Negative pole piece, battery and electric device
By designing a thinned and thickened double-layer coating structure on the negative electrode sheet of the lithium-ion battery, the problem of lithium precipitation at the edge of the battery is solved, and the cycle performance and capacity density of the battery are improved.
Patent Information
- Application Number
- CN202310446083.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-25
AI Technical Summary
Traditional lithium-ion secondary batteries are prone to edge lithium precipitation after continuous high-rate fast charging, which affects the cycle performance and life of the battery.
A negative electrode plate is designed, including a negative electrode current collector, a first coating and a second coating. The edge of the first coating is thinned, while the edge of the second coating is thickened, and the edge of the second coating is thickened. The lithium insertion capacity per unit area is greater than the lithium insertion capacity per unit area of the first coating to reduce the risk of lithium precipitation at the edge of the battery.
The double-layer coating structure reduces the risk of lithium precipitation at the edge of the battery during charging, improves the cycle performance of the battery, and increases the capacity density of the negative electrode sheet.
Smart Images

Figure CN118841519A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a negative electrode plate, a battery and an electrical device. Background Art
[0002] In recent years, the application scope of secondary batteries represented by lithium-ion batteries has become increasingly wide. With the rapid development of lithium-ion secondary batteries, people's demands for their charging speed, battery life, and safety performance are also increasing. Traditional lithium-ion secondary batteries are often prone to edge lithium deposition after continuous high-rate fast charging, which in turn affects the battery's cycle performance and life. Summary of the invention
[0003] Based on this, it is necessary to provide a negative electrode plate, a battery and an electrical device that can reduce the risk of lithium plating at the edge of the battery cell and improve the cycle performance of the lithium-ion battery.
[0004] In order to achieve the above-mentioned object, the first aspect of the present application provides a negative electrode sheet, comprising:
[0005] Anode current collector;
[0006] A first coating layer is disposed on the surface of the negative electrode current collector, comprising a first thinning area, a second thinning area, and a non-thinning area, wherein the first thinning area and the second thinning area are respectively located at the edges of the non-thinning area;
[0007] A second coating layer, at least partially disposed on the first coating layer, comprising a first thickened area, a second thickened area and a non-thickened area, wherein the first thickened area and the second thickened area are respectively located at the edges of the non-thickened area;
[0008] The lithium insertion capacity per unit area of the first coating layer is greater than the lithium insertion capacity per unit area of the second coating layer.
[0009] In the present application, the negative electrode plate includes a negative electrode current collector, a first coating and a second coating. The edges of the first coating are thinned, while the edges of the second coating are thickened, and the lithium insertion capacity per unit area of the second coating is greater than the lithium insertion capacity per unit area of the first coating. In this way, the lithium insertion capacity of the edge of the negative electrode plate is larger than that of the middle part, thereby reducing the risk of lithium deposition at the edge of the battery during charging and improving the cycle performance of the battery. In addition, through double-layer coating, the capacity density of the negative electrode plate can also be improved.
[0010] In some embodiments, the non-thickened region is arranged on the non-thinned region, the first thickened region is at least partially located on the negative electrode current collector, and the first thickened region is at least partially overlapped on the first thinned region, and the second thickened region is at least partially overlapped on the second thinned region.
[0011] In some of the embodiments, in a direction away from the non-thinned region, the thickness of the first thinned region gradually decreases, and the thickness of the second thinned region gradually decreases; and / or,
[0012] In the direction away from the non-thickened area, the thickness of the first thickened area first gradually increases and then gradually decreases, and the thickness of the second thickened area gradually increases.
[0013] In some embodiments, the maximum thickness of the second thickened region is less than the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
[0014] In some embodiments, the maximum thickness of the second thickened region is equal to the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
[0015] In some embodiments, at least a portion of the second thickened region is located on the negative electrode current collector.
[0016] In some embodiments, the maximum thickness of the first thickened region is equal to the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
[0017] In some embodiments, the difference between the maximum thickness of the first thickened area and the thickness of the non-thickened area is 20 μm to 300 μm, and can be 50 μm to 100 μm; and / or,
[0018] The difference between the maximum thickness of the second thickened area and the thickness of the non-thickened area is 20 μm to 300 μm, and can be 50 μm to 100 μm.
[0019] In some embodiments, the non-thickened area completely covers the non-thinned area; and / or,
[0020] The first thickened region completely covers the first thinned region; and / or,
[0021] The second thickened region completely covers the second thinned region.
[0022] In some embodiments, the second coating layer completely covers the first coating layer.
