preferably, the material of the electron transport layer can be C 60 .
[0079] In one example, the process for forming the electron transport layer on the upper surface of the perovskite light absorbing layer may be an evaporation coating method, which specifically includes: placing the semi-finished perovskite solar cell formed above into a vacuum coating apparatus, and when the pressure in the chamber is less than 4×10 -6 Torr, C is evaporated at a specific rate 60 The thickness of the evaporation can be 15nm to 40nm. The specific rate can be Preferably, the specific rate may be
[0080] In one example, the material of the electrode may include silver.
[0081] In one example, the method of forming an electrode on the upper surface of the electron transport layer may include an evaporation coating method. Specifically, the semi-finished perovskite solar cell formed as above is first placed in a vacuum coating apparatus. When the pressure in the chamber is less than 4×10 -6 Torr, start evaporation at a specific rate, and the evaporation thickness can be 50nm to 500nm. The specific rate can be Preferably, the specific rate may be
[0082] In one example, the method for preparing a perovskite solar cell further includes: forming a modification layer between the electron transport layer and the electrode.
[0083] In the embodiments of the present application, the modification layer can be used to modify the contact interface between the electron transport layer and the electrode to improve the electron collection ability at the interface, thereby improving the electron collection rate of the electrode in the perovskite solar cell, effectively improving the photoelectric conversion efficiency of the perovskite solar cell.
[0084] In one example, the material of the modification layer may be 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP).
[0085] In one example, the method for forming the modification layer may include vacuum evaporation. Specifically, the battery may be placed in a vacuum coating apparatus. When the pressure in the chamber is less than 4×10 -6 Torr, a BCP film is deposited on the upper surface of the electron transport layer at a specific rate, and the thickness of the film can be 5nm to 15nm. The specific rate can be Preferably, the specific rate is
[0086] An embodiment of the present application also provides a perovskite solar cell, comprising a conductive substrate, a hole transport layer, a perovskite light absorbing layer, an electron transport layer, a modification layer and an electrode stacked in sequence; wherein the perovskite light absorbing layer is prepared from a perovskite precursor solution of any of the above embodiments.
[0087] like Figure 2 As shown, the perovskite solar cell may include: a conductive substrate 111 , a hole transport layer 112 , a perovskite light absorption layer 113 , an electron transport layer 114 , a modification layer 115 and an electrode 116 .
[0088] The following will conduct performance tests on the preparation method of the perovskite solar cell provided in the embodiments of the present application and related comparative examples.
[0089] [Example 1]
[0090] A specific preparation method of a perovskite solar cell is:
[0091] S101: The conductive substrate is ultrasonically cleaned with deionized water for 30 minutes.
[0092] S102: Treat the conductive substrate with ultraviolet ozone for 30 minutes.
[0093] S103: poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonate) was dropped onto the upper surface of the conductive substrate, spin-coated at a speed of 4000 rpm, and then placed on a 150° C. hot plate for annealing for 25 min.
[0094] S104: Perovskite materials (FAI, CsBr, PbI 2 、PbBr 2 ) and an organic solvent are uniformly mixed to obtain a mixture, and dithiodiphenylamine is added to the mixture to form a perovskite precursor solution; wherein the molar concentration of FAI is 1.079 mol / L, the molar concentration of CsBr is 0.221 mol / L, and the molar concentration of PbI 2The molar concentration of PbBr is 1.079 mol / L. 2 The molar concentration is 0.221 mol / L, and the molar concentration ratio of dithiodiphenylamine to perovskite material is 1:10 4 .
[0095] S105: Spin coating the perovskite precursor solution at a rotation speed of 4000 rpm, adding 500 μL of toluene during the spin coating process, and then annealing on a substrate at 100° C. for 20 minutes to form a perovskite light absorbing layer.
[0096] S106: Place the substrate with the perovskite light absorbing layer in a vacuum coating apparatus, and when the pressure in the chamber is less than 4×10 -6 Torr, started with At a rate of 1.3 % , 30 nm of C was evaporated on the surface of the perovskite light absorbing layer. 60 , to form an electron transport layer.
[0097] S107: On the surface of the electron transport layer 10 nm of BCP was evaporated at a rate of 1000 Å to form a modified layer.
[0098] S108: On the surface of the modified layer 300 nm of Ag was evaporated at a rate of 100 Å to form an electrode.
[0099] [Example 2]
[0100] The perovskite solar cell of Example 2 is prepared by referring to the preparation method of Example 1, except that in S104 of Example 2: the perovskite material (FAI, CsBr, PbI 2 、PbBr 2 ) and an organic solvent are uniformly mixed to obtain a mixture, and thioglycolic acid is added to the mixture to form a perovskite precursor solution; wherein the molar concentration of FAI is 1.079 mol / L, the molar concentration of CsBr is 0.221 mol / L, and the molar concentration of PbI 2 The molar concentration of PbBr is 1.079 mol / L. 2 The molar concentration of thioglycolic acid is 0.221 mol / L, and the molar concentration ratio of thioglycolic acid to perovskite material is 1:10 4 .
[0101] [Example 3]
[0102] The perovskite solar cell of Example 3 is prepared by referring to the preparation method of Example 1, except that in S104 of Example 3: the perovskite material (FAI, CsBr, PbI 2 、PbBr 2) and an organic solvent are uniformly mixed to obtain a mixture, and dithiodiphenylamine is added to the mixture to form a perovskite precursor solution; wherein the molar concentration of FAI is 1.079 mol / L, the molar concentration of CsBr is 0.221 mol / L, and the molar concentration of PbI 2 The molar concentration of PbBr is 1.079 mol / L. 2 The molar concentration is 0.221 mol / L, and the molar concentration ratio of dithiodiphenylamine to perovskite material is 1:10 3 .
