Testing device for simulating local corrosion of reinforcing steel bar in concrete and testing method thereof

By using stainless steel wires and copper bars as auxiliary electrodes in concrete structures, combined with a dry-wet cycle simulation system, efficient and low-cost local corrosion simulation of steel bars in concrete is achieved, solving the low efficiency and reliability of corrosion tests in the existing technology. This reduces the problem and improves the reliability and real-time monitoring capabilities of the corrosion test.

CN118837286APending Publication Date: 2024-10-25BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411061820.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing concrete structure simulation tests cannot effectively simulate local corrosion of steel bars in concrete, and the corrosion test efficiency is low and the cost is high. It is impossible to accurately control the degree of corrosion and monitor damage in real time, resulting in low credibility of simulation test results.

Method used

Design a test device to simulate local corrosion of steel bars in concrete. Stainless steel wires and copper bars are used as preset auxiliary electrodes. Combined with a dry-wet cycle simulation system, local corrosion is achieved through a DC regulated power supply. The corrosion process is monitored in real time, and the current and time to control the degree of rust.

Benefits of technology

It achieves efficient and low-cost simulation of local corrosion of steel bars in concrete structures, improves the reliability and real-time monitoring capabilities of corrosion tests, significantly improves the accuracy of Faraday's law, and is suitable for different types of pressure components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118837286A_ABST
    Figure CN118837286A_ABST
Patent Text Reader

Abstract

The invention discloses a test device for simulating local corrosion of reinforcing steel bars in concrete and a test method thereof.The test device comprises a to-be-corroded test piece, a preset auxiliary electrode, an anchoring system of the preset auxiliary electrode, a dry-wet cycle simulation system and a direct-current voltage-stabilized power source, and the test method comprises the steps that longitudinal bars and stirrups of a local corrosion section are connected to the positive electrode of a power source through pre-buried wires; stainless steel wires (corresponding to longitudinal bars) and copper bars (corresponding to stirrups) are connected to the negative electrode of a power source, alternate circulation conditions are provided through a dry-wet circulation simulation system, the to-be-rusted test piece, the preset auxiliary electrode and the moisturizing sponge form an electrolysis loop, a local non-uniform corrosion test is conducted, a corrosion pool does not need to be built, and the corrosion resistance of the to-be-rusted test piece is improved through the combination of the preset auxiliary electrode method and the veneering method. The non-uniform corrosion of longitudinal bars or stirrups of test pieces with different sizes in any time and any local corrosion section can be realized, the corrosion characteristics of an actual structure are better met, meanwhile, the real-time monitoring capability of the whole corrosion process is improved, and the cost and the resource consumption are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete structure simulation test, in particular to a test device and a test method for simulating local corrosion of steel bars in concrete. Background Art

[0002] Concrete structures have serious durability problems due to the complex service environment and the characteristics of concrete materials themselves, and their deterioration degree continues to deepen with the change of performance over time and the increase of usage demand. Among various durability diseases, structural performance degradation caused by steel corrosion is the most common, especially in marine environments.

[0003] Existing studies have mostly focused on the uniform corrosion of the entire structure, but concrete structures in marine environments show different characteristics of corrosion on the facade due to different chloride ion concentrations, oxygen content and relative humidity at different heights. For example, according to the characteristics of the corrosion environment at different heights, the bridge piers can be divided from the top to the bottom of the pier into the atmospheric zone, the splash and tidal zone, and the underwater zone. The damage caused by the local non-uniform corrosion in the splash and tidal zone is the most serious, and the failure mechanism also changes accordingly.

[0004] The simulation test methods for steel bar corrosion in concrete mainly include internal mixing method, immersion method, power-on method and dry-wet cycle method. Among them, the power-on method is popular because of its faster corrosion rate, including full immersion method, semi-immersion method, veneer method and auxiliary electrode method, but the corroded steel bars are mostly uniformly corroded, which is different from the phenomenon of local or non-uniform corrosion of steel bars commonly seen in actual projects.