[0023] In some embodiments, the ratio of the lithium insertion capacity per unit area of the second coating layer to the lithium insertion capacity per unit area of the first coating layer is 1.08-1.9, and can be optionally 1.2-1.4.
[0024] In some embodiments, the lithium insertion capacity per unit area of the first coating is 0.03 mAh / mm 2 -0.04mAh / mm 2 , optional 0.03mAh / mm 2 -0.035mAh / mm2 ; and / or, the lithium embedding capacity per unit area of the second coating is 0.035 mAh / mm 2 -0.075mAh / mm 2 , optional 0.04mAh / mm 2 -0.05mAh / mm 2 .
[0025] In some embodiments, the active material in the first coating layer is a carbon material, and the active material in the second coating layer is a silicon-doped carbon material; or,
[0026] The active material in the first coating layer and the active material in the second coating layer are both silicon-doped carbon materials, and the doping amount of silicon in the active material of the first coating layer is less than the doping amount of silicon in the active material of the second coating layer.
[0027] In some embodiments, the mass percentage of the binder in the first coating layer is greater than the mass percentage of the binder in the second coating layer.
[0028] The binder in the first coating layer includes polyacrylic acid, and the binder in the second coating layer includes styrene-butadiene rubber.
[0029] The second aspect of the present application provides a secondary battery, comprising the negative electrode plate described in the first aspect of the present application.
[0030] The third aspect of the present application provides an electrical device, which includes the secondary battery described in the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the cross-sectional structure of the negative electrode sheet in one embodiment of the present application.
[0032] Figure 2 It is a schematic diagram of the cross-sectional structure of the negative electrode sheet in another embodiment of the present application.
[0033] Figure 3 It is a schematic diagram of the cross-sectional structure of a negative electrode sheet in another embodiment of the present application.
[0034] Figure 4 It is a schematic diagram of the cross-sectional structure of a negative electrode plate prefabricated sheet in one embodiment of the present application.
[0035] Figure 5 It is a schematic diagram of the cross-sectional structure of a negative electrode plate prefabricated sheet in another embodiment of the present application.
[0036] Figure 6 It is a schematic diagram of the cross-sectional structure of a negative electrode plate prefabricated sheet in another embodiment of the present application.
[0037] Figure 7 This is a schematic diagram of the cross-sectional structure of the negative electrode prefabricated sheet in Comparative Example 3 of the present application.
[0038] Figure 8 Schematic diagram of a secondary battery according to one embodiment of the present application.
[0039] Fig. 9 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.
[0040] Fig.10 Schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source.
[0041] Description of reference numerals:
[0042] 10 negative electrode current collector; 20 first coating layer; 30 second coating layer; 1 secondary battery; 11 housing; 12 electrode assembly; 13 cover plate; 2 electrical device. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme of the present application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application.
[0044] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0045] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0047] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0048] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0049] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features.
[0050] To sum up the background, the problem of battery lithium deposition has become a restrictive factor in the development of high-performance lithium-ion batteries. The research on the problem of battery lithium deposition is particularly interesting. The technical personnel of this application found in the long-term actual production and research and development process that the main reason for the edge lithium deposition phenomenon of lithium-ion secondary batteries after continuous high-rate fast charging is the uneven electrolyte infiltration and the thickening of the SEI film at the edge of the battery cell, which has never led to the deterioration of the dynamics at the edge of the battery cell and the occurrence of lithium deposition. Traditional methods use different ways to solve the technical problem of uneven electrolyte infiltration, including improving the injection process, improving the core winding process, adding electrolyte wetting agents, and selecting suitable diaphragms. The technical personnel of this application pay special attention to the improvement of the kinetic differences at the edge of the battery cell by the structure of the negative electrode plate, thereby solving the problem of lithium deposition caused by uneven electrolyte infiltration.
[0051] See also Figures 1 to 3 Based on this, an embodiment of the present application provides a negative electrode sheet, including:
[0052] Anode current collector 10;
[0053] A first coating layer 20 is disposed on the surface of the negative electrode current collector 10, including a first thinning area, a second thinning area, and a non-thinning area, wherein the first thinning area and the second thinning area are respectively located at the edges of the non-thinning area;
[0054] A second coating 30, at least partially disposed on the first coating, comprising a first thickened area, a second thickened area and a non-thickened area, wherein the first thickened area and the second thickened area are respectively located at the edges of the non-thickened area;
[0055] The lithium insertion capacity per unit area of the second coating layer 30 is greater than the lithium insertion capacity per unit area of the first coating layer 20 .
