Hard carbon composite material and preparation method thereof, negative plate and battery

By doping hard carbon composite materials with phosphorus and sodium elements, and adding amorphous carbon with fluorine or chlorine elements in the shell layer, the problems of large expansion and poor fast charging performance of hard carbon composite materials are solved, and the overall performance of the battery is improved. , including high temperature storage and rate performance.

CN118841537APending Publication Date: 2024-10-25HONEYCOMB ENERGY TECH (SHANGRAO) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410837360.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing hard carbon composite materials have problems such as large expansion and poor fast charging performance in sodium-ion batteries. Moreover, marketed hard carbon materials have low specific capacity and large specific surface area, resulting in low efficiency.

Method used

Using hard carbon composite materials, by doping phosphorus and sodium elements in the core layer, and adding amorphous carbon materials and fluorine or chlorine elements in the shell layer, the composite material with suitable layer spacing and Hard carbon composite material with improved grain size and specific surface area, reducing expansion and improving fast charging performance.

Benefits of technology

It achieves low expansion of hard carbon composite materials, excellent fast charging performance, and improves the high-temperature storage performance, cycle performance and rate performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841537A_ABST
    Figure CN118841537A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a hard carbon composite material, a preparation method thereof, a negative plate and a battery. The hard carbon composite material comprises a core layer and a shell layer coating the surface of the core layer, the core layer comprises a hard carbon material and doped phosphorus and sodium elements, and the shell layer comprises an amorphous carbon material and doped fluorine and / or chlorine elements. According to the hard carbon composite material, the hard carbon material doped with the phosphorus element and the sodium element serves as the core layer, the amorphous carbon doped with the fluoride element and / or the chlorine element serves as the shell layer, and through cooperation of the core layer and the shell layer, the obtained hard carbon composite material has the advantages of being appropriate in interlayer spacing, grain size and specific surface area, low in resistance, high in first efficiency and excellent in fast charging performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a hard carbon composite material and a preparation method thereof, a negative electrode sheet and a battery. Background Art

[0002] As the market's requirements for the energy density and fast charging performance of sodium-ion batteries increase, the negative electrode materials used in sodium-ion batteries are required to have high specific capacity and fast charging performance. At present, the commercial hard carbon materials are mainly biomass materials, which have low specific capacity and high specific surface area, resulting in low initial efficiency. In addition, the hard carbon itself relies on its pore sodium storage to reduce the long insertion and extraction path of sodium ions during its charge and discharge process, reducing its fast charging performance. At present, measures to improve the fast charging and energy density of hard carbon mainly include doping with metals or non-metallic compounds with high specific capacity. The phosphorus materials in the prior art form sodium phosphide in sodium-ion batteries to give them high specific capacity, but they have defects such as large expansion and poor fast charging performance.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] One object of the present invention is to provide a hard carbon composite material to solve the defects of the hard carbon composite materials in the prior art, that is, large expansion and poor fast charging performance. The hard carbon composite material of the present invention can reduce expansion and improve fast charging performance.

[0005] Another object of the present invention is to provide a method for preparing the hard carbon composite material. Through the coordination of various steps, the hard carbon composite material obtained can reduce expansion, improve fast charging performance, and improve the high temperature storage performance, cycle performance and rate performance of the battery.

[0006] Another object of the present invention is to provide a negative electrode sheet.

[0007] Another object of the present invention is to provide a battery as described above.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A hard carbon composite material comprises a core layer and a shell layer coated on the surface of the core layer, the core layer comprises a hard carbon material and doped phosphorus and sodium elements, and the shell layer comprises an amorphous carbon material and doped fluorine and / or chlorine elements.

[0010] In some embodiments, the mass of the shell layer accounts for 1% to 5% of the mass of the hard carbon composite material.

[0011] In some embodiments, the core layer includes, by mass percentage, 1% to 10% phosphorus, 1% to 5% sodium, and 85% to 98% hard carbon material.

[0012] In some embodiments, the interlayer spacing of the hard carbon composite material is 0.38-0.41 nm.

[0013] In some embodiments, the hard carbon composite material has a grain size of 1.85 to 1.98 nm.

[0014] In some embodiments, the hard carbon composite material has a resistance of 0.64 to 0.9 Ω·cm.

[0015] In some embodiments, the specific surface area of ​​the hard carbon composite material is 4.2 to 5 m 2 / g.