[0005] For the immersion method, the specimen is generally immersed in the corrosion pool horizontally, which may be inconsistent with its actual stress state, especially for compressive components with high stirrup ratio or high axial compression ratio (self-weight, upper beam weight). Due to the infiltration of NaCl solution and the accumulation and penetration of corrosion products, it is difficult for experimenters to monitor the internal steel corrosion and rust expansion crack expansion in real time, making the auxiliary control method based on rust expansion crack information to predict the corrosion rate invalid, and ultimately leading to the inherent defects of Faraday's law cannot be compensated. It can be seen that since the immersion method cannot be combined with specific component types to induce non-uniform corrosion of steel bars, and the degree of corrosion cannot be accurately controlled, it will cause a large difference in the similarity between the simulated test environment and the real corrosion environment, resulting in the research results of the simulation test may have low credibility.

[0006] For corrosion tests on concrete structures, even if a larger corrosion pool is built, the number of specimens in each batch of tests is still very limited, especially for the full immersion method in the laboratory. The high requirements for cost and site conditions and the low efficiency of corrosion tests form a huge contrast.

[0007] In summary, there are four main deficiencies in the corrosion test equipment and methods for concrete components or structures: First, the entire specimen is immersed in a NaCl solution for electrical acceleration of corrosion, which cannot achieve the local corrosion characteristics of the steel facade under natural conditions; second, the uniform corrosion of the steel cross section is inconsistent with the fact that a half-moon-shaped corrosion first appears on the side facing the protective layer and causes concrete cracking on the protective layer side, and it is impossible to monitor concrete damage and internal steel corrosion in real time; third, there is a lack of simulation tests considering non-uniform corrosion of longitudinal reinforcement or stirrups and theories on the coupling effect of the two; fourth, the method of horizontally immersing specimens for corrosion is not suitable for different types of specimens, especially for compressive members with high stirrup ratios or high axial compression ratios.

[0008] In order to improve the ability to predict and evaluate the performance of concrete structures in real service environments, it is imperative to establish an electrochemical accelerated corrosion method with high corrosion efficiency, low cost, and the ability to effectively simulate local corrosion of steel bars in concrete, and to develop corresponding test equipment. It is worth noting that the relevant work can also appropriately eliminate the errors in the corrosion rate prediction of Faraday's law, and significantly improve the level of concrete corrosion damage and steel bar corrosion field monitoring technology. Summary of the invention

[0009] The purpose of the present invention is to provide a test device and a test method for simulating local corrosion of steel bars in concrete, overcome the limitations of existing simulated corrosion test technology, establish an electrochemical accelerated corrosion test method and a test device with high corrosion efficiency and controllable cost, which can effectively simulate local corrosion of steel bars in concrete structures, so as to achieve simulation and real-time monitoring of the entire process of steel bar corrosion to the greatest extent, and lay a solid foundation for the durability research of concrete structures in actual engineering.

[0010] To achieve the above object, the present invention provides the following solutions: A test device for simulating local corrosion of steel bars in concrete comprises a test piece to be corroded, a preset auxiliary electrode, an anchoring system for fixing the preset auxiliary electrode, a dry-wet cycle simulation system and a DC regulated power supply, wherein the test piece to be corroded comprises a concrete matrix, longitudinal bars and stirrups arranged in the concrete matrix, the preset auxiliary electrode comprises a stainless steel wire arranged in the concrete matrix, outside the longitudinal bars and along the direction of the longitudinal bars, and a copper bar sequentially sleeved on the outer surface of the concrete matrix at intervals, both ends of the stainless steel wire extend out of the concrete matrix, the copper bar of the stainless steel wire corresponds to the position of the stirrup, one end of the stainless steel wire is connected to the negative electrode of the DC regulated power supply through a wire, the longitudinal bars are connected to the positive electrode of the DC regulated power supply, the copper bar is connected to the negative electrode of the DC regulated power supply, and the stirrup is connected to the positive electrode of the DC regulated power supply, and the dry-wet cycle system is used to perform dry treatment and wet treatment on the test piece to be corroded.