[0056] The negative electrode plate provided in the embodiment of the present application includes a negative electrode current collector, a first coating and a second coating, the edges of the first coating are respectively thinned, and the edges of the second coating are respectively thickened, and the lithium insertion capacity of the second coating is greater than the lithium insertion capacity of the first coating. In this way, the lithium insertion capacity of the edge of the negative electrode plate is larger than that of the middle part, thereby reducing the risk of lithium deposition at the edge of the battery during charging and improving the cycle performance of the battery. In addition, through double-layer coating, the capacity density of the negative electrode plate can also be improved.
[0057] In some embodiments, the ratio of the lithium insertion capacity per unit area of the second coating layer to the lithium insertion capacity per unit area of the first coating layer is 1.08-1.9, and can be optionally 1.2-1.4.
[0058] In some embodiments, the lithium insertion capacity per unit area of the first coating is 0.03 mAh / mm 2 -0.04mAh / mm 2 , optional 0.03mAh / mm 2 -0.035mAh / mm 2 ; and / or, the lithium embedding capacity per unit area of the second coating is 0.035 mAh / mm 2 -0.075mAh / mm 2 , optional 0.04mAh / mm 2 -0.05mAh / mm 2 .
[0059] The lithium insertion capacity per unit area of the coating has a well-known meaning in the art. The gram capacity of the coating can be tested by a buckle test method, and then the lithium insertion capacity per unit area is calculated by a formula. The specific calculation formula is: lithium insertion capacity per unit area = gram capacity * coating weight per unit area. The method for testing the gram capacity of the coating by the buckle test method can specifically include the following steps:
[0060] (1) Disassemble the battery cell and take out the negative electrode sheet, wipe off one side, leaving only the negative electrode sheet on the other side, and cut it into the size S required for the test buckle;
[0061] (2) Assembling the negative electrode sheet, separator, and lithium sheet into a button battery;
[0062] (3) Perform charge and discharge test on button battery: adjust the temperature box to 25℃, let stand for 120min; charge to 2.0V with 5mA constant current, let stand for 10min; discharge to 0.05V with 5mA constant current, let stand for 10min; charge to 2.0V with 5mA constant current; repeat the above cycle 3 times, and the third charge capacity is recorded as the total capacity A of button battery negative electrode;
[0063] (4) Take out the negative electrode after the test and weigh it to obtain the weight W1;
[0064] (5) Wiping off the active material of the negative electrode sheet in step (4) with a solvent and drying it to obtain a copper foil weight W2;
[0065] (6) Gram capacity of coating = A / S / (W1-W2)
[0066] In some embodiments, the non-thickened region is disposed on the non-thinned region, the first thickened region is at least partially located on the negative electrode current collector, and the first thickened region at least partially overlaps the first thinned region, and the second thickened region at least partially overlaps the second thinned region.
[0067] The width of the first thinned area is L11, the width of the second thinned area is L12, and the width of the non-thinned area is L13. The width of the first thickened area is L21, the width of the second thickened area is L22, and the width of the non-thickened area is L23.
[0068] In some embodiments, the non-thickened area completely covers the non-thinned area, and L13 is equal to L23.
[0069] In some embodiments, the first thickened region completely covers the first thinned region, and L11 is smaller than L21.
[0070] In some embodiments, the second thickened region completely covers the second thinned region, and L12 is less than or equal to L22.
[0071] Furthermore, in some embodiments, the second coating layer completely covers the first coating layer, and the width of the first coating layer is smaller than the width of the second coating layer.
[0072] The above-mentioned embodiments and their combined embodiments can further reduce the risk of lithium plating during the charging process.
[0073] In some embodiments, L11 and L12 are the same or different and are each independently selected from 3 mm to 30 mm.
[0074] Further optionally, L11 and L12 are each independently selected from 5 mm to 20 mm.
[0075] In some embodiments, in a direction away from the non-thinned region, the thickness of the first thinned region gradually decreases, and the thickness of the second thinned region gradually decreases.
[0076] In some embodiments, in a direction away from the non-thickened region, the thickness of the first thickened region first gradually increases and then gradually decreases, and the thickness of the second thickened region gradually increases. Figures 1 to 3 As shown, the thickness at the edge of the first thickened area of the second coating 30 is also gradually reduced. When the negative electrode slurry is coated on the surface of the negative collector 10, a certain area with reduced thickness is provided to reduce the risk of curling and bulging of the negative electrode sheet during subsequent use.
[0077] See also Figure 1 In some embodiments, the maximum thickness of the second thickened region is less than the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
[0078] See also Figure 2 In some embodiments, the maximum thickness of the second thickened region is equal to the sum of the thickness of the non-thinned region and the thickness of the non-thickened region. This embodiment can further increase the weight proportion of the active material of the second coating 30 at the end of the battery cell, further reduce the risk of lithium deposition of the negative electrode sheet during charging, and ensure the energy density of the negative electrode sheet. Furthermore, in some embodiments, at least part of the second thickened region is located on the negative electrode current collector 10.