[0016] The method for preparing the hard carbon composite material as described above comprises the following steps:

[0017] A mixture of a carbon source, a phosphorus compound, an inorganic template and an alkaline solution is heat-treated to obtain a first system, wherein the carbon source includes a phenolic compound and an aldehyde compound; the first system is subjected to solid-liquid separation, and the solid is collected and carbonized and activated to obtain phosphorus-doped porous hard carbon; the phosphorus-doped porous hard carbon is treated with sodium vapor to deposit sodium elements to obtain a core layer material; and the core layer material is then treated with a halocarbon gas to deposit halocarbon to obtain a hard carbon composite material.

[0018] In some embodiments, the phenolic compound includes at least one of phenol, cresol, xylenol and m-cresol.

[0019] In some embodiments, the aldehyde compound includes at least one of formaldehyde, acetaldehyde, furfural, butyraldehyde, valeraldehyde and methacrolein.

[0020] In some embodiments, the phosphorus compound includes at least one of triphenyl phosphate, triphenylphosphine, anilide, trimethylolphosphonic acid, benfotiamine, isopropylphenol phosphate, and phenyldichlorophosphate.

[0021] In some embodiments, the inorganic template includes at least one of zinc chloride, zinc oxide, and silicon dioxide.

[0022] In some embodiments, the mass ratio of the carbon source, the phosphorus compound, the inorganic template and the alkaline solution is 100:(1-5):(1-5):(100-500), wherein the mass content of the alkali in the alkaline solution is 15%-22%.

[0023] In some embodiments, the molar ratio of the phenolic compound to the aldehyde compound is 1:(1-1.2).

[0024] In some embodiments, the heat treatment temperature is 45 to 60° C., and the heat treatment time is 10 to 15 hours.

[0025] In some embodiments, the temperature of the carbonization treatment is 300 to 500° C., and the time of the carbonization treatment is 1 to 6 hours.

[0026] In some embodiments, the temperature of the activation treatment is 1000-1200° C., and the time of the activation treatment is 1-6 hours.

[0027] In some embodiments, the phosphorus-doped porous hard carbon is deposited in a sealed container to deposit the sodium element. Before depositing the sodium element, the temperature in the sealed container is controlled to be 900-1100° C. and the pressure is controlled to be 0.1-0.5 MPa.

[0028] In some implementations, the flow rate of the sodium vapor is 50 to 200 mL / min, and the treatment time of the sodium vapor is 30 to 300 min.

[0029] In some embodiments, the halocarbon gas includes at least one of carbon trifluoride, carbon difluoride, and carbon tetrachloride.

[0030] In some implementations, the flow rate of the halocarbon gas is 100 to 500 mL / min, and the treatment time of the halocarbon gas is 30 to 300 min.

[0031] A negative electrode sheet comprises the hard carbon composite material, or the hard carbon composite material prepared by the preparation method of the hard carbon composite material.

[0032] A battery comprises the negative electrode sheet.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The hard carbon composite material of the present invention uses a hard carbon material doped with phosphorus and sodium as a core layer and an amorphous carbon doped with fluoride as a shell layer. Through the coordination of the core layer and the shell layer, the obtained hard carbon composite material has a suitable interlayer spacing, grain size and specific surface area, low resistance, high initial efficiency and excellent fast charging performance.

[0035] (2) The present invention obtains phosphorus-doped porous hard carbon by subjecting a mixture of a carbon source, a phosphorus compound, an inorganic template and an alkaline solution to heat treatment, carbonization treatment and activation treatment, wherein the phosphorus compound improves the specific capacity of the material, and the pores formed by the inorganic template can reduce the full-charge expansion of phosphorus, thereby reducing the expansion while improving the specific capacity of the hard carbon; further, sodium vapor is deposited in the phosphorus-doped porous hard carbon by gasification to reduce the defects of the material pores, and metallic sodium is converted into sodium ions during the charge and discharge process, thereby reducing the sodium ions consumed in forming the SEI film, improving the initial efficiency, and relying on sufficient sodium ions to improve the fast charging performance of the material, and the use of metallic sodium vaporization deposition on the phosphorus-doped porous hard carbon has the advantages of uniform deposition and controllable process; further, halocarbon gas is deposited to form a shell layer, which cooperates with the core layer to further improve the initial efficiency and fast charging performance of the hard carbon composite material.

[0036] (3) The battery of the present invention has excellent high temperature storage performance, cycle performance and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 This is a scanning electron microscope image of the hard carbon composite material in Example 1 of the present invention. DETAILED DESCRIPTION

[0039] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0040] According to one aspect of the present invention, the present invention relates to a hard carbon composite material, which includes a core layer and a shell layer coated on the surface of the core layer, the core layer includes a hard carbon material and doped phosphorus and sodium elements, and the shell layer includes an amorphous carbon material and doped fluorine and / or chlorine elements.

