4-vinylbenzylamine polymer, preparation and application of 4-vinylbenzylamine polymer in preparation of solar cell

By using 4-vinylbenzylamine polymer to passivate perovskite film defects, the problems of perovskite solar cell film stability and performance are solved, and efficient photovoltaic performance improvement and long-term stability are achieved.

CN118834318AInactive Publication Date: 2024-10-25SHENZHEN HIKING PV TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318063.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Perovskite solar cell films are prone to surface defects during the preparation process, leading to reduced carrier transmission efficiency and device stability problems. In particular, moisture and oxygen are prone to corrode the film and degrade battery performance.

Method used

4-vinylbenzylamine polymer is used as a passivator, which is strongly bonded to the perovskite surface cations through its -NH3+ group, and uses the energy level matching and hydrophobic structure of the polymer to protect the film and reduce surface defects and erosion risks. .

Benefits of technology

It effectively improves the photovoltaic performance and stability of perovskite solar cells. It can maintain 95% initial efficiency even after being stored in a nitrogen environment for up to 1,000 hours, significantly extending the stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118834318A_ABST
    Figure CN118834318A_ABST
Patent Text Reader

Abstract

The invention discloses a 4-vinylbenzylamine polymer, preparation thereof and application of solar cell preparation, and particularly relates to a method for preparing a solar cell by using the 4-vinylbenzylamine polymer, and the method comprises the following steps: step 1, pre-treating a bottom electrode; 2, spin-coating the bottom electrode with a perovskite precursor solution to realize preparation of a perovskite absorption layer; 3, preparing a passivating agent solution through a 4-vinyl benzylamine polymer, and spin-coating the perovskite absorption layer with the passivating agent solution to prepare a passivation layer; 4, preparing a second carrier transport layer on the surface of the perovskite absorption layer; and step 5, preparing a top electrode on the surface of the second carrier transport layer to obtain the perovskite solar cell, it can be understood that the 4-vinylbenzylamine polymer is used as the passivating agent to passivate the defects of the perovskite thin film, on the basis of improving the quality of the perovskite thin film, the photovoltaic performance of the perovskite solar cell is further improved, and the solar cell is suitable for large-scale popularization and application. And the stability is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a 4-vinylbenzylamine polymer and its preparation and application in the preparation of solar cells. Background Art

[0002] As a new generation of photovoltaic power generation technology, organic-inorganic hybrid metal perovskite solar cells have the advantages of abundant raw materials and easy synthesis, very good photoelectric properties, short production process, low cost, good light absorption, charge transfer rate, etc., achieving high efficiency, high flexibility, and low cost. They have received extensive attention from academia and industry, and their photoelectric conversion efficiency has exceeded 25%, which is expected to break the traditional silicon battery market. As an important component of solar cells, the perovskite light-absorbing layer will not only affect the photoelectric conversion efficiency of the battery, but also affect the stability of the battery. For perovskite polycrystalline films, there are grain boundaries and surface defects. These defects, as non-radiative recombination centers, will reduce the carrier transfer efficiency and lifespan. In addition, moisture and oxygen can easily corrode the perovskite film crystal layer through the defects, leading to the degradation of the perovskite battery and reducing the photovoltaic performance and stability of the device. Therefore, how to passivate the surface defects of the crystal film is one of the cores of perovskite solar cell research.

[0003] At present, the main method for preparing perovskite thin films is the solution method. The solution method is to configure the organic and inorganic materials required for the perovskite layer into a precursor solution, and prepare the perovskite film on the substrate surface through processes such as spin coating and scraping. However, the existing thin film preparation technology will inevitably form certain defects on the perovskite surface. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problems existing in the background technology and to provide a 4-vinylbenzylamine polymer and its preparation and application in solar cell preparation.

[0005] Specifically, a 4-vinylbenzylamine polymer of the present invention comprises a general structure:

[0006] Wherein, R represents hydrogen, halogen, methyl or methoxy, X represents halogen (such as chlorine, bromine or iodine); n=10~100.

