Positive pole piece and preparation method thereof, battery monomer, battery and electric device
By adding a pore-forming agent to the positive electrode sheet of the battery cell and decomposing it during the formation process to form a pore structure, the problem of insufficient cycle performance of the battery cell is solved, the liquid retention capacity and cycle life of the battery are improved, and the improve the energy density and power performance of the battery.
Patent Information
- Application Number
- CN202310446460.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-25
AI Technical Summary
The cycle performance of battery cells still needs to be improved, and it is difficult to effectively improve the battery's liquid retention capacity and cycle life with existing technology.
During the preparation process of the positive electrode sheet, a pore-forming agent is added and decomposed during the battery monomerization process to form a pore structure to increase the electrolyte retention capacity. By adding alkali metals and/or alkaline earths to the positive electrode slurry Pore-forming agents such as metal tetrahydroborate are combined with polyanionic materials to adjust the content and particle size of the pore-forming agent to form a uniform pore structure.
The cycle life and energy density of the battery cells are significantly improved, the service life of the battery is extended, and the power performance and active ion and electron transmission performance of the battery are improved.
Smart Images

Figure CN118841524A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and more specifically, to a positive electrode plate and a preparation method thereof, a battery cell, a battery and an electrical device. Background Art
[0002] Battery cells are widely used because of their reliable working performance, no pollution, and no memory effect. For example, as environmental protection issues are increasingly valued and new energy vehicles become more popular, the demand for power battery cells will show explosive growth.
[0003] As battery applications become more and more extensive, the requirements for battery performance are becoming increasingly stringent. However, the cycle performance of battery cells still needs to be improved. Summary of the invention
[0004] The present application provides a positive electrode plate and a preparation method thereof, a battery cell, a battery and an electrical device, which can improve the cycle performance of the battery cell.
[0005] In a first aspect, an embodiment of the present application provides a method for preparing a positive electrode sheet, comprising:
[0006] Providing a positive electrode active material and a pore-forming agent, and adding the positive electrode active material and the pore-forming agent into a solvent to mix them into a positive electrode slurry;
[0007] The positive electrode slurry is coated on at least one side of the positive electrode current collector, and after drying, a positive electrode active material layer is formed to prepare a positive electrode sheet, wherein the pore former is configured to decompose and generate gas during the battery monomer formation process.
[0008] Therefore, according to the method implemented in the present application, by adding a pore-forming agent to the positive electrode slurry, when the positive electrode plate is applied to the battery cell, during the formation process (the battery cell is charged for the first time), the pore-forming agent will decompose and release gas, and after the gas is discharged, a pore structure will be left in the positive electrode active material layer. The pore structure is conducive to retaining the electrolyte, thereby increasing the electrolyte retention capacity, thereby extending the cycle life of the battery cell.
[0009] In some embodiments, the pore former includes one or more of alkali metal and / or alkaline earth metal tetrahydroborate, alkali metal and / or alkaline earth metal sulfide, alkali metal and / or alkaline earth metal thiosulfate, alkali metal and / or alkaline earth metal sulfate, alkali metal and / or alkaline earth metal carbonate, alkali metal and / or alkaline earth metal citrate, alkali metal and / or alkaline earth metal glutamate, alkali metal and / or alkaline earth metal squarate. The above-mentioned pore former and polyanion material are used in combination, which is conducive to the uniform pore formation of the pore former in the positive electrode active material layer, and increases the liquid retention, which can further improve the cycle performance.
[0010] In some embodiments, the alkali metal and / or alkaline earth metal tetrahydroborate includes one or more of sodium tetrahydroborate and potassium tetrahydroborate.
[0011] In some embodiments, the alkali metal and / or alkaline earth metal sulfide includes one or more of sodium sulfide, lithium disulfide, and potassium sulfide.
[0012] In some embodiments, the alkali metal and / or alkaline earth metal thiosulfate includes one or more of sodium thiosulfate and potassium thiosulfate.
[0013] In some embodiments, the alkali metal and / or alkaline earth metal sulfate includes one or more of sodium sulfate and potassium sulfate.
[0014] In some embodiments, the alkali metal and / or alkaline earth metal carbonate includes one or more of sodium carbonate and potassium carbonate.
[0015] In some embodiments, the alkali metal and / or alkaline earth metal citrate includes one or more of sodium citrate and lithium citrate.
[0016] In some embodiments, the alkali metal and / or alkaline earth metal glutamate includes one or more of sodium glutamate and potassium glutamate.
[0017] In some embodiments, the alkali metal and / or alkaline earth metal squarate includes one or more of potassium squarate, sodium squarate, and lithium squarate.
[0018] In some embodiments, the positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, and the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1. The above-mentioned polyanion material and pore-forming agent are used in combination, which is conducive to uniform pore formation of the pore-forming agent in the positive electrode active material layer, and increases the liquid retention, which can further improve the cycle performance.
[0019] In some embodiments, based on the total mass of the positive electrode slurry, the ratio of the mass percentage of the pore former to the mass percentage of the positive electrode active material is 1:(8 to 95). When the mass percentage ratio of the pore former to the positive electrode active material is within the above range, it is beneficial for the pore former to uniformly form pores in the positive electrode active material layer and increase the liquid retention, which can further improve the cycle performance.
[0020] In some embodiments, the mass percentage of the pore former is 1% to 20%.
[0021] In some embodiments, the mass percentage of the positive electrode active material is 80% to 95%.
