Preparation method of carbon-coated silicon-carbon negative electrode material based on graphene modification

Through the double coating process of graphene and nano-hard carbon, a birdcage structure is established to block the insertion of ions into the silicon lattice, solving the problems of high volume expansion rate and poor conductivity of silicon-based negative electrode materials, and achieving high energy density and safety. The performance improvement simplifies the process and reduces the cost, making it suitable for industrial production.

CN118841549APending Publication Date: 2024-10-25CHENGDU DAAISBEICENE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928223.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing silicon-based anode materials have poor cycle stability due to their high volume expansion rate, poor conductivity, and low ion diffusion coefficient, making them unable to achieve large-scale market application. Moreover, the modification process cost is high, and it is difficult to match the energy density increase of lithium iron phosphate cathode materials. .

Method used

Preparation method of carbon-coated silicon-carbon negative electrode material using graphene and nano-hard carbon for double coating. Through primary coating and secondary coating processes, a birdcage structure is established to block the insertion of ions into the silicon lattice and improve conductivity. and cyclic stability.

Benefits of technology

It effectively reduces the volume expansion rate of silicon, improves specific capacity, energy density, conductivity and safety performance, simplifies the process, reduces production costs, and is suitable for industrial large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841549A_ABST
    Figure CN118841549A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of battery negative electrode materials, in particular to a preparation method of a carbon-coated silicon-carbon negative electrode material based on graphene modification. According to the preparation method, flawless original graphene powder is used as a coating material, original graphene is dispersed through an industrial pure alcohol or industrial pure ether solvent to perform primary coating modification on coating object micron silicon, and then hard carbon powder is used as a coating material to complete secondary coating; and the graphene-modified carbon-coated silicon-carbon negative electrode material is successfully prepared through cold press molding and hot pressed sintering. Compared with an existing lithium / sodium ion battery negative electrode material, the lithium / sodium ion battery negative electrode material has the advantages that the micron silicon is secondarily coated with the graphene and the nano hard carbon respectively, a coating birdcage structure is arranged for the micron silicon, ions are prevented from being embedded into silicon lattices, and silicon volume expansion is thoroughly eliminated; the specific capacity, the energy density, the electrical conductivity, the thermal conductivity, the fast charging performance and the safety performance of the silicon-carbon negative electrode material are improved, production equipment is simple, the production period is short, the cost is low, and the method is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery negative electrode material preparation, in particular to a method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material. Background Art

[0002] Due to the high economy, safety and cycle performance of lithium iron phosphate batteries, 90% of the positive electrode materials used in mainstream pure electric vehicles, pure electric drive vehicles, and hybrid electric vehicles are lithium iron phosphate materials. The energy density of its battery cells has reached 165Wh / kg of lithium iron phosphate (theoretical specific capacity is 170mAh / g). In the future, the design and exploration of the lithium iron phosphate material system will further improve its energy density, which is expected to reach 200Wh / kg-230Wh / kg, and the energy density will reach its "ceiling". According to the optimal ratio of battery positive and negative electrode energy density of 1:1.1~1.5, the energy density of the matching negative electrode material should be 220Wh / kg~320Wh / kg. Currently, 95% of the negative electrode materials of mainstream mobile energy batteries are graphite and hard carbon (theoretical specific capacity is 370mAh / g), and the maximum energy density can reach 350Wh / kg. However, the market expectation for power batteries is currently 400Wh / kg to 500Wh / kg. The current mainstream positive electrode material lithium iron phosphate system is no longer competent, and the mainstream negative electrode materials graphite and hard carbon are also not competent.