[0011] Preferably, the anchoring system comprises an anchor arranged at the position where the stainless steel wire extends out of the concrete matrix, a high-strength gauze wrapped at both ends of the stainless steel wire and coated with epoxy resin, and the steel wire passes through the anchor.

[0012] Preferably, the wet-dry cycle simulation system includes a moisturizing sponge wrapped around the outside of the concrete matrix, a humidity sensor arranged on the moisturizing sponge, a spray head for spraying the moisturizing sponge, a liquid storage tank connected to the spray head, and a waterproof plastic film wrapped around the outside of the moisturizing sponge after spraying.

[0013] Preferably, it also includes a corrosion test shed, the four sides and the top of which are respectively provided with simple enclosures and covers.

[0014] A test method for simulating local corrosion of steel bars in concrete, comprising the following steps: (1) tying a steel bar skeleton of a concrete specimen, wherein the steel bar skeleton of the specimen to be corroded comprises four longitudinal bars and a plurality of stirrups arranged at intervals in a direction perpendicular to the longitudinal bars; (2) Pass the stainless steel wire used to induce corrosion of the longitudinal reinforcement through the mold, adjust the tension and length of the stainless steel wire, and anchor the stainless steel wire in the local corrosion section. Then, install the steel skeleton to be corroded in the mold, and lead out the two ends of the stainless steel wire; (3) Pour concrete in the mold, remove the mold after one day, and mark the detailed position information of the stirrups on the surface of the concrete specimen, and then cure the specimen to be corroded to the planned age; loosen the stainless steel wire before removing the mold; (4) After the planned age is reached, copper bars with the same shape as the stirrups are arranged and fixed along the surface of the local corroded section according to the marked stirrup positions; the spacing between adjacent copper bars is exactly the same as the spacing between the corresponding stirrups; the distance between the stirrups and the copper bars is the thickness of the concrete cover; (5) First, place and fix the specimen to be corroded vertically, then use a wire to connect one end of the stainless steel wire to the negative pole of the DC stabilized power supply, connect the longitudinal reinforcement to be corroded to the positive pole of the DC stabilized power supply, turn on the DC stabilized power supply, set the current, record the current and time for corrosion; for stirrup corrosion, connect one end of the copper busbar to the negative pole of the DC stabilized power supply, and other operations are the same as for longitudinal reinforcement corrosion; (6) Use a spray shower to spray the NaCl solution in the storage tank onto the moisturizing sponge in the locally corroded area, so that the value range of the humidity sensor is stabilized at 40-50%, and then cover it with a waterproof plastic film; after the expected power-on time is reached, turn off the power and stop the dry-wet cycle.

[0015] Preferably, the current formula in step (5) is as follows:

[0016] In the formula, I corr is the corrosion current (mA); i corr is the corrosion current density (mA / mm 2 ); d is the diameter of the steel bar (mm); l is the length of the rusted section (mm).

[0017] Preferably, the power-on time formula in step (5) is as follows:

[0018] In the formula, t is the rusting time after power on (s); Z Fe is the ionic charge, Z Fe = 2; F is the Faraday constant (96485 C / mol); Δm t is the mass loss of steel bar due to corrosion (g); M Fe is the molecular weight of iron (56 g / mol).

[0019] Compared with the prior art, the present invention has achieved the following technical effects: 1. The present invention selects stainless steel wire and copper bar as preset auxiliary electrodes for the longitudinal reinforcement and stirrups to be rusted, respectively. By adjusting the size parameters of the two so that the anode area is much larger than the cathode area, and combining the distance, position and size ratio of the positive and negative electrodes, the non-uniform corrosion characteristics of the steel bars in the natural environment can be achieved. More importantly, the position of the specified local rusted section and the degree of steel bar corrosion can be accurately controlled.