[0022] In some embodiments, the volume average particle size D of the pore former v50 The volume average particle size D of the positive electrode active material v50 The ratio is 1:(3 to 25). The volume average particle size D of the pore-forming agent v50 The volume average particle size D of the positive electrode active material v50 When the ratio is within the above range, it is beneficial for the pore-forming agent to uniformly form pores in the positive electrode active material layer and increase the liquid retention amount, which can further improve the cycle performance.
[0023] In some embodiments, the volume average particle size D of the pore former v50 0.2 μm to 2 μm; and / or
[0024] In some embodiments, the volume average particle size D of the positive electrode active material is v50 3μm to 15μm.
[0025] In a second aspect, an embodiment of the present application proposes a positive electrode plate, which is prepared by the method described in any embodiment of the first aspect of the present application.
[0026] In a third aspect, the present application provides a method for preparing a battery cell, comprising:
[0027] Providing a positive electrode sheet prepared by the method described in any embodiment of the first aspect of the present application;
[0028] The positive electrode sheet, the separator and the negative electrode sheet are assembled into a shell, and an electrolyte is injected into the shell. During the chemical formation treatment, the pore former in the positive electrode active material layer is decomposed so that the positive electrode active material layer has a pore structure.
[0029] In a fourth aspect, the present application embodiment proposes a battery cell, the battery cell includes a positive electrode sheet, the positive electrode sheet includes: a positive current collector; a positive active material layer disposed on at least one surface of the positive current collector, the porosity of the positive active material layer is 38% to 65%. Since the pore former decomposes into gas, a pore structure is formed in the positive active material layer as the gas volatilizes, so that the porosity of the positive active material layer meets the above range, which is conducive to increasing the liquid retention amount and can further improve the cycle performance.
[0030] In some embodiments, the positive electrode active material layer has a porosity of 40% to 65%.
[0031] In some embodiments, the positive electrode active material layer includes a positive electrode active material, and the mass percentage of the positive electrode active material relative to the positive electrode active material layer is 80% to 98%, and optionally 85% to 95%. The mass percentage of the positive electrode active material is relatively high, which can effectively improve the energy density of the battery cell.
[0032] In some embodiments, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0≤x / m≤1.
[0033] In some embodiments, the surface density of the positive electrode active material layer is 0.2 g / 1540.25 cm 2 Up to 0.4g / 1540.25cm 2 , optional: 0.3g / 1540.25cm 2 Up to 0.38g / 1540.25cm 2 When the surface density of the positive electrode active material layer is within the above range, the capacity density of the battery cell can be increased, and the battery cell can also have excellent active ion and electron transport properties, which can improve the power performance of the battery cell, reduce polarization and side reactions, and further improve the cycle performance of the battery cell.
[0034] In some embodiments, the compaction density of the positive electrode active material layer is 1.8 g / cc to 2.9 g / cc. The compaction density of the positive electrode active material layer within the above range can improve the energy density of the battery cell and further improve the power performance of the battery cell. In addition, a suitable compaction density can further improve the cycle life of the battery cell.
[0035] In a fifth aspect, an embodiment of the present application proposes a battery, comprising a battery cell as described in any embodiment of the fourth aspect of the present application.
[0036] In a sixth aspect, the present application proposes an electrical device, comprising a battery as described in any embodiment of the fifth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0038] Figure 1 It is a schematic diagram of an embodiment of a battery cell of the present application.
[0039] Figure 2 yes Figure 1 A schematic cross-sectional view of a battery cell along line AA.
[0040] Figure 3 It is a schematic diagram of an embodiment of a battery module of the present application.
[0041] Figure 4 It is a schematic diagram of an embodiment of the battery pack of the present application.
[0042] Figure 5 yes Figure 4 An exploded schematic diagram of an embodiment of a battery pack is shown.
[0043] Figure 6 It is a schematic diagram of an embodiment of an electric device including the battery cell of the present application as a power source.
[0044] The drawings are not necessarily drawn to scale.
[0045] The following are the descriptions of the reference numerals:
[0046] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Battery module;
[0047] 5. Battery cell; 51. Housing; 52. Electrode assembly;
[0048] 53. Cover plate;
[0049] 6. Electrical equipment. DETAILED DESCRIPTION
[0050] Hereinafter, the embodiments of the positive electrode sheet and its preparation method, battery cell, battery and electrical device of the present application are specifically disclosed in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0051] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0053] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0054] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0055] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0056] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0057] A battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The separator is located between the positive electrode sheet and the negative electrode sheet to isolate the positive electrode sheet from the negative electrode sheet. Active ions migrate between the positive electrode sheet and the negative electrode sheet through the electrolyte, thereby realizing the charging and discharging of the battery cell.
[0058] During the charge and discharge process of the battery cell, the volume of the electrode assembly may change (such as volume expansion), causing the electrolyte adsorbed in the electrode assembly to be squeezed out. The liquid retention capacity of the electrode assembly is relatively low. During the battery cycle charge and discharge process, the electrolyte is continuously and rapidly consumed, which will deteriorate the cycle performance of the battery cell.
[0059] In view of this, the present application improves the positive electrode plate and the porosity of the positive active material layer in the positive electrode plate, thereby increasing the amount of electrolyte adsorbed by the positive electrode plate, thereby increasing the electrolyte content injected into the battery cell and increasing the injection volume, thereby extending the cycle life of the battery cell.