[0003] People have found that the silicon negative electrode (theoretical specific capacity is 4200mAh / g) material system has a moderate lithium insertion potential (~0.4Vvs.Li+ / Li), and is most likely to replace graphite as the next generation of high-performance lithium-ion (or other) battery negative electrode materials. However, silicon has a fatal weakness of excessive volume expansion rate (>300%). The working principle of ion batteries is that when the battery is charged, ions are deintercalated from the positive electrode, transferred to the negative electrode through the electrolyte, and then embedded in the negative electrode material. When discharging, the ions are reversely deintercalated and embedded. Except for silicon (sulfur), the ions of other materials are embedded in the voids of the material (void embedding), and the material hardly produces volume expansion; but silicon (sulfur) is different. The ion embedding is embedded in the silicon lattice (lattice embedding) rather than the voids, causing the silicon lattice to expand. When deintercalating, the ions are removed from the silicon lattice, which shrinks and reduces the silicon lattice. The ratio of the expansion of the lattice volume after this embedding to the original lattice volume is a unique physical parameter of silicon specifically referred to here, called the volume expansion rate of silicon. The expansion rate of pure silicon is as high as 320%, which is fatal as an electrode material. The silicon of the negative electrode will collapse and fall off after less than 500 cycles of charge and discharge, and in severe cases, it may cause a safety accident of battery short circuit. At the same time, the first charge coulomb efficiency (first efficiency) of silicon is extremely low, only about 65%. The advantages of silicon as a negative electrode material are obvious, and its specific capacity is the highest among all materials currently available. The disadvantages of silicon as a negative electrode material are also obvious, and its volume expansion rate is the highest among all materials currently available. Silicon also has a characteristic that when charged, it naturally allows ions to embed into the lattice rather than the gaps. Only when the silicon lattice is filled with ions can ions fill the gaps, which is called the ion embedding induced characteristic of the silicon lattice. The use of silicon oxidation, nano-sizing, composite, porous, alloying, pre-lithium / sodium, mechanical grinding silicon-carbon composite and other modification methods can alleviate the volume expansion problem faced by silicon-based negative electrode materials, but it cannot be eradicated. In addition, the inherent disadvantages such as poor conductivity and low ion diffusion coefficient make it impossible for silicon-based negative electrode materials to achieve large-scale market applications. Currently, there are only two types of silicon-based negative electrode materials used commercially: silicon-carbon oxide composites (silicon-oxygen) and silicon-carbon mechanical composites (silicon-carbon).

[0004] Silicon oxide generally uses chemical vapor deposition (CVD) to evenly distribute 2nm to 10nm silicon particles in a silicon dioxide matrix. The specific capacity of silicon oxide negative electrode materials is generally 1300mAh / g to 1700mAh / g. Because the silicon material particles are smaller, the dispersion is more uniform, and the material structure is more dense and stable, the material has a lower volume expansion rate and better long-cycle stability. However, since silicon dioxide will react irreversibly with lithium / sodium in the first week, the first efficiency of the material is generally very low (70.6%), which greatly reduces the actual energy density of lithium / sodium batteries. The first efficiency, specific capacity, and cycle life of silicon oxide carbon negative electrodes can be improved by carbon coating, pre-lithium / sodium, and metal doping. Among them, the first efficiency of the silicon oxide negative electrode after pre-lithium / sodium can be increased to 86% to 90%, but it inevitably brings the problem of excessive cost. The American company Sila was the first to launch vapor-deposited silicon-carbon materials, which formed a dense silicon-carbon structure by sequentially depositing silane and hydrocarbon gases. At that time, it was highly recognized by the industry. However, as the industrialization progressed, it was found that ethylene and silicon were difficult to form a highly consistent nano-scale coating, the process difficulty was much higher than expected, and the production cost was still too high (500,000 yuan / ton), and the voice of industry advocacy gradually became smaller. According to a recent survey of high-end carbon materials, the market price of pre-lithium / sodium-treated silicon oxide with a specific capacity of 1400mAh / g and an initial efficiency of 93% has exceeded 1 million yuan / ton (silicon oxide products with an initial efficiency of about 90% are priced at about 800,000 yuan / ton to 900,000 yuan / ton), which is 25 times more expensive than the current graphite price (40,000 yuan / ton), making it impossible for lithium / sodium battery manufacturers to afford it. The problem of residual alkali on the surface of the material after pre-lithium / sodium treatment has not been solved, which will lead to problems such as poor material processability and battery gas production.

