Tellurite sulfate nonlinear optical crystal as well as preparation method and application thereof
Through the development of tellurite sulfate nonlinear optical crystal Ti(TeO3)(SO4), the problems of narrow band gap and small birefringence of existing nonlinear optical materials have been solved, and a wide optical band gap and large laser damage threshold have been achieved, which is suitable for Efficient nonlinear optical materials, especially for applications in the field of optics.
Patent Information
- Application Number
- CN202410864366.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-10-25
AI Technical Summary
Existing nonlinear optical crystal materials such as ZnGeP2 and AgGaS2 have narrow band gaps and low laser damage thresholds, which limit their applications. Moreover, the birefringence of sulfate crystals is small and phase matching cannot be achieved, hindering their wide application in the field of nonlinear optics. .
A tellurite sulfate nonlinear optical crystal Ti(TeO3)(SO4) was developed, which has a wide optical band gap and a large laser damage threshold. It was prepared by a hydrothermal method using a specific Ti, Te, S source ratio and reaction temperature. Under the conditions, a monoclinic crystal is formed, achieving strong frequency doubling effect and phase matching.
It achieves strong frequency doubling effect, wide light transmission range, ultraviolet absorption cut-off wavelength of about 312nm, large laser damage threshold, and is prepared by hydrothermal method. It is simple to operate, has high raw material utilization rate, high product purity, can achieve phase matching, and is suitable for use. for second-order nonlinear optical materials.
Smart Images

Figure CN118835320A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic chemical materials, and in particular to a tellurite sulfate nonlinear optical crystal and a preparation method and application thereof. Background Art
[0002] In recent years, people have devoted themselves to exploring various functional materials with non-centrosymmetric structures that have piezoelectric, pyroelectric, ferroelectric and nonlinear optical properties. Nonlinear optical crystals can use the second harmonic generation process to extend the wavelength of lasers to new spectral regions and are widely used in precision micro-manufacturing, laser spectroscopy, optical communications and other fields. So far, people have discovered many excellent nonlinear optical crystals that are used as core components of optical devices, such as KH 2 PO 4 , LiB 3 O 5 ,KBe 2 BO 3 F 2 β-BaB 2 O 4 、ZnGeP 2 、AgGaS 2 However, these crystals have certain disadvantages, such as ZnGeP 2 、AgGaS 2 The narrow band gap and low laser damage threshold caused by two-photon absorption limit their practical applications. In order to meet the needs of modern science and technology, it is urgent to explore new nonlinear crystal materials with non-centrosymmetric structures and more ideal comprehensive properties.
[0003] Sulfate has [SO 4 ] Tetrahedral units, wide optical band gap, short UV cutoff absorption edge, easy crystal growth and other advantages have attracted more and more attention in the research of optoelectronic functional materials. However, the birefringence of crystals containing only highly symmetrical groups will be very small, such as LiNH 4 SO 4 (0.0078@532nm) and LiKSO 4 (0.00025@546nm), which makes many sulfates unable to achieve phase matching, hindering the application of sulfate crystals. Therefore, exploring new nonlinear sulfate crystals with suitable birefringence has broad application prospects in the field of nonlinear optics. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a tellurium sulfate nonlinear optical crystal and its preparation method and application. The tellurium sulfate nonlinear optical crystal has a very wide optical band gap and a potential large laser damage threshold, and can be used as a nonlinear optical material in the optical field.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A tellurite sulfate nonlinear optical crystal with a chemical formula of Ti(TeO 3 )(SO 4 ), belongs to the monoclinic system, and its crystal space group is P2 1 ;
[0007] Among them, Ti(TeO 3 )(SO 4 ) has a unit cell parameter of α=90°, β=105.062(6)°, γ=90°;
[0008] The present invention also provides a method for preparing a tellurite sulfate nonlinear optical crystal, comprising the following steps:
[0009] The Ti source, Te source, S source and water are uniformly mixed and reacted to crystallize to obtain a tellurite sulfate nonlinear optical crystal.
[0010] As a preferred embodiment of the present invention, the molar ratio of the Ti source, the Te source and the S source in the initial mixed raw material is 1:(0.5-2):(16-32).
[0011] As a preferred embodiment of the present invention, the reaction temperature is 180-300°C.
[0012] As a preferred embodiment of the present invention, the reaction time is ≥24h.
[0013] As a preferred embodiment of the present invention, the Ti source is TiO 2 or Ti(SO 4 ) 2 or TiO(SO 4 ).
[0014] As a preferred embodiment of the present invention, the Te source is TeO 2 .
[0015] As a preferred embodiment of the present invention, the S source is a sulfuric acid solution.
[0016] The invention also provides an application of a tellurite sulfate nonlinear optical crystal as a nonlinear optical material in the field of optics.