[0079] See also Figure 3 In some embodiments, the maximum thickness of the first thickened region is equal to the sum of the thickness of the non-thinned region and the thickness of the non-thickened region. The current density of the negative electrode sheet near the negative electrode tab is relatively large, and the risk of lithium deposition is higher. Figure 3 The illustrated embodiment can further reduce the risk of lithium deposition in the negative electrode sheet during charging. The negative electrode tab can be arranged on the empty foil of the negative electrode sheet near the first thickened area.
[0080] In some embodiments, the difference between the maximum thickness of the first thickened region and the thickness of the non-thickened region is 20 μm to 300 μm.
[0081] Optionally, the difference between the maximum thickness of the first thickened area and the thickness of the non-thickened area is 50 μm to 100 μm.
[0082] In the above "20μm to 300μm", the difference between the maximum thickness of the first thickened area and the thickness of the non-thickened area includes the minimum ratio and the maximum ratio of the range, and each value between the minimum ratio and the maximum ratio. Specific examples include but are not limited to the point values in the embodiment and the following point values: 50μm, 100μm, 150μm, 200μm, 250μm. Or a range consisting of any two values.
[0083] In some embodiments, the difference between the maximum thickness of the second thickened region and the thickness of the non-thickened region is 20 μm to 300 μm.
[0084] Optionally, the difference between the maximum thickness of the second thickened area and the thickness of the non-thickened area is 50 μm to 100 μm.
[0085] In the above “20 μm to 300 μm”, the difference between the maximum thickness of the second thickened area and the thickness of the non-thickened area includes the minimum ratio and the maximum ratio of the range, and each value between the minimum ratio and the maximum ratio. Specific examples include but are not limited to the point values in the embodiment and the following point values: 50 μm, 100 μm, 150 μm, 200 μm, 250 μm. Or a range consisting of any two values.
[0086] In some embodiments, the thickness of the non-thickened area is 30 μm to 380 μm, and can be 50 μm to 100 μm.
[0087] In some embodiments, the thickness of the non-thinning area is 30 μm to 380 μm, and can be 50 μm to 100 μm.
[0088] The thickness T of each coating layer can be measured by using a micrometer, for example, a Mitutoyo 293-100 with an accuracy of 0.1 μm. It should be noted that the thickness of each coating layer described in this application refers to the thickness after cold pressing and used for battery assembly.
[0089] The first coating 20 includes a first active material, and the second coating 30 includes a second active material. The first active material and the second active material can be negative electrode active materials for batteries known in the art. As an example, at least one of the following materials may be included: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0090] In some optional embodiments, the first active material is a carbon material, and the second active material is a silicon-doped carbon material. Optionally, the carbon material is graphite.
[0091] In some optional embodiments, the first active material and the second active material are both silicon-doped carbon materials, and the silicon doping amount in the first active material is less than the silicon doping amount in the second active material. Optionally, the carbon material is graphite.
[0092] In some optional embodiments, the OI value of the first active material is greater than the OI value of the second active material.
[0093] The weight ratio of the first active material in the first coating layer 20 is 70-100 weight %, based on the total weight of the first coating layer 20. The weight ratio of the second active material in the second coating layer 30 is 70-100 weight %, based on the total weight of the second coating layer 30.
[0094] In some embodiments, the first coating layer 20 or the second coating layer 30 may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). The weight ratio of the binder in the first coating layer 20 or the second coating layer 30 is 0-30% by weight, based on the total weight of the first coating layer 20 or the second coating layer 30.
[0095] In some embodiments, the elastic modulus of the first coating 20 is greater than the elastic modulus of the second coating 30, thereby forming a negative electrode pole piece with low rebound in the middle region (non-thickened area / non-thinned area) and high rebound in the edge region (including the area corresponding to the first thickened area / first thinned area and the second thickened area / second thinned area), thereby improving the expansion rebound of the edge portion of the negative electrode pole piece, further reducing the risk of lithium plating, and improving the battery cycle performance.
[0096] Optionally, the mass percentage of the binder in the first coating layer 20 is less than the mass percentage of the binder in the second coating layer 30 .
[0097] Further optionally, the binder in the first coating layer 20 includes polyacrylic acid, and the binder in the second coating layer 30 includes styrene-butadiene rubber.