[0060] Method for preparing positive electrode sheet
[0061] In a first aspect, an embodiment of the present application provides a method for preparing a positive electrode sheet, comprising:
[0062] Step S100, providing a positive electrode active material and a pore-forming agent, and adding the positive electrode active material and the pore-forming agent into a solvent to mix them into a positive electrode slurry;
[0063] Step S200, coating the positive electrode slurry on at least one side of the positive electrode current collector, forming a positive electrode active material layer after drying, and preparing a positive electrode sheet, wherein the pore former is configured to decompose and generate gas during the battery monomer formation treatment.
[0064] According to the method implemented in the present application, by adding a pore-forming agent to the positive electrode slurry, when the positive electrode plate is applied to the battery cell, during the formation process (the battery cell is charged for the first time), the pore-forming agent will decompose and release gas. After the gas is discharged, a pore structure will be left in the positive electrode active material layer. The pore structure is conducive to retaining the electrolyte, thereby increasing the liquid retention capacity of the electrolyte, thereby extending the cycle life of the battery cell. It can be understood that the cycle performance of this system can rely on the liquid storage capacity of the pore structure to a higher extent.
[0065] During the production of battery cells, a formation process is required, which is to use chemical and electrochemical reactions to activate the active substances on the electrode components and convert them into positive and negative electrodes with electrochemical properties.
[0066] In some embodiments, the positive electrode slurry may be coated on one side or both sides of the positive electrode current collector. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode slurry is disposed on any one or both of the two opposite surfaces of the positive electrode current collector; thereby, the positive electrode active material layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0067] The present application is applicable to the sodium salt system of polyanion materials, for example, the positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1.
[0068] In some embodiments, 0<y≤1.
[0069] In some embodiments, 0<m≤2.
[0070] As some examples, the polyanionic material includes one or more of phosphates, pyrophosphates, and mixed polyanionic compounds.
[0071] Exemplarily, the phosphate includes one or more of NaCoPO4, NaFePO4, NaMnPO4 and Na3V2(PO4)3. Na3V2(PO4)3 is converted to NaV2(PO4)3 with a molar amount of sodium being 1. 2 / 3 (PO4).
[0072] Exemplarily, the pyrophosphate includes one or more of Na2CoP2O7, Na2FeP2O7, and Na2MnP2O7.
[0073] Exemplarily, the mixed polyanionic compound includes one or more of Na4Co3(PO4)2P2O7, Na4Fe3(PO4)2P2O7 and Na4Mn3(PO4)2P2O7. Na4Co3(PO4)2P2O7 is converted to NaCo with a molar amount of sodium being 1. 0.75 (PO4) 0.5 (P2O7) 0.25 (NaCo 0.75 P1O 3.75); Na4Fe3(PO4)2P2O7 is converted to NaFe with the molar amount of sodium as 1 0.75 (PO4) 0.5 (P2O7) 0.25 (NaFe 0.75 P1O 3.75 ); Na4Mn3(PO4)2P2O7 is converted to NaMn with the molar amount of sodium as 1 0.75 (PO4) 0.5 (P2O7) 0.25 (NaFe 0.75 P1O 3.75 ).
[0074] In the present application, the polyanionic compound may also be modified, for example, by doping modification and / or surface coating modification.
[0075] In some embodiments, the pore former may include one or more of alkali metal and / or alkaline earth metal tetrahydroborate, alkali metal and / or alkaline earth metal sulfide, alkali metal and / or alkaline earth metal thiosulfate, alkali metal and / or alkaline earth metal sulfate, alkali metal and / or alkaline earth metal carbonate, alkali metal and / or alkaline earth metal citrate, alkali metal and / or alkaline earth metal glutamate, alkali metal and / or alkaline earth metal squarate.
[0076] As some examples, the alkali metal and / or alkaline earth metal tetrahydroborate includes one or more of sodium tetrahydroborate and potassium tetrahydroborate.
[0077] As some examples, the alkali metal and / or alkaline earth metal sulfide includes one or more of sodium sulfide, lithium disulfide, and potassium sulfide.
[0078] As some examples, the alkali metal and / or alkaline earth metal thiosulfate includes one or more of sodium thiosulfate and potassium thiosulfate.
[0079] As some examples, the alkali metal and / or alkaline earth metal sulfate includes one or more of sodium sulfate and potassium sulfate.
[0080] As some examples, the alkali metal and / or alkaline earth metal carbonate includes one or more of sodium carbonate and potassium carbonate.
[0081] As some examples, the alkali metal and / or alkaline earth metal citrate includes one or more of sodium citrate and lithium citrate.
[0082] As some examples, the alkali metal and / or alkaline earth metal glutamate includes one or more of sodium glutamate and potassium glutamate.
[0083] As some examples, the alkali metal and / or alkaline earth metal squarate includes one or more of potassium squarate, sodium squarate, and lithium squarate.
[0084] The above-mentioned pore-forming agent and polyanion material are used in combination, which is beneficial for the pore-forming agent to uniformly form pores in the positive electrode active material layer and increase the liquid retention amount, which can further improve the cycle performance.
[0085] In some embodiments, based on the total mass of the positive electrode slurry, the ratio of the mass percentage of the pore former to the mass percentage of the positive electrode active material is 1:(8 to 95). When the mass percentage ratio of the pore former to the positive electrode active material is within the above range, it is beneficial for the pore former to uniformly form pores in the positive electrode active material layer and increase the liquid retention, which can further improve the cycle performance.