[0017] The beneficial effects of the present invention are as follows: (1) the tellurite sulfate nonlinear optical crystal of the present invention has a strong double-frequency effect (SHG). The Kurtz powder double-frequency test results show that Ti(TeO 3 )(SO 4 ) is 11.6 times that of the standard sample KDP (potassium dihydrogen phosphate); (2) the tellurium sulfate nonlinear optical crystal of the present invention has a wide light transmittance range, and the ultraviolet absorption cut-off wavelength is about 312nm, which has a potential large laser damage threshold; (3) the tellurium sulfate nonlinear optical crystal of the present invention is prepared by a hydrothermal method, which is simple to operate, has a high raw material utilization rate, mild experimental conditions, and high product purity; (4) the tellurium sulfate nonlinear optical crystal of the present invention can achieve phase matching as a second-order nonlinear optical crystal material. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Ti(TeO 3 )(SO 4 ) Crystal structure diagram of the crystal;
[0019] Figure 2 Ti(TeO 3 )(SO 4 ) UV-visible diffuse reflectance spectrum of the crystal;
[0020] Figure 3 Ti(TeO 3 )(SO 4 ) The relationship between the intensity of the frequency-doubled effect and the particle size of the sample;
[0021] Figure 4 Ti(TeO 3 )(SO 4 ) Actual picture of the crystal. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0023] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0024] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0025] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.
[0026] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.
[0027] Example 1
[0028] A method for preparing a tellurite sulfate nonlinear optical crystal comprises the following steps:
[0029] 1.0 mmol TiO 2 (0.080 g) and 0.5 mmol TeO 2 (0.08 g) was dissolved in deionized water, 1.0 mL of concentrated sulfuric acid (16 mol / L) was added, and the mixture was placed in a high-pressure reactor lined with polytetrafluoroethylene. The reaction system was heated to 180 °C / h under hydrothermal conditions and kept at this temperature for 48 h. The reaction system was slowly cooled to room temperature, washed, and dried to obtain Ti(TeO 3 )(SO 4 ) Tellurite sulfate nonlinear optical crystals.
[0030] Example 2
[0031] A method for preparing a tellurite sulfate nonlinear optical crystal comprises the following steps:
[0032] 1.0 mmol TiO 2 (0.080 g) and 0.5 mmol TeO 2 (0.08 g) was dissolved in deionized water, 1.0 mL of concentrated sulfuric acid was added, and the mixture was placed in a high-pressure reactor lined with polytetrafluoroethylene. The reaction system was heated to 300 °C / h under hydrothermal conditions and kept at this temperature for 64 h. The reaction system was slowly cooled to room temperature, washed, and dried to obtain Ti(TeO 3 )(SO 4 ) Tellurite sulfate nonlinear optical crystals.
[0033] Example 3
[0034] A method for preparing a tellurite sulfate nonlinear optical crystal comprises the following steps:
[0035] 1.0 mmol TiO 2 (0.080 g) and 2.0 mmol TeO 2 (0.32 g) was dissolved in deionized water, 2 mL of concentrated sulfuric acid was added, and the mixture was placed in a high-pressure reactor lined with polytetrafluoroethylene. The reaction system was heated to 230 °C / h under hydrothermal conditions and kept at this temperature for 96 h. The reaction system was slowly cooled to room temperature, washed, and dried to obtain Ti(TeO 3 )(SO 4 ) Tellurite sulfate nonlinear optical crystals.
[0036] Example 4
[0037] A method for preparing a tellurite sulfate nonlinear optical crystal comprises the following steps:
[0038] 2.0 mmol TiO(SO 4 ) (0.16 g) and 2.0 mmol TeO 2 (0.32 g) was dissolved in deionized water, 2 mL of concentrated sulfuric acid was added, and the mixture was placed in a high-pressure reactor lined with polytetrafluoroethylene. The reaction system was heated to 300 °C / h under hydrothermal conditions and kept at this temperature for 128 h. The reaction system was slowly cooled to room temperature, washed, and dried to obtain Ti(TeO 3 )(SO 4 ) Tellurite sulfate nonlinear optical crystals.
[0039] Example 5
[0040] A method for preparing a tellurite sulfate nonlinear optical crystal comprises the following steps:
[0041] 3.0 mmol Ti(SO 4 ) 2 (0.24 g) and 0.5 mmol TeO 2 (0.08 g) was dissolved in deionized water, 1 mL of concentrated sulfuric acid was added, and the mixture was placed in a high-pressure reactor lined with polytetrafluoroethylene. The reaction system was heated to 180 °C / h under hydrothermal conditions and kept at this temperature for 48 h. The reaction system was slowly cooled to room temperature, washed, and dried to obtain Ti(TeO 3 )(SO 4 ) Tellurite sulfate nonlinear optical crystals.