[0098] In some embodiments, the first coating layer 20 or the second coating layer 30 may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, carbon black (e.g., acetylene black or Ketjen black), carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the first coating layer 20 or the second coating layer 30 is 0-20% by weight, based on the total weight of the first coating layer 20 or the second coating layer 30.
[0099] In some embodiments, the first coating 20 or the second coating 30 may further include other additives, such as a thickener (e.g., sodium carboxymethyl cellulose (CMC-Na)), etc. The weight ratio of the other additives in the first coating 20 or the second coating 30 is 0-15% by weight, based on the total weight of the first coating 20 or the second coating 30.
[0100] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.
[0101] In some embodiments, the negative electrode sheet can be prepared by:
[0102] The above-mentioned components for preparing the first coating, such as the first active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a first coating slurry, wherein the first coating slurry has a solid content of 40-80wt% and a viscosity at room temperature adjusted to 5000-25000mPa·s.
[0103] The above-mentioned components for preparing the second coating, such as the second active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a second coating slurry, wherein the second coating slurry has a solid content of 40-80wt% and a viscosity at room temperature adjusted to 5000-25000mPa·s.
[0104] like Figure 4 As shown, the first coating slurry is coated on the surface of the negative electrode current collector to form a first coating prefabricated layer 201, and then the second coating slurry is coated on the surface of the first coating prefabricated layer 201 to form a second coating prefabricated layer 301. After drying, it is cold-pressed by a cold rolling mill to form a negative electrode prefabricated sheet, and the negative electrode prefabricated sheet is cut to obtain a negative electrode sheet. The compaction density of the negative electrode sheet is 1.2 to 3.0 g / cm 3 , optional 1.4-1.8g / cm 3 .
[0105] The thickness of the first coating prefabricated layer 201 is the thickness of the first coating, and the thickness of the second coating prefabricated layer 201 is the thickness of the second coating. The thickness T of each layer can be measured by a micrometer, for example, a micrometer with a model of Mitutoyo293-100 and an accuracy of 0.1 μm. It should be noted that the thickness of each layer in the negative electrode prefabricated sheet and the thickness of the first coating and the second coating all refer to the thickness of the corresponding layers in the negative electrode sheet after cold pressing and used to assemble the battery.
[0106] In some other embodiments, Figure 5 or Figure 6 As shown, prepare the negative electrode sheet preform.
[0107] It should be noted that Figures 4 to 6 Schematic diagram of the cross-sectional structure of the negative electrode sheet prefabricated sheet. The cross-section refers to a plane parallel to the thickness direction of the negative electrode sheet prefabricated sheet and perpendicular to the length direction of the negative electrode sheet prefabricated sheet. The dotted line L is the median line of the width of the negative electrode sheet prefabricated sheet. The negative electrode sheet prefabricated sheet can be cut into a plurality of negative electrode sheets by cutting the negative electrode sheet into two strips along the dotted line L and then cutting along the length direction of the negative electrode sheet prefabricated sheet. The thickness of the negative electrode sheet prefabricated sheet corresponds to the thickness of the negative electrode sheet.
[0108] Figure 4 The cross-sectional structure of the negative electrode sheet obtained by cutting the negative electrode sheet prefabricated sheet along the dotted line L is as follows Figure 1 shown. Figure 5 The cross-sectional structure of the negative electrode sheet obtained by cutting the negative electrode sheet prefabricated sheet along the dotted line L is as follows Figure 2 shown. Figure 6 The cross-sectional structure of the negative electrode sheet obtained by cutting the negative electrode sheet prefabricated sheet along the dotted line L is as follows Figure 3 shown.
[0109] The present application also provides a secondary battery, comprising the negative electrode sheet of any of the above embodiments.
[0110] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0111] Positive electrode
[0112] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0113] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0114] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. The polymer material substrate includes at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0115] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery known in the art.
[0116] As an example, the positive electrode active material of a lithium-ion secondary battery may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0117] The weight ratio of the positive electrode active material in the positive electrode film layer is 80-100 weight %, based on the total weight of the positive electrode film layer.
[0118] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.
[0119] In some embodiments, the positive electrode film layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, carbon black (e.g., acetylene black or Ketjen black), carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.
[0120] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry, wherein the positive electrode slurry has a solid content of 40-80wt%, and the viscosity at room temperature is adjusted to 5000-25000mPa·s, the positive electrode slurry is coated on the surface of the positive electrode collector, and after drying, the positive electrode sheet is formed by cold pressing with a cold rolling mill; the compaction density of the positive electrode sheet is 1.5-4.2g / cm 3 , optional: 2.3-3.7g / cm 3 The thickness of the positive electrode film is 30-380 μm.