[0007] In another embodiment, polymers obtained from 4-vinylbenzylamine derivatives can also be used, including poly-4-vinylamphetamine halogen salts and poly-4-acetaldehydebenzylamine halogen salts. General formula (a) is poly-4-vinylamphetamine halogen salt, and general formula (b) is poly-4-acetaldehydebenzylamine halogen salt:

[0008] (a) (b) Wherein, R represents hydrogen, halogen, methyl or methoxy, X represents halogen (such as chlorine, bromine or iodine); n=10~100.

[0009] Furthermore, the present invention also provides a method for preparing a 4-vinylbenzylamine polymer, comprising the following steps: S1: dissolving 4-vinylbenzylamine in 1,4-dioxane, adding sodium hydroxide solution, and adding di-tert-butyl dicarbonate (Diboc) dropwise under ice bath conditions to obtain 4-vinylbenzylamine tert-butyl carbonate through reaction; S2: Add 4-vinylbenzylamine tert-butyl carbonate, potassium sulfate, dilute sulfuric acid and N,N-dimethylformamide into a reaction bottle filled with nitrogen, heat and stir, then add hydrogen peroxide solution to react to obtain poly 4-vinylbenzylamine tert-butyl carbonate; S3: dissolving poly (4-vinylbenzylamine tert-butyl carbonate) in toluene, adding halogen acid and anhydrous ethanol to react, filtering and vacuum drying to obtain the product poly (4-vinylbenzylamine halogen salt).

[0010] Furthermore, “S1” also includes the following steps: S11: After adding di-tert-butyl dicarbonate (Diboc) dropwise, react at 40°C for 12 hours; S12: After the reaction is completed, 4-vinylbenzylamine tert-butyl carbonate is obtained by separation through column chromatography.

[0011] Furthermore, in the "S1", the sodium hydroxide solution added is a 50% sodium hydroxide solution, the molar ratio of the 4-vinylbenzylamine to the di-tert-butyl dicarbonate is 1:2, the mass ratio of the 4-vinylbenzylamine to the sodium hydroxide solution is 1:2, and the mass ratio of the 4-vinylbenzylamine to the 1,4-dioxane is 1:15.

[0012] Further, in "S2", the mass of 4-vinylbenzylamine tert-butyl carbonate is 1.9 g (8.6 mmol), the mass of potassium sulfate is 0.2 g (1.2 mmol), the volume of dilute sulfuric acid is 2 ml, the volume of N,N-dimethylformamide is 8 ml, and the hydrogen peroxide solution is a hydrogen peroxide solution treated with nitrogen; Furthermore, after the hydrogen peroxide solution is added to the "S2" for reaction, the following steps are also included: a solution with a product is obtained by column chromatography separation, concentrated and then added to anhydrous methanol for precipitation, filtered and vacuum dried to obtain poly 4-vinylbenzylamine tert-butyl carbonate.

[0013] Furthermore, the mass ratio of the poly 4-vinylbenzylamine tert-butyl carbonate to the halogen acid in "S3" is 1:50.

[0014] Further, the structure of the 4-vinylbenzylamine tert-butyl carbonate is as follows: .

[0015] Further, the poly 4-vinylbenzylamine tert-butyl carbonate has the following structure: .

[0016] Further, the poly 4-vinylbenzylamine halogen salt structure is as follows: .

[0017] Furthermore, the present invention also provides a method for preparing a solar cell using a 4-vinylbenzylamine polymer, comprising the following steps: S1: pretreating the bottom electrode; S2: spin coating the perovskite precursor solution on the bottom electrode to prepare the perovskite absorption layer; S3: preparing a passivation agent solution through 4-vinylbenzylamine polymer, and spin coating the passivation agent solution on the perovskite absorption layer to prepare the passivation layer; S4: preparing a second carrier transport layer on the surface of the perovskite absorption layer; S5: preparing a top electrode on the surface of the second carrier transport layer to obtain a perovskite solar cell.