[0041] The hard carbon composite material of the present invention uses a hard carbon material doped with phosphorus and sodium elements as a core layer and an amorphous carbon doped with fluoride as a shell layer. Through the coordination of the core layer and the shell layer, the obtained hard carbon composite material has suitable interlayer spacing, grain size and specific surface area, low resistance, high initial efficiency and excellent fast charging performance.

[0042] In some embodiments, the mass of the shell layer accounts for 1% to 5% of the mass of the hard carbon composite material, including but not limited to 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc., or any range between the two. In some embodiments, the core layer includes, by mass percentage: 1% to 10% phosphorus, 1% to 5% sodium, and 85% to 98% hard carbon material. In some embodiments, phosphorus includes but is not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., or any range between the two; sodium includes but is not limited to 1%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., or any range between the two; hard carbon materials include but are not limited to 85%, 86%, 88%, 90%, 91%, 92%, 93%, 95%, 96% or 98%, etc., or any range between the two. The hard carbon composite material of the present invention is more conducive to improving the initial efficiency and improving the fast charging performance through the combination of the above-mentioned components in appropriate proportions.

[0043] In some embodiments, the interlayer spacing of the hard carbon composite material is 0.38-0.41 nm, including but not limited to 0.38 nm, 0.385 nm, 0.39 nm, 0.398 nm, 0.4 nm, 0.405 nm, 0.41 nm, etc., or any range between the two. In some embodiments, the grain size of the hard carbon composite material is 1.85-1.98 nm, such as 1.85 nm, 1.88 nm, 1.90 nm, 1.91 nm, 1.92 nm, 1.94 nm, 1.95 nm, 1.98 nm, etc., or any range between the two. In some embodiments, the hard carbon composite material has a resistance of 0.64 to 0.9 Ω·cm, such as 0.64 Ω·cm, 0.65 Ω·cm, 0.68 Ω·cm, 0.7 Ω·cm, 0.75 Ω·cm, 0.8 Ω·cm, 0.85 Ω·cm or 0.9 Ω·cm, or any range between two values. In some embodiments, the hard carbon composite material has a specific surface area of ​​4.2 to 5 m 2 / g, for example 4.2m 2 / g, 4.3m 2 / g, 4.5m 2 / g, 4.8m 2 / g5,m 2 / g, etc., or any range between the two. The hard carbon composite material of the present invention has suitable interlayer spacing, grain size, specific surface area, low resistance and excellent electrical properties.

[0044] According to another aspect of the present invention, the present invention also relates to a method for preparing the hard carbon composite material as described above, comprising the following steps:

[0045] A mixture of a carbon source, a phosphorus compound, an inorganic template and an alkaline solution is heat-treated to obtain a first system, wherein the carbon source includes a phenolic compound and an aldehyde compound; the first system is subjected to solid-liquid separation, and the solid is collected and carbonized and activated to obtain phosphorus-doped porous hard carbon; the phosphorus-doped porous hard carbon is treated with sodium vapor to deposit sodium elements to obtain a core layer material; and the core layer material is then treated with a halocarbon gas to deposit halocarbon to obtain a hard carbon composite material.

[0046] The present invention obtains phosphorus-doped porous hard carbon by heat-treating, carbonizing and activating a mixture of a carbon source, a phosphorus compound, an inorganic template and an alkaline solution, and improves the specific capacity of the material by adding a phosphorus compound, and uses an inorganic template to form pores to reduce the full-charge expansion of phosphorus, so that the expansion is reduced while improving the specific capacity of the hard carbon. Sodium vapor is further deposited in the phosphorus-doped porous hard carbon by gasification to reduce the defects of the material pores, and metallic sodium is converted into sodium ions during the charge and discharge process to reduce the sodium ions consumed in forming the SEI film, improve the first efficiency, and rely on sufficient sodium ions to improve the fast charging performance of the material, and the use of metallic sodium gasification deposition on the phosphorus-doped porous hard carbon has the advantages of uniform deposition and controllable process. A halogenated carbon coating layer is further deposited, and the cooperation with the core layer further improves the first efficiency and fast charging performance of the hard carbon composite material.