[0042] Test Case
[0043] 1. Frequency doubling performance test: The frequency doubling effect and phase matching test of the nonlinear optical crystal prepared by the present invention are obtained by the Kurtz powder frequency doubling test method. The specific operation steps are as follows: the tellurite sulfate nonlinear optical crystal of Example 1 is first ground and sieved into powders of different particle size ranges (20-40, 40-80, 80-100, 100-125, 125-150, 150-200, 200-300 microns), and then loaded into a sample cell with glass windows on both sides, and then the sample cell is placed in Nb 3+ In the laser optical path with YAG pulse laser as the light source, the sample cell is irradiated with fundamental frequency light with a wavelength of 1064 nanometers, and the frequency-doubled signal is displayed on the oscilloscope through the photomultiplier tube.
[0044] The intensity of the frequency doubling effect is plotted against the particle size. If the intensity increases first and then tends to a plateau as the particle size increases, it indicates phase matching; if the intensity increases first and then decreases as the particle size increases, it indicates phase mismatch. The KDP single crystal powder of the same particle size is used as a standard sample, and the sample with the particle size after the frequency doubling effect reaches the plateau is taken and the frequency doubling signal intensity measured by KDP is compared to obtain the relative size of the frequency doubling effect (see the test results in point 3 below).
[0045] 2. Crystal structure test: The tellurium sulfate nonlinear optical crystal structure prepared in Example 1 was determined by single crystal X-ray diffraction structure analysis. It belongs to the monoclinic system P2 1 Space group.
[0046] Ti(TeO 3 )(SO 4 )’s unit cell parameters are: α=90°, β=105.062(6)°, γ=90°.
[0047] Ti(TeO 3 )(SO 4 ), each asymmetric unit contains one Te atom, one S atom, one Ti atom and seven O atoms. All these atoms are in normal positions, and the two-fold rotation axis is parallel to the b axis. Figure 1 As shown, each Te atom forms [TeO 3 ] group; each S atom forms [SO 4 ] group; each Ti atom is coordinated with six O atoms to form a typical [TiO 6 ] octahedron. The three short Ti-O bonds are connected to the three [SO 4 ] groups share oxygen atoms, while the three long Ti-O bonds are connected to three [TeO 3 ] groups share oxygen atoms and together constitute its three-dimensional spatial structure.
[0048] 3. Performance test results: Ti(TeO 3 )(SO 4 ) Crystal (Example 1) UV-visible diffuse reflectance spectrum is as follows Figure 2 As shown in Figure 2, the UV absorption cutoff wavelength is about 312 nm; the relationship between the SHG intensity and the sample particle size is shown in Figure 2. Figure 3 As shown in Figure 2, this tellurite sulfate has a high-intensity second-order nonlinear optical effect and can achieve phase matching. The frequency doubling effect is about 11.6 times that of KDP. The crystals obtained by the hydrothermal method are shown in Figure 2. Figure 4 As shown, the quality is good, indicating that their crystal growth habits are very good.
[0049] In summary, the tellurite sulfate nonlinear optical crystal prepared in the present invention has excellent comprehensive properties and can be used as a second-order nonlinear optical crystal material.
[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A tellurite sulfate nonlinear optical crystal, characterized in that: The chemical formula is Ti(TeO3)(SO4), it belongs to the monoclinic system, and its crystal space group is P21; The unit cell parameters of Ti(TeO3)(SO4) are α=90°, β=105.062(6)°, γ=90°.
2. The method for preparing the tellurite sulfate nonlinear optical crystal according to claim 1, characterized in that: The following steps are involved: The Ti source, Te source, S source and water are uniformly mixed and reacted to crystallize to obtain a tellurite sulfate nonlinear optical crystal.
3. The method for preparing a tellurite sulfate nonlinear optical crystal according to claim 2, characterized in that: The molar ratio of the Ti source, the Te source and the S source in the initial mixed raw material is 1:(0.5-2):(16-32).
4. The method for preparing a tellurite sulfate nonlinear optical crystal according to claim 2, characterized in that: The reaction temperature is 180-300°C.
5. The method for preparing a tellurite sulfate nonlinear optical crystal according to claim 2, characterized in that: The reaction time is ≥24h.
6. The preparation method according to claim 2, characterized in that: The Ti source is TiO2 or Ti(SO4)2 or TiO(SO4).
7. The preparation method according to claim 1, characterized in that: The Te source is TeO2.
8. The preparation method according to claim 1, characterized in that: The S source is concentrated sulfuric acid.
9. Application of the tellurite sulfate nonlinear optical crystal according to claim 1 as a nonlinear optical material in the field of optics.