[0018] Compared with the prior art, the present invention has the following beneficial technical effects: When the 4-vinylbenzylamine polymer of the present invention passivates the perovskite light-absorbing layer, firstly -NH 3+ The group can be combined with Pb 2+ Strong bonding can effectively eliminate cationic defects. Secondly, its energy level is located between the carrier transport layer and the perovskite material, which can achieve the effect of energy level matching. The 4-vinylbenzylamine polymer will combine with the surface defects of the perovskite to reduce the risk of film decomposition. At the same time, since the degree of polymerization of the polymer molecules is controllable and the structure is orderly, the hydrophobic effect of the polymer chain structure can protect the perovskite from the erosion of water and oxygen in the air, which is beneficial to the performance stability and preservation of the perovskite battery. The perovskite solar cell passivated with the 4-vinylbenzylamine polymer of the present invention can be stored in a nitrogen environment for up to 1000 hours and can maintain a maximum of 95% of the initial efficiency, showing extremely high stability.

[0019] In summary, the present invention uses 4-vinylbenzylamine polymer as a passivator to passivate the defects of the perovskite film, thereby further improving the photovoltaic performance of the perovskite solar cell and improving its stability on the basis of improving the quality of the perovskite film. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a flow chart of the preparation method of 4-vinylbenzylamine polymer; Figure 2is a synthetic route diagram of 4-vinylbenzylamine polymer; Figure 3 Prepare a flow chart for a solar cell. DETAILED DESCRIPTION

[0021] It should be noted that, in the case of no conflict, the embodiments in the present invention and the features in the embodiments can be combined with each other. Hereinafter, the disclosure of the application will be further described according to specific embodiments. However, the specific embodiments listed are only for illustrative purposes, and are not intended to limit the disclosure. Those skilled in the art will recognize that the specific features in any of the following embodiments can be used for any other embodiment, as long as it does not deviate from the main purpose of the application.

[0022] Hereinafter, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which this application belongs. Terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.

[0023] The specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0024] Embodiment 1: The invention provides a 4-vinylbenzylamine polymer, which can be used as a passivator of a perovskite layer and for preparing a solar cell.

[0025] Its general formula is as follows:

[0026] Wherein R = H, halogen (F, Cl, Br), methyl, methoxy and other functional groups; X represents halogen (such as chlorine, bromine or iodine); n = 10~100.

[0027] In another embodiment, polymers obtained from 4-vinylbenzylamine derivatives can also be used, including poly-4-vinylamphetamine halogen salts and poly-4-acetaldehydebenzylamine halogen salts. General formula (a) is poly-4-vinylamphetamine halogen salt, and general formula (b) is poly-4-acetaldehydebenzylamine halogen salt:

[0028] (b) The 4-vinylbenzylamine polymer of the present invention can passivate the cation and anion defects on the surface of the perovskite crystal, and further enhance the binding ability through hydrogen bonds or ionic bonds, effectively passivating the surface defects of the perovskite. Specifically, the -NH3+ The group treats the surface of the perovskite film and uses the ordered and dense structure of the polymer to protect the perovskite film. On the basis of improving the quality of the perovskite film, the photovoltaic performance of the perovskite solar cell is further improved and its environmental stability is enhanced.

[0029] Furthermore, this embodiment provides a method for preparing a 4-vinylbenzylamine polymer, comprising the following steps: S1: dissolving 4-vinylbenzylamine in 1,4-dioxane, adding sodium hydroxide solution, and adding di-tert-butyl dicarbonate (Diboc) dropwise under ice bath conditions to obtain 4-vinylbenzylamine tert-butyl carbonate through reaction; S2: Add 4-vinylbenzylamine tert-butyl carbonate, potassium sulfate, dilute sulfuric acid and N,N-dimethylformamide into a reaction bottle filled with nitrogen, heat and stir, then add hydrogen peroxide solution to react to obtain poly 4-vinylbenzylamine tert-butyl carbonate; S3: dissolving poly (4-vinylbenzylamine tert-butyl carbonate) in toluene, adding halogen acid and anhydrous ethanol to react, filtering and vacuum drying to obtain the product poly (4-vinylbenzylamine halogen salt).