[0121] The thickness T of the positive electrode film layer can be measured by using a micrometer, for example, a Mitutoyo 293-100 micrometer with an accuracy of 0.1 μm. It should be noted that the thickness of the positive electrode film layer described in this application refers to the thickness of the positive electrode film layer in the positive electrode sheet used for assembling the battery after cold pressing.
[0122] Electrolytes
[0123] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0124] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0125] In some embodiments, the electrolyte salt of the lithium ion secondary battery can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0126] The electrolyte salt of the sodium ion secondary battery can be selected from one or more of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.
[0127] The concentration of the electrolyte salt is usually 0.5-5 mol / L.
[0128] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0129] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0130] Isolation film
[0131] In some embodiments, the secondary battery further includes a separator.
[0132] In some embodiments, the isolation film can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation film is a multi-layer composite film, the materials of the base films of each layer can be the same or different, without particular limitation.
[0133] In some embodiments, the isolation film has a thickness of 3-30 μm, and optionally 5-12 μm.
[0134] In some embodiments, the air permeability of the isolation membrane may be 100s / 100mL-800s / 100mL; alternatively, the air permeability of the isolation membrane may be 150s / 100mL-350s / 100mL, tested according to national standard GB / T 36363-2018.
[0135] The thickness of the isolation can be measured by using a micrometer, for example, a Mitutoyo 293-100 micrometer with an accuracy of 0.1 μm.
[0136] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0137] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0138] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0139] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 8 The secondary battery 1 is a square structure as an example.
[0140] In some embodiments, reference Fig. 9 The outer package may include a shell 11 and a cover plate 13. The shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 11 has an opening connected to the receiving cavity, and the cover plate 13 can be covered on the opening to close the receiving cavity.
[0141] The positive electrode sheet, the negative electrode sheet and the separator can be wound or laminated to form an electrode assembly 12. The electrode assembly 12 is encapsulated in the housing cavity. The electrolyte is infiltrated in the electrode assembly 12. The number of electrode assemblies 12 contained in the secondary battery 1 can be one or more, which can be adjusted according to needs.
[0142] In some embodiments, the secondary batteries 1 may be assembled into a battery module. The number of secondary batteries 1 included in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0143] In the battery module, the plurality of secondary batteries 1 may be arranged in sequence along the length direction of the battery module. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 1 may be fixed by fasteners.
[0144] Optionally, the battery module may further include a housing having a receiving space, and the plurality of secondary batteries 1 are received in the receiving space.
[0145] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0146] The battery pack may include a battery box and a plurality of battery modules disposed in the battery box. The battery box includes an upper box body and a lower box body, and the upper box body can be covered on the lower box body to form a closed space for accommodating the battery modules. The plurality of battery modules can be arranged in the battery box in any manner.
[0147] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited to these.
[0148] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0149] Fig.10 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.
[0150] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0151] Example
[0152] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the present application will be further described in detail in conjunction with the embodiments below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its applications. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0153] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0154] Example 1
[0155] (1) Preparation of negative electrode sheet
[0156] First coating: add the first active material, conductive agent acetylene black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) into solvent water in a mass ratio of 96.5:0.5:1.8:1.2 and mix evenly to form a first active slurry; evenly coat the first active slurry on the negative electrode current collector copper foil, dry it, and then cold press it to form a first coating.
[0157] Second coating: add the second active material, conductive agent acetylene black, thickener sodium carboxymethyl cellulose (CMC), and binder styrene butadiene rubber (SBR) into solvent water in a mass ratio of 96.5:0.5:1.8:1.2 and mix evenly to form a second active slurry; evenly apply the second active slurry on the first coating, dry and then cold press to form a second coating to obtain a negative electrode preform.
[0158] The schematic diagram of the cross-sectional structure of the negative electrode preform formed is as follows: Figure 4 As shown, it is ensured that a structure in which the first coating is thinner and the second coating is thicker is formed in the striping area (the area shown in the dotted box A, i.e., the area near the dotted line L) and the edge of the coating, the coating width of the first coating is L1, and the coating width of the second coating is L2, ensuring that L2 is greater than L1.
[0159] The negative electrode sheet prefabricated sheet is cut along the dotted line L to obtain the negative electrode sheet.
[0160] (2) Preparation of positive electrode sheet
[0161] The nickel-cobalt-manganese (NCM111) ternary material, the conductive agent acetylene black, the conductive carbon nanotubes, and the binder polyvinylidene fluoride (PVLF) are dissolved in a solvent N-methylpyrrolidone (NMP) at a weight ratio of 97.9:1.7:0.4:1, and the positive electrode slurry is obtained after being fully stirred and mixed. Thereafter, the positive electrode slurry is evenly coated on the positive electrode collector, and then dried, cold pressed, and cut to obtain the positive electrode sheet.