[0047] In some embodiments, the phenolic compound includes at least one of phenol, cresol, xylenol and meta-methylphenol, and the phenolic compound includes any one of the above, or a combination of several, such as a combination of phenol and cresol, a combination of xylenol and meta-methylphenol, etc. In some embodiments, the aldehyde compound includes at least one of formaldehyde, acetaldehyde, furfural, butyraldehyde, valeraldehyde and methacrolein, and the aldehyde compound can be one of the above, or a combination of multiple, such as a combination of formaldehyde and acetaldehyde, a combination of acetaldehyde, furfural and butyraldehyde, etc. In some embodiments, the molar ratio of the phenolic compound to the aldehyde compound is 1: (1 to 1.2), such as 1: 1, 1: 1.1 or 1: 1.2, etc. The carbon source of the present invention adopts a suitable amount of phenolic compounds and aldehyde compounds to cooperate, which is more conducive to obtaining high-performance porous carbon hard carbon materials, and is conducive to further doping with phosphorus and sodium elements to improve the electrochemical properties of hard carbon composite materials.

[0048] In some embodiments, the phosphorus compound includes at least one of triphenyl phosphate, triphenyl phosphine, aniline phosphine, trimethyl phosphine, benfotiamine, isopropyl phenol phosphate and phenyl dichlorophosphate. The phosphorus compound of the present invention can be any one of the above, or a combination of several, such as a combination of triphenyl phosphate and triphenyl phosphine, a combination of aniline phosphine and trimethyl phosphine, a combination of triphenyl phosphine, isopropyl phenol phosphate and phenyl dichlorophosphate, etc.

[0049] In some embodiments, the inorganic template includes at least one of zinc chloride, zinc oxide and silicon dioxide. The present invention uses the above inorganic template to form pores, which can reduce the full charge expansion of phosphorus, thereby improving the hard carbon specific capacity and reducing expansion.

[0050] In some embodiments, the mass ratio of the carbon source, the phosphorus compound, the inorganic template and the alkaline solution is 100:(1-5):(1-5):(100-500), such as 100:1:1:100, 100:2:2:130, 100:3:3:300, 100:5:5:500, etc., wherein the mass content of the alkali in the alkaline solution is 15% to 22%, such as 15%, 16%, 17%, 18%, 19%, 20% or 22%, etc., or any range value between the two, and the alkaline solution includes sodium hydroxide solution. The present invention adopts a suitable amount ratio of carbon source, phosphorus compound, inorganic template and alkaline solution, which is more conducive to obtaining phosphorus-doped porous carbon with excellent physical and chemical properties, so as to facilitate subsequent sodium deposition and halocarbon coating.

[0051] In some embodiments, the heat treatment temperature is 45 to 60°C, including but not limited to 45°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C, etc., or any range between the two. The heat treatment time is 10 to 15h, such as 10h, 11h, 12h, 13h, 14h or 15h, etc., or any range between the two. The present invention adopts a suitable heat treatment temperature to make the phenolic compound and the aldehyde compound react better.

[0052] In some embodiments, the temperature of the carbonization treatment is 300-500°C, such as 300°C, 320°C, 350°C, 370°C, 400°C, 420°C, 450°C, 480°C, 500°C, etc., or any range between the two. The time of the carbonization treatment is 1-6h, such as 1h, 2h, 3h, 4h, 5h, 6h, etc., or any range between the two. The present invention ensures the effect of carbonization by suitable carbonization treatment conditions.

[0053] In some embodiments, the temperature of the activation treatment is 1000-1200°C, such as 1000°C, 1020°C, 1050°C, 1080°C, 1100°C, 1120°C, 1150°C, 1180°C, 1200°C, etc., or any range between the two. The time of the activation treatment is 1-6h, such as 1h, 2h, 3h, 4h, 5h, 6h, etc., or any range between the two. The present invention uses suitable activation treatment conditions to make the phosphorus-doped porous hard carbon have excellent activity, and can further ensure the subsequent sodium deposition effect and the coating effect of the halogenated carbon.

[0054] In some embodiments, the phosphorus-doped porous hard carbon is deposited in a sealed container to deposit the sodium element. Before depositing the sodium element, the temperature in the sealed container is controlled to be 900-1100°C, such as 900°C, 920°C, 950°C, 980°C, 1000°C, 1020°C, 1050°C, 1080°C, 1100°C, etc., or any range between the two. The pressure in the sealed container is controlled to be 0.1-0.5Mpa, such as 0.1Mpa, 0.2Mpa, 0.3Mpa, 0.4Mpa, 0.5Mpa, etc., or any range between the two. The present invention controls the temperature and pressure in the sealed container, which is more conducive to the deposition of the sodium element and the subsequent deposition of the halocarbon gas, and is more conducive to improving the comprehensive electrical properties of the hard carbon composite material.