[0030] Specifically, in step S1, the added hydrogen peroxide solution is a 50% sodium hydroxide solution, di-tert-butyl dicarbonate (Diboc) is added dropwise under ice bath conditions, and the mixture is reacted at 40° C. for 12 hours. After the reaction is completed, 4-vinylbenzylamine tert-butyl carbonate is obtained by column chromatography separation with a yield of 92.5%; wherein the molar ratio of 4-vinylbenzylamine to di-tert-butyl dicarbonate is 1:2, the mass ratio of 4-vinylbenzylamine to 50% sodium hydroxide solution is 1:2, the mass ratio of the reactant to 1,4-dioxane is 1:15, and the structure of 4-vinylbenzylamine tert-butyl carbonate is as follows: .

[0031] Specifically, in step S2, the specific content of the reactants added to the reaction bottle filled with nitrogen is: 1.9g (8.6mmol) 4-vinylbenzylamine tert-butyl carbonate, 0.2g (1.2mmol) potassium sulfate, 2ml dilute sulfuric acid and 8ml N, N-dimethylformamide were heated and stirred at 60°C, and then a nitrogen-treated hydrogen peroxide solution was added after stirring, and the reaction was continued for 24 hours. The solution with the product was separated by column chromatography, concentrated, added to anhydrous methanol for precipitation, filtered and vacuum dried to obtain poly-4-vinylbenzylamine tert-butyl carbonate, with a reaction yield of 75.2%. The structure of poly-4-vinylbenzylamine tert-butyl carbonate is as follows: .

[0032] Specifically, in step S3, after poly 4-vinylbenzylamine tert-butyl carbonate is dissolved in toluene, halogen acid (57wt.%) is added and stirred for 12 hours, anhydrous ethanol is added and stirred for 12 hours, filtered and vacuum dried to obtain the product poly 4-vinylbenzylamine halogen salt, wherein the mass ratio of poly 4-vinylbenzylamine tert-butyl carbonate to halogen acid is 1:50, and the structure of poly 4-vinylbenzylamine halogen salt is as follows: .

[0033] Furthermore, the poly-4-vinyl amphetamine halogen salt can be synthesized using the above method; the poly-4-acetaldehyde benzylamine halogen salt needs to first react the acetaldehyde group with alcohol to generate acetal, and then can be synthesized using the above method.

[0034] Furthermore, this embodiment also provides a method for preparing a solar cell using a 4-vinylbenzylamine polymer, comprising the following steps: Step 1: Clean the bottom electrode by ultrasonically cleaning the substrate with deionized water, acetone, and ethanol in sequence and drying it with nitrogen; Step 2: UV-ozone treatment of the bottom electrode surface; Step 3: dissolving Cs0.05(MA0.15FA0.85)0.95Pb(I0.85Br0.15)3 in a mixture of dimethylformamide and dimethyl sulfoxide in a volume ratio of 9:1, stirring for 6 hours, and preparing a perovskite precursor solution with a concentration of 0.6 mol / L; spin coating the obtained perovskite precursor solution on the bottom electrode at a spin coating speed of 1500 rpm and a spin coating time of 30 seconds; annealing after spin coating; annealing temperature of 100°C and annealing time of 30 minutes to obtain a perovskite absorption layer; Step 4: dissolving poly 4-vinylbenzylamine halogen salt in chlorobenzene to prepare a passivation agent solution with a concentration of 0.5 mg / mL, and spin-coating the passivation agent solution on the perovskite absorption layer at a rotation speed of 3000 rpm for 30 seconds; then placing it in a low vacuum environment and standing for 60 minutes to complete the preparation of the passivation layer; Step 5: Prepare a second carrier transport layer on the perovskite surface; Step 6: Prepare a top electrode on the surface of the second carrier transport layer to obtain a perovskite solar cell.