[0086] Exemplarily, the ratio of the mass percentage of the pore former to the mass percentage of the positive electrode active material can be 1:8, 1:9, 1:10, 1:12, 1:14, 1:15, 1:16, 1:18, 1:19, 1:20, 1:22, 1:24, 1:25, 1:26, 1:27, 1:28, 1:30, 1:32, 1:34, 1:35, 1:36, 1:37, 1:38, 1:40, 1:42, 1:45, 1:46, 1:48, 1:50, 1:52, 1:55, 1:56, 1:58, 1:60, 1:65, 1:70, 1:75, 1:80, 1:85, 1:90, 1:95 or a range consisting of any two of the above values.
[0087] In some embodiments, the mass percentage of the pore-forming agent is 1% to 20%. For example, the mass percentage of the pore-forming agent can be 1%, 2%, 5%, 6%, 7%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, or a range consisting of any two of the above values.
[0088] In some embodiments, the mass percentage of the positive electrode active material is 80% to 95%. For example, the mass percentage of the positive electrode active material can be 80%, 82%, 85%, 86%, 88%, 90%, 91%, 92%, 93%, 94%, 95% or a range consisting of any two of the above values.
[0089] In some embodiments, the volume average particle size D of the pore former v50 The volume average particle size D of the positive electrode active material v50 The ratio is 1:(3 to 25). The volume average particle size D of the pore-forming agent v50 The volume average particle size D of the positive electrode active material v50When the ratio is within the above range, it is beneficial for the pore-forming agent to uniformly form pores in the positive electrode active material layer and increase the liquid retention amount, which can further improve the cycle performance.
[0090] The volume average particle size D of the pore former v50 The volume average particle size D of the positive electrode active material v50 The ratio can be 1:3, 1:4, 1:5, 1:6, 1:8, 1:9, 1:10, 1:12, 1:15, 1:16, 1:18, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25 or a range consisting of any two of the above values.
[0091] In some embodiments, the volume average particle size D of the pore former v50 For example, the volume average particle size D of the pore former is 0.2 μm to 2 μm. v50 It may be 0.2 μm, 0.3 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.2 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.8 μm, 2 μm, or a range consisting of any two of the above values.
[0092] In some embodiments, the volume average particle size D of the positive electrode active material is v50 For example, the volume average particle size D of the positive electrode active material is 3 μm to 15 μm. v50 It can be 3μm, 3.3μm, 3.5μm, 3.8μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, 13μm, 13.5μm, 14.5μm, 15μm or a range consisting of any two of the above values.
[0093] In the embodiment of the present application, the volume average particle size D of the material v50 It refers to the particle size corresponding to 50% of the volume distribution. The volume average particle size Dv50 can be tested by Mastersizer 2000E laser particle size analyzer according to GB / T 19077-2016.
[0094] In some embodiments, the positive electrode slurry may further include a positive electrode conductor. The positive electrode active material layer may further include a positive electrode conductor. The present application has no particular restrictions on the type of the positive electrode conductor. As an example, the positive electrode conductor includes at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. In some embodiments, based on the total mass of the positive electrode active material layer, the mass percentage of the positive electrode conductor is ≤5%.
[0095] In some embodiments, the positive electrode slurry may also optionally include a positive electrode binder. The positive electrode active material layer may also include a positive electrode binder. The present application has no particular restrictions on the type of the positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode active material layer, the mass percentage of the positive electrode binder is ≤5%.
[0096] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0097] Positive electrode
[0098] In a second aspect, an embodiment of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode active material layer disposed on at least one surface of the positive electrode collector.
[0099] In some embodiments, the positive electrode active material layer includes a positive electrode active material and a pore former. The positive electrode sheet can also be prepared by any embodiment of the first aspect of the present application.
[0100] In some embodiments, the pore-forming agent generates gas that is released due to decomposition during the formation of the battery monomer, and the content of the pore-forming agent in the positive electrode active material layer is relatively small, or even contains no pore-forming agent. The positive electrode sheet is derived from the battery monomer, and the positive electrode sheet soaked in the electrolyte in the battery monomer is taken out, and the obtained positive electrode sheet is dried at 120°C to obtain the required positive electrode sheet for detection.
[0101] The present application is applicable to the sodium salt system of polyanion materials, for example, the positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1.
[0102] In some embodiments, the pore former may include one or more of alkali metal and / or alkaline earth metal tetrahydroborate, alkali metal and / or alkaline earth metal sulfide, alkali metal and / or alkaline earth metal thiosulfate, alkali metal and / or alkaline earth metal sulfate, alkali metal and / or alkaline earth metal carbonate, alkali metal and / or alkaline earth metal citrate, alkali metal and / or alkaline earth metal glutamate, alkali metal and / or alkaline earth metal squarate.
[0103] The types, mass contents and particle sizes of the positive electrode active material and pore-forming agent are as described above and will not be repeated here.
[0104] The positive electrode sheet of the embodiment of the present application can be regarded as coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, pore-forming agent, optional conductive agent, optional binder and any other components in a solvent and stirring them evenly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto. The positive electrode sheet is not assembled into a battery cell, or assembled into a battery without undergoing a formation process.