[0005] The technical route for the mechanical composite preparation of silicon and carbon is different from that of the CVD method. The CVD method first nano-sizes silicon, then uses carbon as the core and coats it with nano-silicon. The method for preparing silicon-carbon mechanical composites is to mechanically mix silicon and carbon in a certain proportion to obtain a silicon-carbon composite material. The loss of its specific capacity and the reduction of its volume expansion rate are basically presented in accordance with the silicon-carbon ratio. The introduction of mechanical grinding can also suppress the expansion rate. Before 2021, the preparation of silicon-carbon materials by grinding was widely favored. In theory, grinding silicon particles to less than 20nm without agglomeration can greatly solve the problem of silicon negative electrode expansion, but it has been proved that this exceeds the limit of the grinding process. Even if the preparation of nano-silicon below 20nm is achieved, it is difficult to ensure its dispersibility, which increases the difficulty of subsequent carbon coating. In addition, silicon nano-sizing solves the problem of lattice expansion superposition, but it cannot solve the problem of lattice expansion itself. Even if the silicon particles are ground to a single lattice particle (particle size of about 2nm), the volume expansion rate of the material is still 60%. Judging from the performance of existing materials, the cycle performance of silicon-carbon by grinding is still poor, still only 500 to 600 times. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a carbon-coated silicon-carbon negative electrode material based on graphene modification, in which original graphene and nano-hard carbon are used to completely coat silicon to block ions from being embedded in the silicon lattice.

[0007] The object of the present invention is achieved by the following technical solution: a method for preparing a carbon-coated silicon-carbon negative electrode material based on graphene modification, which comprises the following steps:

[0008] S1. Primary coating: taking defect-free original graphene powder, adding 1-20 μm micron silicon powder into a coating machine, and adding industrial pure alcohol or industrial pure ether solvent for dispersion and primary coating, the resulting slurry is dried to obtain graphene-modified and coated silicon composite material powder, wherein the primary coating time is 6 to 24 hours;

[0009] S2. Secondary coating: adding 30 to 200 nm hard carbon powder, the graphene-modified coated silicon composite powder obtained in step S1 and the modifier to a coating machine for secondary coating to obtain graphene-modified carbon-coated silicon composite powder; wherein the secondary coating time is 30 to 90 min;

[0010] S3 cold pressing: cold pressing the graphene-modified carbon-coated silicon composite powder prepared in step S2 into a cold pressed block, wherein the cold pressing pressure is 10 to 30 MPa;

[0011] S4. Hot pressing and sintering: The cold pressed block is placed in a vacuum hot pressing and sintering furnace for hot pressing and sintering. The sintering temperature is 550 to 750 ° C and the hot pressing is 80 to 150 kgf / cm 2 , vacuum degree<1.5×10 -2 Pa, the sintering time is 2 to 4 hours, and the sintering is followed by cooling and crushing to obtain the carbon-coated silicon-carbon negative electrode material based on graphene modification.

[0012] Furthermore, in step S1, the weight ratio of the micron silicon powder to the defect-free original graphene powder is 5 to 20:1, and the volume ratio of the total weight of the defect-free original graphene powder and the micron silicon powder to the industrial pure alcohol or industrial pure ether solvent is 1 mg:1 ml.

[0013] Furthermore, the primary coating in step S1 is performed using an ultrasonic dispersion coating machine, and the power of the coating machine is ≥1500W.

[0014] Furthermore, the slurry drying in step S1 is carried out in a vacuum drying oven, the drying temperature is 90-110° C., and the drying time is 60-90 min.

[0015] Furthermore, in step S2, the weight ratio of nano hard carbon powder to micron silicon powder is 3 to 19:1.