[0162] (3) Preparation of electrolyte
[0163] The organic solvent is a mixed solution containing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (LEC), wherein the volume ratio of EC, EMC and LEC is 1:1:1. In an argon atmosphere glove box with a water content of <10ppm, fully dried LiPF6 is dissolved in the organic solvent and mixed evenly to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0164] (4) Isolation film
[0165] A polyethylene microporous film is used as the porous isolation membrane substrate.
[0166] (5) Preparation of batteries
[0167] The positive electrode sheet, negative electrode sheet and separator are wound to obtain a bare cell, and then the finished battery is obtained by adopting the above-mentioned aluminum-plastic film packaging, liquid injection, formation, exhaust and other processes.
[0168] Example 2
[0169] The preparation method is basically the same as that of Example 1, except that the cross-sectional structure diagram of the negative electrode preform is as follows: Figure 5 shown.
[0170] Example 3
[0171] The preparation method is basically the same as that of Example 1, except that the cross-sectional structure diagram of the negative electrode preform is as follows: Figure 6 shown.
[0172] Embodiments 4 to 6
[0173] The preparation method is basically the same as that of Example 1, except that the first active material in Example 1 is replaced by the corresponding first active material shown in Table 1, and the second active material in Example 1 is replaced by the corresponding second active material shown in Table 1.
[0174] Embodiment 7-8
[0175] The preparation method is basically the same as that of Example 1, except that the second active material, the first coating binder and its mass fraction, and the second coating binder and its mass fraction in Example 1 are replaced with the corresponding second active material, the first coating binder and its mass fraction, and the second coating binder and its mass fraction shown in Table 1, and the proportion of the active materials is adjusted accordingly to ensure that the total mass of the coating is the same between the embodiments. For example, in Example 7, the mass fraction of the binder in the first coating is changed to 1.8%, and the mass fraction of the first active material is adjusted to 90.5%, which is calculated based on the total mass of the first coating (excluding the mass of the solvent).
[0176] Comparative Example 1
[0177] The preparation method is basically the same as that of Example 3, except that the cross-sectional structure diagram of the negative electrode preform is as follows: Figure 7 As shown, Figure 7 and Figure 6 The difference is that Figure 7 The structure where the first coating is thinned and the second coating is thickened is not performed at the middle dividing line (the area near the dotted line L).
[0178] Comparative Example 2
[0179] The preparation method is basically the same as that of Example 3, except that the first coating and the second coating have the same composition.
[0180] The gram capacities of the first coating layer and the second coating layer in the above embodiments and comparative examples are listed in Table 1. According to the formula: lithium insertion capacity per unit area = gram capacity * coating weight per unit area, the ratio of the lithium insertion capacity per unit area of the first coating layer to the lithium insertion capacity per unit area of the second coating layer is R = first coating gram capacity / second coating gram capacity.
[0181] Test Case
[0182] 1. Cycle performance test
[0183] Each secondary battery prepared as above was charged to 4.25V at a constant current of 0.5C at 25°C, then charged at a constant voltage of 4.25V until the current dropped to 0.05C, and then discharged to 2.8V at a constant current of 1C to obtain the first cycle discharge capacity (Cd1); the charging and discharging were repeated to the nth cycle, and the discharge capacity of the lithium-ion battery after n cycles was obtained, which was recorded as Cdn, and the capacity retention rate of the secondary battery was calculated according to the following formula:
[0184] Capacity retention rate = discharge capacity after n cycles (Cdn) / first cycle discharge capacity (Cd1).
[0185] 2. Lithium dendrites
[0186] After each of the secondary batteries prepared above was cycled 1200 times according to the charge and discharge method described in the above "1. Cycle Performance Test", the secondary batteries were disassembled in a glove box (H2O < 0.1ppm, O2 < 0.1ppm), and the surface morphology of the negative electrode was visually observed to determine whether lithium dendrites were generated. If there were no white spots on the negative electrode, it was determined that there was no lithium deposition, if there were sporadic white spots on the negative electrode, it was determined that there was slight lithium deposition, and if there were dense white spots on the negative electrode, it was determined that there was severe lithium deposition.
[0187] Table 1
[0188]
[0189]
[0190] It should be noted that the mass fractions of graphite and silicon in Table 1 are based on the total mass of the active material, for example, "97% graphite + 3% silicon" means that the mass fraction of graphite in the active material is 97%, and the mass fraction of silicon is 3%; the mass fractions of SBR and PAA are based on the total mass of the first coating or the second coating (excluding the mass of the solvent), for example, "1.2% SBR" means that the mass fraction of SBR in the coating is 1.2%. The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-mentioned embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0191] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description and drawings may be used to interpret the contents of the claims.