[0105] Method for preparing battery cell
[0106] In a third aspect, the present application proposes a method for preparing a battery cell, the method comprising:
[0107] Step S100, providing a positive electrode active material and a pore-forming agent, and adding the positive electrode active material and the pore-forming agent into a solvent to mix them into a positive electrode slurry;
[0108] Step S200, coating the positive electrode slurry on at least one side of the positive electrode current collector, forming a positive electrode active material layer after drying, and preparing a positive electrode sheet;
[0109] Step S300, assembling the positive electrode plate, the separator and the negative electrode plate into a shell, injecting electrolyte into the shell, and during the chemical formation treatment, the pore former in the positive electrode active material layer is decomposed to provide a pore structure in the positive electrode active material layer.
[0110] According to the method implemented in the present application, by adding a pore-forming agent to the positive electrode slurry, the pore-forming agent will decompose and release gas during the formation process (the battery cell is charged for the first time). After the gas is discharged, a pore structure will be left in the positive electrode active material layer. The pore structure is conducive to retaining the electrolyte, thereby increasing the electrolyte retention capacity, thereby extending the cycle life of the battery cell.
[0111] The present application is applicable to the sodium salt system of polyanion materials, for example, the positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1.
[0112] In some embodiments, the pore former may include one or more of alkali metal and / or alkaline earth metal tetrahydroborate, alkali metal and / or alkaline earth metal sulfide, alkali metal and / or alkaline earth metal thiosulfate, alkali metal and / or alkaline earth metal sulfate, alkali metal and / or alkaline earth metal carbonate, alkali metal and / or alkaline earth metal citrate, alkali metal and / or alkaline earth metal glutamate, alkali metal and / or alkaline earth metal squarate.
[0113] The types, mass contents and particle sizes of the positive electrode active material and pore-forming agent are as described above and will not be repeated here.
[0114] Battery Cell
[0115] In a fourth aspect, the present application proposes a battery cell, which includes a positive electrode sheet. The positive electrode sheet of the embodiment of the present application can be a positive electrode sheet prepared as in any embodiment of the first aspect of the present application, or a positive electrode sheet of any embodiment of the second aspect of the present application; or the battery cell of the embodiment of the present application is prepared by any embodiment of the third aspect of the present application.
[0116] In the embodiment of the present application, before the battery cell is formed, the positive electrode active material layer of the positive electrode plate includes a positive electrode active material and a pore-forming agent; after the battery cell is formed, the pore-forming agent decomposes to form a gas that is released, thereby making the composition of the positive electrode active material layer of the battery cell different.
[0117] In some embodiments, the porosity of the positive electrode active material layer is 38% to 65%. Since the pore-forming agent decomposes into gas, a pore structure is formed in the positive electrode active material layer as the gas volatilizes, so that the porosity of the positive electrode active material layer meets the above range, which is conducive to increasing the liquid retention amount and can further improve the cycle performance.
[0118] Optionally, the porosity of the positive electrode active material layer is 40% to 65%, which can further improve the cycle performance.
[0119] Exemplarily, the porosity of the positive electrode active material layer can be 38%, 39%, 40%, 42%, 45%, 46%, 47%, 48%, 50%, 52%, 54%, 55%, 56%, 58%, 60%, 62%, 63%, 64%, 65% or a range consisting of any two of the above values.
[0120] In the embodiment of the present application, the porosity of the positive electrode active material layer is a well-known meaning in the art, and can be detected by using well-known equipment and methods in the art, for example, according to GB / T24586, using a gas displacement method for measurement. Porosity P = (V1-V2) / V1*100%, where V1 is the apparent volume of the sample, and V2 is the actual volume of the sample.
[0121] In some embodiments, after the pore former is decomposed, relatively little or even no pore former remains, so that the mass percentage of the positive electrode active material relative to the positive electrode active material layer is 80% to 98%. The mass percentage of the positive electrode active material is relatively high, which can effectively improve the energy density of the battery cell.
[0122] Optionally, the mass percentage of the positive electrode active material relative to the positive electrode active material layer is 85% to 95%.
[0123] Exemplarily, the mass percentage of the positive electrode active material relative to the positive electrode active material layer is 85%, 86%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, or a range consisting of any two of the above values.
[0124] In some embodiments, the surface density of the positive electrode active material layer is 0.2 g / 1540.25 cm 2 Up to 0.4g / 1540.25cm 2 .
[0125] When the surface density of the positive electrode active material layer is within the above range, the capacity density of the battery cell can be improved, and the battery cell can also have excellent active ion and electron transport performance, which can improve the power performance of the battery cell, reduce polarization and side reactions, and thus further improve the cycle performance of the battery cell.
[0126] Optionally, the surface density of the positive electrode active material layer can be 0.3 g / 1540.25 cm 2 Up to 0.38g / 1540.25cm 2 .
[0127] For example, the surface density of the positive electrode active material layer may be 0.2 g / 1540.25 cm 2 , 0.22g / 1540.25cm 2 , 0.23g / 1540.25cm 2 , 0.25g / 1540.25cm 2 , 0.26g / 1540.25cm 2 , 0.28g / 1540.25cm 2 , 0.30g / 1540.25cm 2 , 0.32g / 1540.25cm 2 , 0.34g / 1540.25cm 2 , 0.35g / 1540.25cm 2 , 0.36g / 1540.25cm 2 , 0.37g / 1540.25cm 2 , 0.38g / 1540.25cm 2 , 0.39g / 1540.25cm 2 , 0.4g / 1540.25cm 2 Or a range consisting of any two of the above values.