[0016] Furthermore, the modifier in step S2 is at least one of an organic dry modifier or an inorganic dry modifier, the weight ratio of the modifier to the mixed powder in step S2 is 1:90-110, and the mixed powder is a mixture of nano hard carbon powder and graphene modified and coated silicon composite material powder. Organic dry modifiers include glucose, phenolic acid, polyvinyl alcohol, etc., and inorganic dry modifiers include manganese oxide, zinc oxide, etc.

[0017] Furthermore, the secondary coating in step S2 is performed by a continuous powder surface coating and modification machine, and the rotation speed of the coating machine is set to 2000-7000 rpm.

[0018] The theoretical specific capacity of silicon is 4200mAh / g. The theoretical specific capacity of carbon varies according to its form: soft carbon: 220mAh / g, carbon nanotubes: 340mAh / g, hard carbon / graphite: 370mAh / g, and graphene: 2000mAh / g.

[0019] Although defect-free graphene is the material with the best electrical and thermal conductivity in the world, and also the material with the highest specific capacity among carbon-based materials, these superb properties also indicate the super strong van der Waals forces between its molecules, which makes it difficult to disperse and easy to agglomerate, making it difficult to apply.

[0020] The present invention uses graphene and nano-carbon as coating materials, and micron silicon as the core for coating. Theoretically, the logic is rigorous, and the "blocking ions from embedding into the silicon lattice" has been successfully verified in actual preparation. Therefore, in the present invention, the silicon core particle size used is 1 to 20 μm, the hard carbon particle size used is 30 to 200 nm, and the graphene particle size used is 2 to 10 nm. The more uniform and complete the coating layer is, the smaller the exposed silicon surface area is. Even if there is the ion embedding induction characteristic of the silicon lattice, the opportunity for ions to embed into the silicon lattice is smaller. When charging, the ions can only be embedded in the interlayer gaps of silicon and carbon, which ultimately solves the problem of silicon expansion. This is the birdcage structure used in chemical engineering. The birdcage structure is coated with nano-carbon to lock the silicon particles in the cage and block the ions from embedding into the silicon lattice.

[0021] At the same time, the present invention innovates a secondary coating process, and the coating materials are graphene as the first coating material and nano-hard carbon as the second coating material. Graphene coating not only blocks ions from being embedded in the silicon lattice and reduces the silicon expansion rate, but more importantly, it can modify the negative electrode material to improve the material's electrical conductivity, thermal conductivity, fast charging performance, and safety performance. Since graphene is expensive, it is mainly used for modification purposes, and the task of completely blocking ions from being embedded in the silicon lattice is placed on the secondary coated nano-hard carbon. The secondary coating is carried out in a continuous powder surface coating and modification machine operating in a high-speed gas-solid vortex mixing operation. After coating, we can see that the carbon has completely coated the silicon particles, and the silicon particles are no longer visible. The coating effect is very obvious (seeFigure 2 , Figure 3 ). This coating effect has not been reported so far. Through experimental tests, it was found that the material expansion rate is below 30% (reaching the charging volume expansion rate of carbon, which is less than the thermal expansion rate of carbon), and the number of cycles can be guaranteed to be more than 3,000 times. No other domestic patents or technical documents have been found to report this.