[0035] It is understood that when the 4-vinylbenzylamine polymer of the present invention passivates the perovskite light-absorbing layer, first -NH 3+ The group can be combined with Pb 2+Strong bonding can effectively eliminate cationic defects. Secondly, its energy level is located between the carrier transport layer and the perovskite material, which can achieve the effect of energy level matching. The 4-vinylbenzylamine polymer will combine with the surface defects of the perovskite to reduce the risk of film decomposition. At the same time, since the degree of polymerization of the polymer molecules is controllable and the structure is orderly, the hydrophobic effect of the polymer chain structure can protect the perovskite from the erosion of water and oxygen in the air, which is beneficial to the performance stability and preservation of the perovskite battery. The perovskite solar cell passivated with the 4-vinylbenzylamine polymer of the present invention can be stored in a nitrogen environment for up to 1000 hours and can maintain a maximum of 95% of the initial efficiency, showing extremely high stability.

[0036] In order to verify the beneficial effects of the present invention, the present invention also provides the following: Example 2: In this example, the R group in the general formula of Example 1 is designated as F, and the other steps are the same as those of Example 1 to obtain a perovskite solar cell.

[0037] Example 3: In this example, the R group in the general formula of Example 1 is designated as Br, and the other steps are the same as those of Example 1 to obtain a perovskite solar cell.

[0038] Example 4: In this example, the R group in the general formula of Example 1 is designated as a methyl group, and the other steps are the same as those of Example 1 to obtain a perovskite solar cell.

[0039] Example 5: In this example, the R group in the general formula of Example 1 is designated as a methoxy group, and the other steps are the same as those of Example 1 to obtain a perovskite solar cell.

[0040] Example 6: In this example, the amount of addition in step S2 of the method for preparing 4-vinylbenzylamine polymer in Example 1 is changed to adding 0.05g potassium sulfate and 0.5ml dilute sulfuric acid, so that the degree of polymerization of poly 4-vinylbenzylamine tert-butyl carbonate is 23, and the other steps are the same as in Example 1 to obtain a perovskite solar cell.

[0041] Example 7: In this example, the amount of addition in step S2 of the method for preparing 4-vinylbenzylamine polymer in Example 1 is changed to adding 0.5g potassium sulfate and 5ml dilute sulfuric acid, so that the degree of polymerization of poly 4-vinylbenzylamine tert-butyl carbonate is 87, and the other steps are the same as in Example 1 to obtain a perovskite solar cell.

[0042] Comparative Example 1: In this comparative example, 4-vinylbenzylamine iodate is used as a passivating agent, and the steps for preparing a perovskite solar cell are the same as those in Example 1 to obtain a perovskite solar cell.

[0043] The perovskite solar cells prepared in the above Examples 1 to 7 and Comparative Example 1 were characterized respectively, and the results are shown in Table 1.

[0044]

[0045] Table 1 From the efficiency of the perovskite solar cell devices prepared by Comparative Example 1 and Examples 1 to 7 in Table 1, it can be seen that the device efficiencies obtained by the preparation methods of Examples 1 to 7 are higher than those of the comparative examples, which indicates that the perovskite solar cell modified by 4-vinylbenzylamine polymer has higher photoelectric performance. From the humidity stability of the perovskite solar cell devices in Table 1, it can be seen that within the 1000-hour test time, the efficiency of the comparative device dropped to 85%, and the efficiency of the devices prepared by Examples 1 to 7 dropped to about 90% to 95% of the initial value. This is because 4-vinylbenzylamine polymer modification can passivate the surface defects of the perovskite film, thereby reducing the defect density, and 4-vinylbenzylamine polymer modification can reduce phase change or chemical degradation, thereby extending the long-term stability of the device.

[0046] In summary, the present invention uses 4-vinylbenzylamine polymer as a passivator to passivate the defects of the perovskite film, thereby further improving the photovoltaic performance of the perovskite solar cell and improving its stability on the basis of improving the quality of the perovskite film.