[0128] The surface density of the positive electrode active material layer in the embodiment of the present application is a well-known meaning in the art and can be tested by methods known in the art. For example, take a single-sided coated and cold-pressed positive electrode sheet (if it is a double-sided coated positive electrode sheet, the positive electrode active material layer on one side can be wiped off first), punch it into a small disc with an area of S1, weigh it, and record it as M1. Then wipe off the positive electrode active material layer of the above-weighed positive electrode sheet, weigh the weight of the positive electrode collector, and record it as M0. The surface density of the positive electrode active material layer = (the weight of the positive electrode sheet M1-the weight of the positive electrode collector M0) / S1.
[0129] In some embodiments, the positive electrode active material layer has a compaction density of 1.8 g / cc to 2.9 g / cc.
[0130] The compaction density of the positive electrode active material layer is within the above range, which can improve the energy density of the battery cell and further improve the power performance of the battery cell. In addition, the appropriate compaction density can further improve the cycle life of the battery cell.
[0131] Illustratively, the compaction density of the positive electrode active material layer can be 1.8 g / cc, 1.9 g / cc, 2.0 g / cc, 2.1 g / cc, 2.2 g / cc, 2.5 g / cc, 2.6 g / cc, 2.7 g / cc, 2.8 g / cc, 2.9 g / cc or a range consisting of any two of the above values.
[0132] The compaction density of the positive electrode active material layer in the embodiment of the present application is a well-known meaning in the art and can be tested by methods known in the art. For example, take a single-sided coated and cold-pressed positive electrode sheet (if it is a double-sided coated sheet, the positive electrode active material layer on one side can be wiped off first), test the thickness of the positive electrode active material layer, and then test the surface density of the positive electrode active material layer according to the above method. The compaction density of the positive electrode active material layer = the surface density of the positive electrode active material layer / the thickness of the positive electrode active material layer.
[0133] [Negative electrode]
[0134] The battery cell may also include a negative electrode tab.
[0135] In some embodiments, the negative electrode plate includes a negative electrode current collector. During charging, sodium ions gain electrons on the surface of the negative electrode current collector to generate a sodium metal layer.
[0136] Optionally, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil or copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0137] Furthermore, the negative electrode plate further comprises a conductive layer disposed on the negative electrode current collector, and the conductive layer comprises a negative electrode conductive agent. As an example, the negative electrode conductive agent may comprise at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0138] In other embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0139] The material of the negative electrode current collector is as described above and will not be repeated here.
[0140] The negative electrode active material may be a negative electrode active material for a battery cell known in the art. As an example, the negative electrode active material may include but is not limited to at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may include at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy material. The tin-based material may include at least one of elemental tin, tin oxide, and tin alloy material.
[0141] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. The embodiment of the present application has no particular restrictions on the type of the negative electrode conductive agent. As an example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. In some embodiments, based on the total weight of the negative electrode film layer, the mass percentage of the negative electrode conductive agent is ≤5wt%.
[0142] In some embodiments, the negative electrode film layer may also optionally include a negative electrode binder. The embodiment of the present application has no particular restrictions on the type of the negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS). In some embodiments, based on the total weight of the negative electrode film layer, the mass percentage of the negative electrode binder is ≤5wt%.
[0143] In some embodiments, the negative electrode film layer may further include other additives. As an example, other additives may include thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, etc. In some embodiments, based on the total weight of the negative electrode film layer, the mass percentage of the other additives is ≤2wt%.
[0144] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0145] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional conductive agent, optional binder, and other optional auxiliary agents in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.
[0146] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the embodiments of the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode collector and the negative electrode film layer and disposed on the surface of the negative electrode collector. In some other embodiments, the negative electrode plate described in the embodiments of the present application further includes a protective layer covering the surface of the negative electrode film layer.
[0147] [Electrolyte]
[0148] The battery cells also include an electrolyte.
[0149] During the charge and discharge process of the battery cell, active ions are embedded and released back and forth between the positive electrode and the negative electrode, and the electrolyte plays a role in conducting active ions between the positive electrode and the negative electrode. The embodiment of the present application has no particular limitation on the type of electrolyte, which can be selected according to actual needs.
[0150] The electrolyte solution includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not specifically limited and can be selected according to actual needs.
[0151] As an example, the electrolyte salt may include, but is not limited to, at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).
[0152] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0153] In some embodiments, the electrolyte may further include additives, for example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, additives that improve battery low temperature power performance, etc.
[0154] [Isolation film]
[0155] The battery cell also includes a separator.
[0156] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0157] In some embodiments, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0158] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly by a winding process and / or a lamination process.
[0159] In some embodiments, the battery cell may include an outer packaging, which may be used to package the electrode assembly and the electrolyte.
[0160] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS).
[0161] The shape of the battery cell of the present application can be cylindrical, square or any other shape; optionally, the shape of the battery cell of the present application is cylindrical, which is more conducive to improving the liquid retention capacity of the battery cell, such as Figure 1 The battery cell 5 is a cylindrical structure as an example.
[0162] In some embodiments, Figure 1 and Figure 2 As shown, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are enclosed to form a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive pole sheet, the negative pole sheet and the isolation film can form an electrode assembly 52 through a winding process and / or a lamination process. Optionally, the positive pole sheet, the negative pole sheet and the isolation film can form an electrode assembly 52 through a lamination process, and the electrode assembly 52 formed by this process is more conducive to improving the liquid retention capacity of the battery cell. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, which can be adjusted according to demand.