[0022] It should be noted that the present invention does not use graphene oxide (GO) or reduced graphene oxide (rGO) with serious defects to coat and prepare silicon-carbon negative electrode materials. There are examples of lithium-ion batteries using silicon-carbon negative electrodes coated with GO or rGO. First of all, in these examples, due to severe lattice distortion and electron hole defects, the intermolecular van der Waals forces are greatly reduced and more easily electrochemically wetted, which indicates that it is easier to disperse initially and the modification is easier to carry out. Although the electrical performance of lithium-ion batteries in the early stage of modification is still far from the results of the original graphene modification, it improves the electrical performance of the negative electrode material after all. However, as the cycle continues to deepen, the nucleation overpotential of GO or rGO becomes gradually higher than that of the original graphene, indicating that the Coulomb efficiency (CE) of the GO or rGO modified electrode begins to decline, and the decline is accelerated, resulting in severe electrolyte interface (SEI) growth and related FEC consumption, and a large number of dendrites will be generated at the positive electrode after the cycle. The reason is that the structural defects of GO or rGO itself are integrated into the modified material, causing a large number of structural defects in the modified material, because highly defective GO or rGO will promote the growth of unstable SEI, forming filamentous lithium dendrites at the positive electrode, and the dendrites produced bring major safety hazards of combustion and explosion. Secondly, the lattice defects used for GO or rGO lead to incomplete particles and incomplete coating effects. After coating, the surface of silicon particles is exposed everywhere (a broken birdcage), which cannot block the ions from being embedded in the silicon lattice, and the expansion rate of the material cannot be greatly reduced. Thirdly, another serious defect of GO or rGO is the residual defect of acid ions. No matter what method is used to wash GO and rGO, the acid ions in their molecules cannot be completely removed. Under certain environmental conditions, acid ions will precipitate from the materials modified by GO and rGO, and then corrode or poison the materials, and also produce harmful environments for the human body in contact.

[0023] The present invention has the following advantages: The present invention discloses a method for preparing carbon-coated silicon-carbon negative electrode materials based on graphene modification, using defect-free nano-original graphene powder as the first coating material, dispersing original graphene on micron silicon through industrial pure alcohol or industrial pure ether solvent for the first coating modification, and then using 30nm to 200nm hard carbon powder as the second coating material to complete the secondary coating, and successfully preparing graphene-modified battery silicon-carbon negative electrode materials. Compared with the existing lithium / sodium ion battery negative electrode materials, the present invention uses graphene and nano-hard carbon to coat micron silicon for the second time, sets a coating birdcage structure for it, blocks ions from being embedded in the silicon lattice to completely eliminate the silicon volume expansion rate; improves the specific capacity, energy density, electrical conductivity, thermal conductivity, fast charging performance and safety performance of silicon-carbon negative electrode materials, and has simple production equipment, short production cycle, simple process, low cost, and is suitable for industrial large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a flow chart of the preparation method of carbon-coated silicon-carbon negative electrode material based on graphene modification.

[0025] Figure 2 This is a 8000x SEM image of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 2.

[0026] Figure 3 This is a 10,000x SEM image of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 3.

[0027] Figure 4 This is the energy density test diagram of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 1.

[0028] Figure 5 This is the specific capacity test curve of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 1.

[0029] Figure 6 This is the specific capacity test curve of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 2.

[0030] Figure 7 This is the specific capacity test curve of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 3.

[0031] Figure 8 This is the specific capacity test curve of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 4.

[0032] Fig. 9 This is the specific capacity test curve of the graphene-modified carbon-coated silicon-carbon negative electrode material prepared in Experimental Example 5. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments, and the protection scope of the present invention is not limited to the following: Embodiment 1: A method for preparing a carbon-coated silicon-carbon negative electrode material based on graphene modification, which comprises the following steps:

[0034] S1. Primary coating: Take defect-free original graphene powder, add 1 to 20 μm micron silicon powder to an ultrasonic dispersion coating machine, the power of the coating machine is 1500W, and add industrial pure alcohol solvent for dispersion and primary coating, the primary coating time is 6h, and the resulting slurry is dried to obtain a graphene-modified silicon composite material powder;

[0035] The weight ratio of the micron silicon powder to the defect-free original graphene powder is 20:1, and the volume ratio of the total weight of the defect-free original graphene powder and the micron silicon powder to the industrial pure alcohol solvent is 1 mg:1 ml; the slurry is dried in a vacuum drying oven at a drying temperature of 90° C. and a drying time of 60 min;

[0036] S2. Secondary coating: The hard carbon powder of 30 to 200 nm, the graphene-modified silicon composite powder obtained in step S1 and the modifier are added to a continuous powder surface coating modifier for secondary coating, the speed of the coating machine is set to 2000 rpm, the secondary coating time is 30 min, and a graphene-modified carbon-coated silicon composite powder is obtained;