[0055] In some implementation modes, the flow rate of the sodium vapor is 50-200 mL / min, such as 50 mL / min, 80 mL / min, 100 mL / min, 120 mL / min, 150 mL / min or 200 mL / min, or any range between the two. The treatment time of the sodium vapor is 30-300 min, such as 30 min, 50 min, 100 min, 150 min, 200 min, 250 min, 300 min, or any range between the two. The sodium vapor of the present invention adopts suitable flow rate and treatment time, so as to ensure the deposition effect of the sodium element.

[0056] In some embodiments, the halogenated carbon gas includes at least one of carbon trifluoride, carbon difluoride and carbon tetrachloride, such as a combination of carbon trifluoride and carbon difluoride, a combination of carbon difluoride and carbon tetrachloride, and a combination of carbon trifluoride and carbon tetrachloride.

[0057] In some embodiments, the flow rate of the halocarbon gas is 100 to 500 mL / min, for example, 50 mL / min, 80 mL / min, 100 mL / min, 120 mL / min, 150 mL / min, 200 mL / min, 300 mL / min, 400 mL / min, 500 mL / min, etc., or any range between the two. The treatment time of the halocarbon gas is 30 to 300 min, for example, 30 min, 50 min, 60 min, 70 min, 90 min, 100 min, 150 min, 200 min, 300 min, etc., or any range between the two. The halocarbon gas of the present invention adopts a suitable flow rate and treatment time to ensure the coating effect of the halocarbon layer, so as to improve the initial effect and fast charging performance of the hard carbon composite material finally obtained.

[0058] According to another aspect of the present invention, the present invention also relates to a negative electrode sheet, comprising the hard carbon composite material, or a hard carbon composite material prepared by the preparation method of the hard carbon composite material.

[0059] The negative electrode sheet of the present invention comprises a negative electrode current collector and a negative electrode material layer arranged on at least one side surface of the negative electrode current collector, and the negative electrode material layer comprises the above-mentioned hard carbon composite material.

[0060] According to another aspect of the present invention, the present invention also relates to a battery, comprising the negative electrode sheet.

[0061] The battery of the present invention comprises the above-mentioned negative electrode sheet, positive electrode sheet, separator and electrolyte.

[0062] The battery of the present invention has excellent capacity, initial efficiency, high temperature storage performance, cycle performance and rate performance.

[0063] The following is further explained with reference to specific embodiments and comparative examples.

[0064] Example 1

[0065] A method for preparing a hard carbon composite material comprises the following steps:

[0066] (1) 74 g of phenol, 26 g of formaldehyde, 3 g of triphenyl phosphate, and 3 g of zinc chloride were added to 300 g of a 20 wt% sodium hydroxide alkaline solution, and the mixture was reacted at 50 °C for 12 h via a phenol-formaldehyde reaction. The residue was filtered and pre-carbonized at 400 °C for 3 h. The residue was then heated to 1100 °C and activated with water vapor for 3 h to obtain phosphorus-doped porous hard carbon.

[0067] (2) The phosphorus-doped porous hard carbon was transferred to a closed pressure reactor, the temperature was raised to 1000°C and the pressure was 0.3 MPa, sodium vapor was introduced at a flow rate of 100 mL / min for 120 min, and then carbon trifluoride gas was introduced at a pressure of 0.3 MPa and a flow rate of 300 mL / min for 120 min to obtain a hard carbon composite material.

[0068] Example 2

[0069] A method for preparing a composite material comprises the following steps:

[0070] (1) 71 g of cresol, 29 g of acetaldehyde, 1 g of triphenylphosphine and 1 g of zinc oxide were added to 100 g of 20 wt% sodium hydroxide alkaline solution, reacted at 50 °C for 12 h through a phenol-formaldehyde reaction, filtered, and the resulting filter residue was pre-carbonized at 300 °C for 6 h, then heated to 1000 °C and activated with water vapor for 6 h to obtain phosphorus-doped porous hard carbon.

[0071] (2) The phosphorus-doped porous hard carbon was transferred to a closed pressure reactor, the temperature was raised to 900°C and the pressure was 0.1 MPa, sodium vapor was introduced at a flow rate of 50 mL / min for 300 min, and then carbon difluoride gas was introduced at a pressure of 0.1 MPa and a flow rate of 100 mL / min for 300 min to obtain a hard carbon composite material.

[0072] Example 3

[0073] A method for preparing a composite material comprises the following steps:

[0074] (1) Add 51 g of dibenzoyl phenol, 49 g of furfural, 5 g of aniline phosphine and 5 g of silicon dioxide to 500 g of 20 wt% sodium hydroxide alkaline solution, react at 50 °C for 12 h through a phenol-formaldehyde reaction, filter, and pre-carbonize the filter residue at 500 °C for 1 h. Then, heat it to 1200 °C and activate it with water vapor for 1 h to obtain phosphorus-doped porous hard carbon.