[0047] The above is one or more implementation methods provided in combination with specific contents, and it is not intended that the specific implementation of the present invention is limited to these descriptions. Any similarity or similarity with the method, structure, etc. of the present invention, or any technical deduction or replacement made on the premise of the concept of the present invention, shall be regarded as the protection scope of the present invention.

Claims

1. A 4-vinylbenzylamine polymer, characterized in that Including the general structure: ; Wherein R represents hydrogen, halogen, methyl or methoxy; X represents halogen; n=10~100.

2. A method for preparing a 4-vinylbenzylamine polymer, characterized in that: The steps include: S1: dissolving 4-vinylbenzylamine in 1,4-dioxane, adding sodium hydroxide solution, and adding di-tert-butyl dicarbonate dropwise under ice bath conditions to obtain 4-vinylbenzylamine tert-butyl carbonate through reaction; S2: Add 4-vinylbenzylamine tert-butyl carbonate, potassium sulfate, dilute sulfuric acid and N,N-dimethylformamide into a reaction bottle filled with nitrogen, heat and stir, then add hydrogen peroxide solution to react to obtain poly 4-vinylbenzylamine tert-butyl carbonate; S3: dissolving poly (4-vinylbenzylamine tert-butyl carbonate) in toluene, adding halogen acid and anhydrous ethanol to react, filtering and vacuum drying to obtain the product poly (4-vinylbenzylamine halogen salt).

3. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: The "S1" also includes the following steps: S11: After adding di-tert-butyl dicarbonate dropwise, react at 40° C. for 12 hours; S12: After the reaction is completed, 4-vinylbenzylamine tert-butyl carbonate is obtained by separation through column chromatography.

4. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: In the "S2", the sodium hydroxide solution added is a 50% sodium hydroxide solution, the molar ratio of the 4-vinylbenzylamine to the di-tert-butyl dicarbonate is 1:2, the mass ratio of the 4-vinylbenzylamine to the sodium hydroxide solution is 1:2, and the mass ratio of the 4-vinylbenzylamine to the 1,4-dioxane is 1:

15.

5. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: In the "S2", the mass of the 4-vinylbenzylamine tert-butyl carbonate is 1.9 g (8.6 mmol), the mass of the potassium sulfate is 0.2 g (1.2 mmol), the volume of the dilute sulfuric acid is 2 ml, the volume of the N,N-dimethylformamide is 8 ml, and the hydrogen peroxide solution is a hydrogen peroxide solution treated with nitrogen; After the hydrogen peroxide solution is added to the "S2" for reaction, the following steps are also included: a solution with a product is obtained by column chromatography separation, concentrated and then added to anhydrous methanol for precipitation, filtered and vacuum dried to obtain poly 4-vinylbenzylamine tert-butyl carbonate.

6. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: The mass ratio of the poly 4-vinylbenzylamine tert-butyl carbonate to the halogen acid in "S3" is 1:

50.

7. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: The structure of the 4-vinylbenzylamine tert-butyl carbonate is as follows: 。 8. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: The structure of the poly-4-vinylbenzylamine tert-butyl carbonate is as follows: 。 9. The method for preparing a 4-vinylbenzylamine polymer according to claim 2, characterized in that: The poly 4-vinylbenzylamine halogen salt structure is as follows: 。 10. A method for preparing a solar cell using a 4-vinylbenzylamine polymer, characterized in that: The steps include: Step 1: pre-treating the bottom electrode; Step 2: Spin-coating the perovskite precursor solution on the bottom electrode to prepare the perovskite absorption layer; Step 3: preparing a passivation agent solution by using a 4-vinylbenzylamine polymer, and spin-coating the passivation agent solution on the perovskite absorption layer to prepare the passivation layer; Step 4: preparing a second carrier transport layer on the surface of the perovskite absorption layer; Step 5: Prepare a top electrode on the surface of the second carrier transport layer to obtain a perovskite solar cell.