[0163] The preparation method of the battery cell of the present application is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, the separator and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the electrolyte is injected after drying, and the battery cell is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0164] In some embodiments of the present application, the battery cells according to the present application can be assembled into a battery module. The battery module can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery module.
[0165] Figure 3 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 3 As shown, in the battery module 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.
[0166] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.
[0167] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0168] Figure 4 and Figure 5 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 4 and Figure 5 As shown, the battery pack 1 may include a battery box and a battery module 4 disposed in the battery box, wherein the battery module 4 includes a plurality of battery cells. The battery box includes an upper box body 2 and a lower box body 3, wherein the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery module 4; further, the battery box may also include an intermediate box body, wherein the intermediate box body is located between the upper box body 2 and the lower box body 3, and the intermediate box body, the upper box body 2 and the lower box body 3 together form a closed space for accommodating the battery module 4. The battery module in the battery box may be set to one or more, and the plurality of battery modules 4 may be arranged in the battery box in any manner.
[0169] Electrical devices
[0170] In a fifth aspect, an embodiment of the present application provides an electric device, which includes at least one of the battery cells, battery modules or battery packs of the present application. The battery cells, battery modules or battery packs can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.
[0171] The electrical device may select a battery cell, a battery module or a battery pack according to its usage requirements.
[0172] Figure 6Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.
[0173] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a battery cell may be used as a power source.
[0174] Example
[0175] The following examples describe the disclosure of the present application in more detail, and these examples are only for illustrative purposes, as it is obvious to those skilled in the art that various modifications and variations can be made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further treatment, and the instruments used in the examples are commercially available.
[0176] Example 1 Preparation of sodium ion battery
[0177] 1. Preparation of positive electrode sheet
[0178] Aluminum foil with a thickness of 12 μm was used as the positive electrode current collector.
[0179] The positive electrode active material NaFePO4, the pore-forming agent sodium tetrahydroborate, the conductive agent carbon black, and the binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in a proper amount of solvent NMP at a weight ratio of 87:3:5:5 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0180] 2. Preparation of negative electrode sheet
[0181] A copper foil with a thickness of 8 μm was used as the negative electrode current collector.
[0182] 3. Isolation film
[0183] A porous polyethylene (PE) film is used as the isolation membrane.
[0184] 4. Preparation of electrolyte
[0185] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents ethylene carbonate EC and diethyl carbonate DMC are mixed in a volume ratio of 1:1 to obtain an electrolyte solvent, and then sodium hexafluorophosphate and the mixed solvent are mixed to prepare an electrolyte with a lithium salt concentration of 1 mol / L.
[0186] 5. Preparation of sodium ion batteries
[0187] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then the electrode assembly is obtained through a stacking process; the electrode assembly is placed in an outer packaging shell, and after drying, the electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0188] Comparative Example 1
[0189] A sodium ion battery was prepared by a method similar to that in Example 1. The difference from Example 1 was that no pore former was added to the positive electrode slurry of Comparative Example 1, and the weight ratio of the positive electrode active material NaFePO4, the conductive agent carbon black, and the binder polyvinylidene fluoride (PVDF) was 90:5:5.
[0190] Example 2
[0191] A sodium ion battery was prepared by a method similar to that of Example 1. The difference from Example 1 was that the content of the pore former was adjusted in Examples 2-1 and 2-3.
[0192] Example 3
[0193] A sodium ion battery was prepared by a method similar to that of Example 1. The difference from Example 1 was that the type of pore former was adjusted in Examples 3-1 and 3-2.
[0194] Example 4
[0195] A sodium ion battery was prepared by a method similar to that of Example 1. The difference from Example 1 was that the type of positive electrode active material was adjusted in Examples 4-1 and 4-2.
[0196] Example 5
[0197] A sodium ion battery was prepared by a method similar to that of Example 1. The difference from Example 1 was that parameters such as the volume average particle size of the pore former and the volume average particle size of the positive electrode active material were adjusted in Examples 5-1 to 5-4.
[0198] The data of the comparative examples and embodiments are shown in Table 1.
[0199] Test Section
[0200] 1. Test of element content in positive electrode
[0201] The carbon / metal / other non-metallic element contents were obtained by inductively coupled plasma emission spectroscopy (ICP) using Agilent ICP-OES730. The carbon / metal / other non-metallic elements were then calculated using the ICP results, and the mass percentage of each component was calculated accordingly.
[0202] 2. Cycle performance of sodium ion batteries
[0203] At 25°C, the secondary battery is charged to 3.85V at a constant current of 0.33C, then charged to a current of 0.05C at a constant voltage of 3.85V, and then discharged to 1.5V at a constant current of 1C. This is a charge and discharge cycle. Taking the capacity of the first discharge as 100%, calculate the capacity retention rate of the battery after 500 cycles. The capacity retention rate (%) of the battery after 500 cycles = the discharge capacity of the 500th cycle / the capacity of the first discharge × 100%.
[0204] Test Results
[0205] The test results are shown in Table 1.