[0075] (2) The phosphorus-doped porous hard carbon was transferred to a closed pressure reactor, the temperature was raised to 1100°C and the pressure was 0.5 MPa, sodium vapor was introduced at a flow rate of 200 mL / min for 30 min, and then carbon tetrachloride gas was introduced at a pressure of 0.5 MPa and a flow rate of 500 mL / min for 30 min to obtain a hard carbon composite material.

[0076] Example 4

[0077] A method for preparing a hard carbon composite material comprises the following steps:

[0078] (1) Add 51 g of dihydroxyphenol, 49 g of furfural, 2 g of aniline phosphate, 3 g of isopropylphenol phosphate, 2.5 g of silicon dioxide and 2.5 g of zinc oxide to 500 g of 15 wt% sodium hydroxide alkaline solution, react at 60 ° C for 1 hour through phenol-formaldehyde reaction, filter, and pre-carbonize the filter residue at 500 ° C for 1 hour, then raise the temperature to 1050 ° C and activate it with water vapor for 1.5 hours to obtain phosphorus-doped porous hard carbon.

[0079] (2) The phosphorus-doped porous hard carbon was transferred to a closed pressure reactor, the temperature was raised to 1070°C and the pressure was 0.4 MPa, sodium vapor was introduced at a flow rate of 150 mL / min for 45 min, and then carbon tetrachloride gas and carbon trifluoride gas were introduced at a pressure of 0.4 MPa and a flow rate of 220 mL / min for 30 min to obtain a hard carbon composite material.

[0080] Example 5

[0081] A method for preparing a hard carbon composite material comprises the following steps:

[0082] (1) Add 51 g of dibenzoyl phenol, 49 g of furfural, 2 g of triphenyl phosphate, 3 g of isopropyl phenol phosphate, 2 g of zinc chloride, and 3 g of silicon dioxide to 500 g of a 20 wt% sodium hydroxide alkaline solution, react at 50 °C for 12 h through a phenol-formaldehyde reaction, filter, and pre-carbonize the resulting filter residue at 500 °C for 1 h, then heat to 1200 °C and activate with water vapor for 1 h to obtain phosphorus-doped porous hard carbon.

[0083] (2) The phosphorus-doped porous hard carbon was transferred to a closed pressure reactor, the temperature was raised to 1100°C and the pressure was 0.5 MPa, sodium vapor was introduced at a flow rate of 200 mL / min for 30 min, and then carbon trifluoride gas and carbon tetrachloride gas were introduced at a pressure of 0.5 MPa and a flow rate of 250 mL / min for 30 min to obtain a hard carbon composite material.

[0084] Comparative Example 1

[0085] A method for preparing a composite material, which is different from Example 1 in that triphenyl phosphate and zinc chloride are not added in step (1), and the rest is the same as Example 1.

[0086] Comparative Example 2

[0087] A method for preparing a composite material, which is different from Example 1 in that sodium vapor is not introduced in step (2), and the rest is the same as Example 1.

[0088] Experimental example

[0089] 1. Scanning electron microscope image

[0090] The hard carbon composite material prepared in Example 1 was tested by scanning electron microscope (SEM). The test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the hard carbon composite material has a granular structure with uniform size and a particle size of 1 to 5 μm.

[0091] 2. Physical and chemical properties test of hard carbon composite materials

[0092] With reference to the test method in GB / T-43114-2023 "Hard Carbon", the specific surface area of ​​the hard carbon composite materials prepared in each embodiment and comparative example was tested, and the interlayer spacing and grain size La of the material were tested by XRD; and the powder resistance was tested by a four-probe tester.

[0093] The physical and chemical properties test results of the hard carbon composite material are shown in Table 1.

[0094] Table 1 Physical and chemical properties test results of hard carbon composite materials

[0095] Group La(nm) Powder resistance (Ω·cm) <![CDATA[Specific surface area (m 2 / g)]]> Interlayer spacing (nm) Example 1 1.86 0.78 4.53 0.384 Example 2 1.78 0.65 4.69 0.389 Example 3 1.95 0.89 4.23 0.380 Example 4 1.93 0.87 4.25 0.381 Example 5 1.92 0.86 4.28 0.382 Comparative Example 1 2.08 1.01 3.12 0.365 Comparative Example 2 2.16 1.23 3.89 0.378

[0096] As can be seen from Table 1, the hard carbon composite material of the present invention has suitable interlayer spacing, grain size and specific surface area, and low powder resistance, which is beneficial to increasing the insertion and extraction rate of sodium ions during the charge and discharge process and improving the rate performance.