[0020] 2. The present invention sets auxiliary electrodes respectively according to the types of steel bars to be rusted, which can achieve non-uniform corrosion of the longitudinal bars or stirrups to be rusted, wherein the distance between the steel bars to be rusted and the corresponding auxiliary electrodes completely matches the design parameters, which can effectively improve the similarity between the simulated environment and the real environment.

[0021] 3. The distance between the preset auxiliary electrode and the steel bar to be rusted is short in the present invention, and the energy consumed by the concrete resistance is small, which can significantly improve the accuracy of calculating the mass loss of steel bar corrosion using the Faraday law.

[0022] 4. The combined veneer method and the auxiliary electrode method of the present invention significantly lower the threshold for indoor and outdoor corrosion tests of large-size specimens and improve the corrosion efficiency: first, only a simple test shed needs to be set up to avoid the construction of a large corrosion pool, reducing site conditions and costs; second, the number of specimens in each batch is increased to shorten the test cycle.

[0023] 5. The present invention targets compression members with high stirrup ratio or axial compression ratio, or concrete structures with compression members as basic components, and vertically places the specimens for veneer corrosion in accordance with their stress state and corrosion scenario, properly solving the defects of the immersion method that concrete damage and steel bar corrosion cannot be dynamically monitored. At the same time, the width of the rust expansion cracks observed in real time can also be used to predict the degree of corrosion of the internal steel bars, as an auxiliary method for calculating the corrosion rate using the Faraday law. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0025] Figure 1 It is a schematic diagram of the spatial arrangement of the local corrosion test of steel bars in concrete components of the present invention.

[0026] Figure 2 The figure shows the corrosion zones (bottom) and detailed structures of the concrete pier column of the present invention.

[0027] Figure 3 This is a front view of the concrete pier column corrosion zone (bottom) and the test device provided in Example 1.

[0028] Figure 4 This is a top view of the concrete pier column corrosion zone (bottom) and the test device in Example 1.

[0029] Figure 5 This is a schematic structural diagram of the corrosion zone (middle part) of the concrete pier provided in Example 1.

[0030] Figure 6 A front view of the test device for the corrosion zone (middle part) of the concrete pier provided in Example 1.

[0031] Figure 7 This is a front view of the concrete beam local corrosion test device provided in Example 2.

[0032] In the figure: 1-concrete matrix; 2-longitudinal steel bars; 3-hoops; 4-stainless steel wires; 5-copper busbars; 6-anchors; 7-stainless steel U-shaped buckles; 8-moisturizing sponges; 9-waterproof plastic film; 10-DC regulated power supply; 11-conducting wires; 12-liquid storage tanks; 13-spray shower heads; 14-humidity sensors; 15-rusted concrete components; 16-DC regulated power supply equipment box; 17-rust test shed. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The purpose of the present invention is to provide a test device and a test method for simulating local corrosion of steel bars in concrete, overcome the limitations of existing simulated corrosion test technology, establish an electrochemical accelerated corrosion test method and a test device with high corrosion efficiency and controllable cost, which can effectively simulate local corrosion of steel bars in concrete structures, so as to achieve simulation and real-time monitoring of the entire process of steel bar corrosion to the greatest extent, and lay a solid foundation for the durability research of concrete structures in actual engineering.