[0037] The weight ratio of nano hard carbon powder to micron silicon powder is 5:1; the modifier is glucose, the weight ratio of the modifier to the mixed powder in step S2 is 1:90, and the mixed powder is a mixture of hard carbon powder and graphene-modified and coated silicon composite material powder;

[0038] S3 cold pressing: The graphene-modified carbon-coated silicon composite powder prepared in step S2 is cold pressed into a cold pressed block, wherein the cold pressing pressure is 10 MPa;

[0039] S4. Hot pressing and sintering: The cold pressed block is placed in a vacuum hot pressing and sintering furnace for hot pressing and sintering. The sintering temperature is 550°C and the hot pressing is 80kgf / cm 2 , the vacuum degree is 1.3×10 -2 Pa, the sintering time is 2h, and the sintering is followed by cooling and crushing to obtain the carbon-coated silicon-carbon negative electrode material based on graphene modification.

[0040] Embodiment 2: A method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material, comprising the following steps:

[0041] S1. Primary coating: Take defect-free original graphene powder, add 1 to 20 μm micron silicon powder to an ultrasonic dispersion coating machine, the power of the coating machine is 1800W, and add industrial pure ether solvent for dispersion and primary coating, the primary coating time is 24h, and the resulting slurry is dried to obtain a graphene-modified silicon composite material powder;

[0042] The weight ratio of the micron silicon powder to the defect-free original graphene powder is 20:1, and the volume ratio of the total weight of the defect-free original graphene powder and the micron silicon powder to the industrial pure ether solvent is 1 mg:1 ml; the slurry is dried in a vacuum drying oven at a drying temperature of 110° C. and a drying time of 90 min;

[0043] S2. Secondary coating: 30 to 200 nm hard carbon powder, the graphene-modified silicon composite powder obtained in step S1 and the modifier are added to a continuous powder surface coating modifier for secondary coating, the coating machine speed is set to 7000 rpm, the secondary coating time is 90 min, and a graphene-modified carbon-coated silicon composite powder is obtained;

[0044] The weight ratio of nano hard carbon powder to micron silicon powder is 19:1; the modifier is manganese oxide, the weight ratio of the modifier to the mixed powder in step S2 is 1:110, and the mixed powder is a mixture of hard carbon powder and graphene-modified and coated silicon composite material powder;

[0045] S3 cold pressing: The graphene-modified carbon-coated silicon composite powder prepared in step S2 is cold pressed into a cold pressed block, wherein the cold pressing pressure is 30 MPa;

[0046] S4. Hot pressing and sintering: The cold pressed block is placed in a vacuum hot pressing and sintering furnace for hot pressing and sintering. The sintering temperature is 750°C and the hot pressing is 150kgf / cm 2 , vacuum degree is 1.0×10 -2 Pa, the sintering time is 4h, and the sintering is followed by cooling and crushing to obtain the carbon-coated silicon-carbon negative electrode material based on graphene modification.

[0047] Embodiment 3: A method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material, comprising the following steps:

[0048] S1. Primary coating: Take defect-free original graphene powder, add 1 to 20 μm micron silicon powder to an ultrasonic dispersion coating machine, the power of the coating machine is 2000W, and add industrial pure alcohol solvent for dispersion and primary coating, the primary coating time is 14h, and the resulting slurry is dried to obtain a graphene-modified silicon composite material powder;

[0049] The weight ratio of the micron silicon powder to the defect-free original graphene powder is 10:1, and the volume ratio of the total weight of the defect-free original graphene powder and the micron silicon powder to the industrial pure alcohol solvent is 1 mg:1 ml; the slurry is dried in a vacuum drying oven at a drying temperature of 100° C. and a drying time of 75 min;