Claims
1. A negative electrode plate, characterized in that: include: Anode current collector; A first coating layer is disposed on the surface of the negative electrode current collector, comprising a first thinning area, a second thinning area, and a non-thinning area, wherein the first thinning area and the second thinning area are respectively located at the edges of the non-thinning area; A second coating layer, at least partially disposed on the first coating layer, comprising a first thickened area, a second thickened area and a non-thickened area, wherein the first thickened area and the second thickened area are respectively located at the edges of the non-thickened area; The lithium insertion capacity per unit area of the second coating layer is greater than the lithium insertion capacity per unit area of the first coating layer.
2. The negative electrode sheet according to claim 1, characterized in that: The non-thickened region is arranged on the non-thinned region, the first thickened region is at least partially located on the negative electrode current collector, and the first thickened region is at least partially overlapped on the first thinned region, and the second thickened region is at least partially overlapped on the second thinned region.
3. The negative electrode sheet according to claim 1, characterized in that: In a direction away from the non-thinned area, the thickness of the first thinned area gradually decreases, and the thickness of the second thinned area gradually decreases; and / or, In the direction away from the non-thickened area, the thickness of the first thickened area first gradually increases and then gradually decreases, and the thickness of the second thickened area gradually increases.
4. The negative electrode sheet according to any one of claims 1 to 3, characterized in that: The maximum thickness of the second thickened region is less than the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
5. The negative electrode sheet according to any one of claims 1 to 3, characterized in that: The maximum thickness of the second thickened region is equal to the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
6. The negative electrode sheet according to claim 5, characterized in that: At least a portion of the second thickened region is located on the negative electrode current collector.
7. The negative electrode sheet according to any one of claims 1 to 6, characterized in that: The maximum thickness of the first thickened region is equal to the sum of the thickness of the non-thinned region and the thickness of the non-thickened region.
8. The negative electrode sheet according to any one of claims 1 to 7, characterized in that: The difference between the maximum thickness of the first thickened area and the thickness of the non-thickened area is 20 μm to 300 μm, and can be 50 μm to 100 μm; and / or, The difference between the maximum thickness of the second thickened area and the thickness of the non-thickened area is 20 μm to 300 μm, and can be 50 μm to 100 μm.
9. The negative electrode sheet according to any one of claims 1 to 7, characterized in that: The non-thickened area completely covers the non-thinned area; and / or, The first thickened region completely covers the first thinned region; and / or, The second thickened region completely covers the second thinned region.
10. The negative electrode sheet according to claim 9, characterized in that: The second coating layer completely covers the first coating layer.
11. The negative electrode sheet according to any one of claims 1 to 10, characterized in that: The ratio of the lithium insertion capacity per unit area of the second coating layer to the lithium insertion capacity per unit area of the first coating layer is 1.08-1.9, and can be optionally 1.2-1.
4.
12. The negative electrode sheet according to any one of claims 1 or 11, characterized in that: The lithium insertion capacity per unit area of the first coating is 0.03 mAh / mm 2 -0.04mAh / mm 2 , optional 0.03mAh / mm 2 -0.035mAh / mm 2 ; and / or, the lithium embedding capacity per unit area of the second coating is 0.035 mAh / mm 2 -0.075mAh / mm 2 , optional 0.04mAh / mm 2 -0.05mAh / mm 2 .
13. The negative electrode sheet according to claim 11 or 12, characterized in that: The active material in the first coating layer is a carbon material, and the active material in the second coating layer is a silicon-doped carbon material; or, The active material in the first coating layer and the active material in the second coating layer are both silicon-doped carbon materials, and the doping amount of silicon in the active material of the first coating layer is less than the doping amount of silicon in the active material of the second coating layer.
14. The negative electrode sheet according to claim 13, characterized in that: The mass percentage of the binder in the first coating layer is greater than the mass percentage of the binder in the second coating layer.
15. The negative electrode sheet according to claim 13, characterized in that: The binder in the first coating layer includes polyacrylic acid, and the binder in the second coating layer includes styrene-butadiene rubber.
16. A secondary battery, characterized in that: It comprises the negative electrode sheet as described in any one of claims 1 to 15.
17. An electrical device, characterized in that: Comprising the secondary battery as claimed in claim 16.
Citation Information
Cited By
Negative pole piece, preparation method thereof and battery
CN119852307A
Battery pole piece, electroplating method thereof, electroplating device, battery cell and battery
CN121407170A