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0036] Embodiment 1

[0037] refer to Figures 1 to 7 , a test device for simulating local corrosion of steel bars in concrete, comprising a test piece to be corroded, a preset auxiliary electrode, an anchoring system for fixing the preset auxiliary electrode, a dry-wet cycle simulation system and a DC regulated power supply, wherein the test piece to be corroded comprises a concrete matrix, longitudinal bars and stirrups arranged in the concrete matrix, the preset auxiliary electrode comprises a stainless steel wire arranged in the concrete matrix, outside the longitudinal bars and along the direction of the longitudinal bars, and a copper bar sequentially sleeved on the outer surface of the concrete matrix at intervals, both ends of the stainless steel wire extend out of the concrete matrix, the copper bar of the stainless steel wire corresponds to the position of the stirrup, one end of the stainless steel wire is connected to the negative electrode of the DC regulated power supply through a wire, the longitudinal bars are connected to the positive electrode of the DC regulated power supply, the copper bar is connected to the negative electrode of the DC regulated power supply, and the stirrup is connected to the positive electrode of the DC regulated power supply, and the dry-wet cycle system is used to perform dry treatment and wet treatment on the test piece to be corroded.

[0038] refer to Figure 2 The anchoring system includes an anchor arranged at the place where the stainless steel wire extends out of the concrete matrix, a high-strength gauze wrapped at both ends of the stainless steel wire and coated with epoxy resin, and the steel wire passes through the anchor.

[0039] refer to Figure 2The wet-dry cycle simulation system includes a moisturizing sponge wrapped on the outside of the concrete matrix, a humidity sensor arranged on the moisturizing sponge, a spray shower for spraying the moisturizing sponge, a liquid storage tank connected to the spray shower, and a waterproof plastic film wrapped on the outside of the moisturizing sponge after spraying.

[0040] refer to Figure 1 , also includes a corrosion test shed, the four sides and top of which are simple enclosures and covers respectively.

[0041] A test method for simulating local corrosion of steel bars in concrete, comprising the following steps: Binding a reinforced concrete specimen skeleton, wherein the reinforced concrete specimen skeleton comprises four longitudinal bars and a plurality of stirrups spaced apart in a direction perpendicular to the longitudinal bars; First, the stainless steel wire used to induce longitudinal reinforcement corrosion is passed through the mold, the tensioning degree and length of the stainless steel wire are adjusted, and the stainless steel wire anchoring technology is used to fix it in the local rusted section, and then the steel bar to be corroded is installed in the mold to achieve local non-uniform corrosion, and the conductor is led out; Pour concrete in the mold, remove the mold after one day, mark the detailed position information of the stirrups on the surface of the concrete specimen, and then cure the concrete specimen to the planned age; loosen the stainless steel wire before removing the mold; After reaching the planned age, copper bars with the same shape as the stirrups are arranged and fixed along the surface of the local corroded section according to the marked stirrup positions; the copper bars are fixed with reference to the copper bar anchoring technology, and the spacing between adjacent copper bars is exactly the same as the spacing between the corresponding stirrups; the distance between the stirrups and the copper bars is the thickness of the concrete cover. Due to the different distances between the copper bars and each point on the circumference of the steel bar, the different resistance spacing and concrete resistance lead to different current densities on the steel bar surface, so as to achieve non-uniform corrosion of the stirrups; First, place and fix the concrete specimen vertically, and take safety precautions. Then, connect one end of the stainless steel wire to the negative pole of the DC stabilized power supply, connect the longitudinal reinforcement to be corroded to the positive pole of the DC stabilized power supply, turn on the DC stabilized power supply, set the current, and record the current and time for corrosion. For stirrup corrosion, connect one end of the copper bar to the negative pole of the DC stabilized power supply. Other operations are the same as for longitudinal reinforcement corrosion. In order to form an electrolytic circuit and ensure that the air can fully contact the steel bars, a dry-wet cycle simulation system was established. The ratio of dry treatment to wet treatment was 3:4. The wet treatment method included sticking a moisturizing sponge on the concrete surface of the local rusted section, and using a spray shower to spray the NaCl solution in the storage tank on the moisturizing sponge in the local rusted section to stabilize the value range of the humidity sensor at 40-50%, and then covering it with a waterproof plastic film; after the expected power-on time was reached, the power was turned off to stop the dry-wet cycle.