[0103] In order to more clearly illustrate the technical effects of the embodiments of the present application, the present application also points out the structure and preparation method of the perovskite solar cell of Comparative Example 1.
[0104] [Comparative Example 1]
[0105] The perovskite solar cell of Comparative Example 1 is prepared by referring to the preparation method of Example 1, except that in S104 of Comparative Example 1: the perovskite materials (FAI, CsBr, PbI 2 、PbBr 2 ) and an organic solvent are mixed evenly to obtain a perovskite precursor solution; wherein the molar concentration of FAI is 1.079 mol / L, the molar concentration of CsBr is 0.221 mol / L, and the molar concentration of PbI 2 The molar concentration of PbBr is 1.079 mol / L. 2 The molar concentration is 0.221 mol / L.
[0106] The following is a performance test of the perovskite solar cells provided in Examples 1 to 3 of the present application and Comparative Example 1, so as to obtain the short-circuit current density Jsc, open-circuit voltage Voc, fill factor Fill Factor, and photoelectric conversion efficiency PCE of the corresponding battery devices. The test results are shown in Table 1.
[0107] Table 1 Performance test results of perovskite solar cells of Examples 1 to 3 and Comparative Example 1
[0108]
[0109] It can be seen from Table 1 above that compared with Comparative Example 1, the short-circuit current density, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cells of Examples 1 to 3 of the present application are significantly improved, which indicates that the perovskite light-absorbing layer formed by adding mercapto additives in Examples 1 to 3 of the present application has better quality.
[0110] In summary, the embodiments of the present application add a passivation material to the perovskite precursor solution to prepare a perovskite film, thereby achieving deep passivation of internal defects of the perovskite film and not forming a two-dimensional structure on the surface of the perovskite film, thereby avoiding the situation of hindering carrier transport, improving the photoelectric conversion efficiency, and thus improving the performance of the perovskite solar cell.
[0111] The embodiment of the present application may also provide a photovoltaic module (not shown), including at least one battery string, the battery string includes at least two perovskite solar cells as described above, and adjacent perovskite solar cells can be connected together by series welding.
[0112] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components may form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0113] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.
[0114] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when a specific feature, structure or characteristic is described in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0115] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0116] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A perovskite precursor solution, characterized in that: include: Perovskite material, wherein the perovskite material has an ABX3 structure; Organic solvents; The additive comprises a mercapto chelating agent, and the mercapto chelating agent is used for passivating the perovskite material.
2. The perovskite precursor solution according to claim 1, characterized in that The thiol chelating agent is a small molecule thiol chelating agent; wherein the molecular weight of the small molecule thiol chelating agent is 47-274.
3. The perovskite precursor solution according to claim 2, characterized in that The small molecule mercapto chelating agent includes one or more of thioglycolic acid, mercaptosuccinic acid, dimercaptosuccinic acid, dimercaptopropanol or sodium dimercaptopropane sulfonate.
4. The perovskite precursor solution according to claim 1, characterized in that The additive further comprises: one or both of a compound containing a carbon-oxygen double bond and a compound containing a phosphorus-oxygen double bond.
5. The perovskite precursor solution according to claim 4, characterized in that: The compound containing a carbon-oxygen double bond includes one or more of acetylacetone, diacetyl methane and phenylethylenedione; The compound containing a phosphorus-oxygen double bond includes one or both of ethylenediaminephosphonic acid and oxadiazolephosphonic acid.
6. The perovskite precursor solution according to claim 1, characterized in that: The molar concentration ratio of the additive to the perovskite material is 1:10 5 ~1:
10.
7. The perovskite precursor solution according to any one of claims 1 to 6, characterized in that: A is a monovalent cation, including a mixture of one or several monovalent cations selected from cesium, rubidium, methylamine, and formamidinium; B is a divalent cation, including a mixture of one or several divalent cations selected from lead, copper, zinc, gallium, tin, and calcium; and X is a monovalent anion, including a mixture of one or several monovalent anions selected from iodine, bromine, chlorine, fluorine, and thiocyanate.
8. The perovskite precursor solution according to any one of claims 1 to 6, characterized in that: The organic solvent includes one or more of acetonitrile, 2-methoxyethanol, dimethylacetamide, and N,N'-dimethylpropyleneurea.
9. A method for preparing a perovskite solar cell, characterized in that: include: providing a conductive substrate; forming a hole transport layer on the upper surface of the conductive substrate; Placing the perovskite precursor solution according to any one of claims 1 to 8 on the upper surface of the hole transport layer to form a perovskite light absorbing layer; An electron transport layer and an electrode are sequentially formed on the upper surface of the perovskite light absorbing layer.
10. A perovskite solar cell, characterized in that: It comprises a conductive substrate, a hole transport layer, a perovskite light absorbing layer, an electron transport layer, a modification layer and an electrode stacked in sequence; wherein the perovskite light absorbing layer is prepared from the perovskite precursor solution according to any one of claims 1 to 8.
11. A photovoltaic module, characterized in that: include: At least one cell string, the cell string comprising at least two perovskite solar cells as claimed in claim 10.
12. A photovoltaic system, characterized in that: The photovoltaic system comprises the photovoltaic assembly according to claim 11.
Citation Information
Cited By
Perovskite light emitting diode device based on interface reaction activation and preparation method thereof
CN121568497A