[0050] S2. Secondary coating: 30 to 200 nm hard carbon powder, the graphene-modified silicon composite powder obtained in step S1 and the modifier are added to a continuous powder surface coating modifier for secondary coating, the speed of the coating machine is set to 55000 rpm, the secondary coating time is 60 min, and a graphene-modified carbon-coated silicon composite powder is obtained;

[0051] The weight ratio of nano hard carbon powder to micron silicon powder is 10:1; the modifier in step S2 is phenolic, and the weight ratio of the modifier to the mixed powder in step S2 is 1:99, and the mixed powder is a mixture of hard carbon powder and graphene-modified and coated silicon composite material powder;

[0052] S3 cold pressing: The graphene-modified carbon-coated silicon composite powder prepared in step S2 is cold pressed into a cold pressed block, wherein the cold pressing pressure is 22MPa;

[0053] S4. Hot pressing and sintering: The cold pressed block is placed in a vacuum hot pressing and sintering furnace for hot pressing and sintering. The sintering temperature is 600°C and the hot pressing is 120kgf / cm 2 , vacuum degree is 0.8×10 -2 Pa, the sintering time is 3h, and the sintering is followed by cooling and crushing to obtain the carbon-coated silicon-carbon negative electrode material based on graphene modification.

[0054] The beneficial effects of the present invention are described below by experiments:

[0055] Experimental Example 1: A method for preparing a carbon-coated silicon-carbon negative electrode material based on graphene modification, the flow chart is as follows Figure 1 As shown, it includes the following steps:

[0056] S1. One coating: Take 0.5% of the total weight of the defect-free original graphene powder (commercially available, NTCGPDFL series graphene powder) of the graphene-modified carbon-coated silicon-carbon negative electrode material (hereinafter referred to as silicon-carbon negative electrode material), and 5% of the total weight of 1-5μm micron silicon powder of the silicon-carbon negative electrode material, add an ultrasonic dispersion coating machine, the power of the coating machine is 1500W, and add industrial pure alcohol solvent for dispersion and one coating, the coating time is 12h, the total weight (m) of the defect-free original graphene powder and the micron silicon powder and the volume (v) of the industrial pure alcohol solvent is m:v=1mg:1ml, so that the mixed powder is in a flowable paste in the container (with no stratification at rest as the standard), and the resulting slurry is carried out in a vacuum drying oven, the drying temperature is 100°C, and the drying time is 60min, that is, the graphene-modified coated silicon composite material powder;

[0057] S2. Secondary coating: 94.5% of the total weight of the silicon-carbon negative electrode material, 200nm hard carbon powder, the graphene-modified coated silicon composite material powder obtained in step S1, and 1% of the total weight of the silicon-carbon negative electrode material modifier polyvinyl alcohol are added to a continuous powder surface coating modifier for secondary coating, the speed of the coating machine is set to 4000rpm, the secondary coating time is 60min, and the graphene-modified carbon-coated silicon composite material powder is obtained;

[0058] S3 cold pressing: The graphene-modified carbon-coated silicon composite powder prepared in step S2 is placed in a graphite mold and cold pressed into a cold block using a hydraulic press at room temperature, wherein the cold pressing pressure is 30 MPa;

[0059] S4. Hot pressing and sintering: The cold pressed block is placed in a vacuum hot pressing and sintering furnace for hot pressing and sintering. The sintering temperature is 580°C and the hot pressing pressure is 110kgf / cm 2 , vacuum degree is 1.0×10 -2 Pa, the sintering time is 2 h, and after cooling, the obtained material block is crushed in a dry ultrasonic jet airflow mill.

[0060] Experimental Example 2: The preparation method is the same as that of Experimental Example 1, except that the amount of defect-free original graphene powder is 1% of the total weight of the silicon-carbon negative electrode material, the amount of micron silicon powder is 10% of the total weight of the silicon-carbon negative electrode material, and the amount of hard carbon powder is 89% of the total weight of the silicon-carbon negative electrode material.