[0206] Table 1
[0207]
[0208] As can be seen from Table 1, no porogen is added in Comparative Example 1, and the porosity of the positive electrode active material layer is relatively small, which is not conducive to the adsorption of electrolyte. Compared with Comparative Example 1, the embodiment of the present application sets a porogen in the positive electrode slurry. During the formation process of the battery cell, the porogen decomposes to generate gas. As the gas is released, the positive electrode active material layer generates a porous structure, so that the amount of electrolyte adsorbed by the positive electrode sheet increases, thereby increasing the content of electrolyte injected into the battery cell, increasing the injection amount, and thus extending the cycle life of the battery cell.
[0209] The embodiments of the present application can adjust the pore-forming effect by adjusting at least one of the type, content and particle size of the pore-forming agent; and the present application is applicable to a variety of polyanionic materials.
[0210] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application is described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A method for preparing a positive electrode sheet of a battery cell, comprising: Providing a positive electrode active material and a pore-forming agent, and adding the positive electrode active material and the pore-forming agent into a solvent to mix them into a positive electrode slurry; The positive electrode slurry is coated on at least one side of the positive electrode current collector, and after drying, a positive electrode active material layer is formed to prepare a positive electrode sheet, wherein the pore former is configured to decompose and generate gas during the battery monomer formation process.
2. The method according to claim 1, wherein: The pore-forming agent comprises one or more of alkali metal and / or alkaline earth metal tetrahydroborate, alkali metal and / or alkaline earth metal sulfide, alkali metal and / or alkaline earth metal thiosulfate, alkali metal and / or alkaline earth metal sulfate, alkali metal and / or alkaline earth metal carbonate, alkali metal and / or alkaline earth metal citrate, alkali metal and / or alkaline earth metal glutamate, alkali metal and / or alkaline earth metal squarate; Optionally, The alkali metal and / or alkaline earth metal tetrahydroborate includes one or more of sodium tetrahydroborate and potassium tetrahydroborate; The alkali metal and / or alkaline earth metal sulfide includes one or more of sodium sulfide, lithium disulfide, and potassium sulfide; The alkali metal and / or alkaline earth metal thiosulfate includes one or more of sodium thiosulfate and potassium thiosulfate; The alkali metal and / or alkaline earth metal sulfate includes one or more of sodium sulfate and potassium sulfate; The alkali metal and / or alkaline earth metal carbonate includes one or more of sodium carbonate and potassium carbonate; The alkali metal and / or alkaline earth metal citrate includes one or more of sodium citrate and lithium citrate; The alkali metal and / or alkaline earth metal glutamate includes one or more of sodium glutamate and potassium glutamate; The alkali metal and / or alkaline earth metal squarate includes one or more of potassium squarate, sodium squarate, and lithium squarate.
3. The method according to claim 1 or 2, wherein: The positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1.
4. The method according to any one of claims 1 to 3, wherein: Based on the total mass of the positive electrode slurry, the ratio of the mass percentage of the pore former to the mass percentage of the positive electrode active material is 1:(8 to 95); Optionally, The mass percentage of the pore-forming agent is 1% to 20%; and / or The mass percentage of the positive electrode active material is 80% to 95%.
5. The method according to any one of claims 1 to 4, wherein: The volume average particle size D of the pore former v50 The volume average particle size D of the positive electrode active material v50 The ratio is 1:(3 to 25); Optionally, The volume average particle size D of the pore former v50 0.2 μm to 2 μm; and / or The volume average particle size D of the positive electrode active material v50 3μm to 15μm.
6. A positive electrode sheet prepared by the method according to any one of claims 1 to 5.
7. A method for preparing a battery cell, comprising: Providing a positive electrode sheet as claimed in any one of claims 1 to 5; The positive electrode sheet, the separator and the negative electrode sheet are assembled into a shell, and an electrolyte is injected into the shell. During the chemical formation treatment, the pore former in the positive electrode active material layer is decomposed so that the positive electrode active material layer has a pore structure.
8. A battery cell, comprising a positive electrode sheet, wherein the positive electrode sheet comprises: Positive electrode current collector; A positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the porosity of the positive electrode active material layer is 38% to 65%; Available from 40% to 65%.
9. The battery cell according to claim 8, wherein: The positive electrode active material layer comprises a positive electrode active material, and the mass percentage of the positive electrode active material relative to the positive electrode active material layer is 80% to 98%, and can be 85% to 95%; and / or The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0≤x / m≤1.
10. The battery cell according to claim 8 or 9, wherein: The surface density of the positive electrode active material layer is 0.2 g / 1540.25 cm 2 Up to 0.4g / 1540.25cm 2 , optional: 0.3g / 1540.25cm 2 Up to 0.38g / 1540.25cm 2 ; and / or The compaction density of the positive electrode active material layer is 1.8 g / cc to 2.9 g / cc.
11. A battery comprising the battery cell according to any one of claims 8 to 10.
12. An electrical device comprising the battery as claimed in claim 11.
Citation Information
Patent Citations
Lithium ion battery silicon negative electrode plate and its preparation method and lithium ion battery
CN103811719A
Electrode pad for graphene-based supercapacitor and preparation method of electrode pad
CN105679548A
High-loading active substance electrode as well as preparation and application thereof
CN108134089A
Positive pole piece of lithium ion battery, and production method and application thereof
CN112151889A
Positive electrode active material, method for preparing same, and positive electrode and lithium battery using same
WO2012141503A2
Cited By
Biomass-based sodium-ion battery hard carbon material as well as preparation method and application thereof
CN120664526A
Biomass-based sodium-ion battery hard carbon materials, their preparation methods and applications
CN120664526B