[0042] Furthermore, the stainless steel wire anchoring technology: holes matching the steel wire are reserved in the molds at both ends of the specimen, and are accurately arranged according to the designed size and position; specially designed steel wire anchors are installed at both ends of the holes and the steel wire is passed through them; high-strength gauze coated with epoxy resin is wrapped at both ends of the steel wire, and after it is cured and dried, the steel wire is firmly anchored to the end of the specimen by adjusting the position of the anchor and tightening the clip.

[0043] The combination of epoxy resin and high-strength gauze forms a solid shell that firmly adheres to the surface of the steel wire and provides additional friction to prevent the steel wire from slipping. At the same time, it reasonably solves the problem of a single steel wire being unable to be anchored in the clamp, avoiding end damage or even pinching. Therefore, this method can ensure that the steel wire is always in the predetermined position during the pouring and curing process to achieve the expected corrosion target.

[0044] Furthermore, copper busbar anchoring technology: strictly control the shape and size of the copper busbar, determine the installation position according to the calibration information of the stirrups, and make it close to the surface of the specimen; install four sets of stainless steel U-shaped clips at equal intervals along the circumference of the specimen to ensure that the copper busbar is fixed and locked by the slot.

[0045] Furthermore, the moisturizing sponge and plastic film fixing technology: after the copper busbar is installed, the moisturizing sponge and waterproof plastic film sprayed with NaCl solution are wrapped around the test piece for one week, and then fixed with a detachable cable tie and a strong plastic buckle. The detachable cable tie is mainly used to facilitate the spraying of NaCl and the observation of rust cracks and products.

[0046] In order to avoid excessive corrosion current density causing the steel bar corrosion state to be inconsistent with the natural environment, the current density ( i corr ) should not exceed 600 μA / cm 2 , the current formula corresponding to a single steel bar is as follows:

[0047] In the formula, I corr is the corrosion current (mA); i corr is the corrosion current density (mA / mm 2 ); d is the diameter of the steel bar (mm); l is the length of the rusted section (mm).

[0048] The evaluation index of steel bar corrosion degree is mass loss rate. Firstly, the steel bar corrosion loss mass ( Δm t ), and then use Faraday's law to calculate the corresponding theoretical power-on time:

[0049] In the formula, t is the rusting time after power on (s); Z Fe is the ionic charge, Z Fe = 2; F is the Faraday constant (96485 C / mol); Δm t is the mass loss of steel bar due to corrosion (g); M Fe is the molecular weight of iron (56 g / mol).

[0050] Embodiment 2

[0051] As described in Example 1, a test device and a test method for simulating local corrosion of steel bars in concrete are provided. The specimen to be corroded is a concrete beam. The local corrosion that significantly affects its performance includes the tensile longitudinal reinforcement at the bottom of the specimen and the stirrups in the shear span. Other specific implementation methods will not be described in detail.

[0052] Adaptive changes made according to actual needs are all within the protection scope of the present invention.

[0053] It should be noted that it is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the invention. Any reference numeral in a claim should not be regarded as limiting the claim to which it relates.

Claims

1. A test device for simulating local corrosion of steel bars in concrete, characterized in that: The invention comprises a test piece to be corroded, a preset auxiliary electrode, an anchoring system for fixing the preset auxiliary electrode, a dry-wet cycle simulation system and a DC regulated power supply. The test piece to be corroded comprises a concrete matrix, longitudinal bars and stirrups arranged in the concrete matrix. The preset auxiliary electrode comprises a stainless steel wire arranged in the concrete matrix, outside the longitudinal bars and along the direction of the longitudinal bars, and a copper bar sleeved on the outer surface of the concrete matrix in sequence and at intervals. Both ends of the stainless steel wire extend out of the concrete matrix, and the copper bar of the stainless steel wire corresponds to the position of the stirrup. One end of the stainless steel wire is connected to the negative electrode of the DC regulated power supply through a wire, the longitudinal bars are connected to the positive electrode of the DC regulated power supply, the copper bar is connected to the negative electrode of the DC regulated power supply, and the stirrup is connected to the positive electrode of the DC regulated power supply. The dry-wet cycle system is used to perform dry treatment and wet treatment on the test piece to be corroded.