[0097] 3. Performance test of button battery

[0098] The hard carbon composite materials in each embodiment and comparative example were used as negative electrode materials and assembled into button batteries according to the following steps:

[0099] Add binder, conductive agent and solvent to the negative electrode material, stir to make slurry, apply it on copper foil, dry and roll to get negative electrode sheet. The binder used is LA132 binder, the conductive agent is SP, the solvent is double distilled water, the amount ratio of negative electrode material, SP, LA132, double distilled water is 94g:2g:4g:220mL; the electrolyte includes: electrolyte (NaPF6) and solvent (EC and DEC), the volume ratio of EC and DEC is 1:1, and the concentration of NaPF6 is 1.1mol / L. The metal sodium sheet is used as the counter electrode, and the diaphragm is a polyethylene propylene (PEP) composite membrane.

[0100] The battery was assembled in an argon-filled glove box, and the electrochemical performance was tested on a Wuhan Blue Power CT2001A battery tester, with a charge and discharge voltage range of 0.00V-2.00V and a charge and discharge rate of 0.1C. The charging DCR (50% SOC) and cycle performance (0.2C / 0.2C, 100 times) of the button battery were also tested.

[0101] The test results of button cells are shown in Table 2.

[0102] Table 2 Test results of button batteries

[0103]

[0104] It can be seen from Table 2 that the hard carbon composite materials obtained in each embodiment of the present invention have excellent first discharge specific capacity, first efficiency and rate performance. The reasons include: the doped phosphorus in the present invention can improve the specific capacity of the material, and the sodium doping can reduce the loss of sodium ions during the charge and discharge process and improve the first efficiency. At the same time, the inorganic template can reduce the full charge expansion of phosphorus by pore formation and improve the cycle performance; in addition, the surface coating of an appropriate amount of halogenated carbon is further beneficial to improve the capacity, first efficiency and rate performance of the hard carbon composite material.

[0105] 4. Soft pack battery test

[0106] The hard carbon composite materials in each embodiment and comparative example are used as negative electrode materials, and the negative electrode sheets are prepared by slurry mixing and coating. 1 / 3 Mn 1 / 3 Ni 1 / 3 O2) as the positive electrode, NaPF6 (solvent is EC+DEC, volume ratio is 1:1, concentration is 1.3mol / L) as the electrolyte, and celegard2400 as the separator to prepare a 5Ah soft pack battery. The soft pack battery was tested for high temperature storage performance, cycle performance and rate performance, as follows:

[0107] High temperature storage performance test: The capacity of the battery in a fully charged state is tested at 60°C and is found to be X1. After being placed at 60°C for 30 days, the capacity of the battery is tested again and is found to be X2. The charge retention is calculated to be X2 / X1*100%. The battery is then fully charged to a fully charged state (100% SOC), the capacity of the battery is tested to be X3, and the recovery capacity is calculated to be X3 / X1*100%.

[0108] Cycle performance test conditions: temperature 25°C, 1C / 1C, voltage range 2.0-3.95V, 500 cycles.

[0109] Rate performance test conditions: 100% SOC (3.95V, 2C rate + 0.1C rate) charged at a rate of 2C in constant current and constant voltage mode, and then calculated as constant current ratio = constant current capacity / (constant current capacity + constant voltage capacity).

[0110] The electrical performance test results of the soft pack battery are shown in Table 3.

[0111] Table 3 Electrical performance test results of soft pack batteries

[0112] Group Charge retention rate Capacity recovery Cycle performance Constant current ratio Example 1 95.5% 97.2% 94.1% 97.2% Example 2 95.1% 96.9% 94.0% 97.6% Example 3 96.3% 97.6% 94.8% 96.5% Example 4 96.1% 97.5% 94.5% 96.8% Example 5 95.8% 97.3% 94.3% 97.0% Comparative Example 1 92.8% 93.9% 91.4% 93.2% Comparative Example 2 91.7% 92.4% 90.9% 92.1%

[0113] It can be seen from Table 3 that the high-temperature storage performance, cycle performance and rate performance (constant current ratio) of the batteries obtained from the hard carbon composite materials of each embodiment of the present invention are significantly better than those of the comparative examples. The reasons include: the core layer of the hard carbon material in the embodiment of the present invention is doped with elemental phosphorus and elemental sodium, which can increase the specific capacity of the material, reduce the sodium ions consumed in forming the SEI film during charging and discharging, and improve the storage and cycle performance; the shell layer is amorphous carbon doped with fluorine and / or chlorine, which is beneficial to further improve the capacity and fast charging performance of the composite material; the composite material has low powder resistivity and high interlayer spacing, which can increase the insertion and extraction rate of sodium ions during charging and discharging, and improve the rate performance.

[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A hard carbon composite material, It is characterized in that The hard carbon composite material comprises a core layer and a shell layer coated on the surface of the core layer, the core layer comprises a hard carbon material and doped phosphorus and sodium elements, and the shell layer comprises an amorphous carbon material and doped fluorine and / or chlorine elements.

2. The hard carbon composite material according to claim 1, It is characterized in that The mass of the shell layer accounts for 1% to 5% of the mass of the hard carbon composite material; Measured in percentage by mass, the core layer comprises: 1% to 10% phosphorus element, 1% to 5% sodium element and 85% to 98% hard carbon material.

3. The hard carbon composite material according to claim 1, It is characterized in that Contains at least one of the following features (1) to (4): (1) The interlayer spacing of the hard carbon composite material is 0.38 to 0.41 nm; (2) The grain size of the hard carbon composite material is 1.85 to 1.98 nm; (3) The electrical resistance of the hard carbon composite material is 0.64 to 0.9 Ω·cm; (4) The specific surface area of ​​the hard carbon composite material is 4.2 to 5 m 2 / g.

4. The method for preparing the hard carbon composite material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Heat-treating a mixture of a carbon source, a phosphorus compound, an inorganic template and an alkaline solution to obtain a first system, wherein the carbon source includes a phenolic compound and an aldehyde compound; performing solid-liquid separation on the first system, collecting solids and performing carbonization treatment and activation treatment to obtain phosphorus-doped porous hard carbon; The phosphorus-doped porous hard carbon is treated with sodium vapor to deposit sodium elements to obtain a core layer material; and the core layer material is treated with a halocarbon gas to deposit halocarbon to obtain a hard carbon composite material.

5. The method for preparing the hard carbon composite material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (6): (1) The phenolic compound comprises at least one of phenol, cresol, xylenol and m-cresol; (2) the aldehyde compound comprises at least one of formaldehyde, acetaldehyde, furfural, butyraldehyde, valeraldehyde and methacrolein; (3) the phosphorus compound comprises at least one of triphenyl phosphate, triphenyl phosphine, anilide phosphine, trimethylolphosphonic acid, benfotiamine, isopropylphenol phosphate and phenyl dichlorophosphate; (4) The inorganic template comprises at least one of zinc chloride, zinc oxide and silicon dioxide; (5) The mass ratio of the carbon source, the phosphorus compound, the inorganic template and the alkaline solution is 100:(1-5):(1-5):(100-500), wherein the mass content of the alkali in the alkaline solution is 15%-22%; (6) The molar ratio of the phenolic compound to the aldehyde compound is 1:(1-1.2).

6. The method for preparing the hard carbon composite material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (3): (1) The temperature of the heat treatment is 45 to 60° C., and the time of the heat treatment is 10 to 15 hours; (2) The temperature of the carbonization treatment is 300 to 500° C., and the time of the carbonization treatment is 1 to 6 hours; (3) The temperature of the activation treatment is 1000-1200°C, and the time of the activation treatment is 1-6 hours.

7. The method for preparing the hard carbon composite material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (2): (1) The phosphorus-doped porous hard carbon is deposited with the sodium element in a sealed container. Before depositing the sodium element, the temperature in the sealed container is controlled to be 900-1100° C. and the pressure is controlled to be 0.1-0.5 MPa; (2) The flow rate of the sodium vapor is 50 to 200 mL / min, and the treatment time of the sodium vapor is 30 to 300 min.

8. The method for preparing the hard carbon composite material according to claim 4, It is characterized in that Contains at least one of the following features (1) to (2): (1) The halogenated carbon gas comprises at least one of carbon trifluoride, carbon difluoride and carbon tetrachloride; (2) The flow rate of the halocarbon gas is 100 to 500 mL / min, and the treatment time of the halocarbon gas is 30 to 300 min.

9. A negative electrode sheet, It is characterized in that The invention comprises the hard carbon composite material according to any one of claims 1 to 3, or a hard carbon composite material prepared by the preparation method of the hard carbon composite material according to any one of claims 4 to 8.

10. A battery, It is characterized in that Includes the negative electrode sheet as described in claim 9.