2. A test device for simulating local corrosion of steel bars in concrete according to claim 1, characterized in that: The anchoring system comprises an anchor arranged at the position where the stainless steel wire extends out of the concrete matrix, a high-strength gauze wrapped at both ends of the stainless steel wire and coated with epoxy resin, and the steel wire passes through the anchor.

3. A test device for simulating local corrosion of steel bars in concrete according to claim 2, characterized in that: The wet-dry cycle simulation system includes a moisturizing sponge wrapped around the outside of the concrete matrix, a humidity sensor arranged on the moisturizing sponge, a spray shower for spraying the moisturizing sponge, a liquid storage tank connected to the spray shower, and a waterproof plastic film wrapped around the outside of the moisturizing sponge after spraying.

4. A test device for simulating local corrosion of steel bars in concrete according to claim 3, characterized in that: It also includes a corrosion test shed, the four sides and top of which are respectively provided with simple enclosures and covers.

5. A test method for simulating local corrosion of steel bars in concrete, characterized in that: The test device for simulating local corrosion of steel bars in concrete according to any one of claims 1 to 4 comprises the following steps: (1) tying a steel bar skeleton of a concrete specimen, wherein the steel bar skeleton of the specimen to be corroded comprises four longitudinal bars and a plurality of stirrups arranged at intervals in a direction perpendicular to the longitudinal bars; (2) Pass the stainless steel wire used to induce corrosion of the longitudinal reinforcement through the mold, adjust the tension and length of the stainless steel wire, and anchor the stainless steel wire in the local corrosion section. Then, install the steel skeleton to be corroded in the mold, and lead out the two ends of the stainless steel wire; (3) Pour concrete in the mold, remove the mold after one day, and mark the detailed position information of the stirrups on the surface of the concrete specimen, and then cure the specimen to be corroded to the planned age; loosen the stainless steel wire before removing the mold; (4) After the planned age is reached, copper bars with the same shape as the stirrups are arranged and fixed along the surface of the local corroded section according to the marked stirrup positions; the spacing between adjacent copper bars is exactly the same as the spacing between the corresponding stirrups; the distance between the stirrups and the copper bars is the thickness of the concrete cover; (5) First, place and fix the specimen to be corroded vertically, then use a wire to connect one end of the stainless steel wire to the negative pole of the DC stabilized power supply, connect the longitudinal reinforcement to be corroded to the positive pole of the DC stabilized power supply, turn on the DC stabilized power supply, set the current, record the current and time for corrosion; for stirrup corrosion, connect one end of the copper busbar to the negative pole of the DC stabilized power supply, and other operations are the same as for longitudinal reinforcement corrosion; (6) Use a spray shower to spray the NaCl solution in the storage tank onto the moisturizing sponge in the locally corroded area, so that the value range of the humidity sensor is stabilized at 40-50%, and then cover it with a waterproof plastic film; after the expected power-on time is reached, turn off the power and stop the dry-wet cycle.

6. A test method for simulating local corrosion of steel bars in concrete according to claim 5, characterized in that: The formula for the current in step (5) is as follows:

7. In the formula, I corr is the corrosion current (mA); i corr is the corrosion current density (mA / mm 2 ); d is the diameter of the steel bar (mm); l is the length of the rusted section (mm).

8. A test method for simulating local corrosion of steel bars in concrete according to claim 5, characterized in that: The formula for the power-on time in step (5) is as follows:

9. In the formula, t is the rusting time after power on (s); Z Fe is the ionic charge, Z Fe = 2; F is the Faraday constant (96485 C / mol); Δm t is the mass loss of steel bar due to corrosion (g); M Feis the molecular weight of iron (56 g / mol).