[0061] Experimental Example 3: The preparation method is the same as that of Experimental Example 1, except that the amount of defect-free original graphene powder is 2% of the total weight of the silicon-carbon negative electrode material, the amount of micron silicon powder is 15% of the total weight of the silicon-carbon negative electrode material, and the amount of hard carbon powder is 84% ​​of the total weight of the silicon-carbon negative electrode material.

[0062] Experimental Example 4: The preparation method is the same as that of Experimental Example 1, except that the amount of defect-free original graphene powder is 2% of the total weight of the silicon-carbon negative electrode material, the amount of micron silicon powder is 22% of the total weight of the silicon-carbon negative electrode material, and the amount of hard carbon powder is 76% of the total weight of the silicon-carbon negative electrode material.

[0063] Experimental Example 5: The preparation method is the same as that of Experimental Example 1, except that the amount of defect-free original graphene powder is 3% of the total weight of the silicon-carbon negative electrode material, the amount of micron silicon powder is 21% of the total weight of the silicon-carbon negative electrode material, and the amount of hard carbon powder is 76% of the total weight of the silicon-carbon negative electrode material.

[0064] Scanning electron microscope (SEM) observations were performed on Experimental Examples 1-5, and satisfactory coating results were obtained. Here, SEM photos of Experimental Examples 2 and 3, which are most likely to become the preferred negative electrode material formulations for the next generation of ion batteries, are selected ( Figure 2 and Figure 3 ). There are no silicon particles in the photo, indicating that graphene and nano-hard carbon have been evenly coated on the silicon particles.

[0065] Here we select the curve of Experiment 1 with the lowest specific capacity and energy density ( Figure 4 , Figure 5 ). The figure shows that even in Experimental Example 1, its specific capacity and energy density are much better than the current graphite negative electrode materials.

[0066] We also tested the specific capacity and energy density of Experimental Examples 1-5 and obtained satisfactory results. Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 and Fig. 9 , the test conditions are shown in Table 1:

[0067] Table 1: Specific capacity and energy density test conditions for Experimental Examples 1-5

[0068]

[0069] The performance of the graphene-modified carbon-coated silicon-carbon negative electrode materials prepared in Experimental Examples 1-5 was tested, and the experimental results are shown in Table 2:

[0070] Table 2: Performance test results of graphene-modified carbon-coated silicon-carbon negative electrode material samples prepared in Experimental Examples 1-5

[0071]

[0072] The experiment found that:

[0073] -When using an ultrasonic separator to disperse graphene, the power cannot be less than 600W. The greater the power, the better the dispersion effect. When the power is greater than 1500W, the dispersion effect does not change much, so an ultrasonic separator with a power greater than 1500W can be selected;

[0074] - After the first coating, use a vacuum drying oven to dry. If the drying temperature is low, the drying time will be long. After many experiments, it is best to dry at 100°C for 60 minutes;

[0075] - After the first coating, no separated graphene can be observed by SEM. Due to the high light transmittance of graphene, it is almost certain that the graphene has been evenly coated on the silicon particles and the gaps between the silicon particles have been filled;

[0076] -In the secondary coating process of nano-hard carbon, a continuous powder surface coating and modification machine with high-speed gas-solid vortex mixing is selected, which has high modification efficiency and basically does not destroy the original particle shape of the powder. The parameter selection also shows that the higher the speed, the shorter the coating time, but if the speed is too high, the coating is uneven. After many experiments, 4000 rpm mixing and stirring for 60 minutes was selected for secondary coating;

[0077] -When hydraulic material blocks are implemented before sintering, increased pressure is beneficial to material properties, but too high pressure will make crushing difficult after sintering. After many experiments, 30MPa was selected;

[0078] - Similarly, in the hot pressing vacuum sintering process, the sintering temperature is selected as 580℃ and the hot pressing is selected as 110kgf / cm 2 , the vacuum degree is selected as 1×10 -2 Pa, sintering time is 2 hours;

[0079] -After hot-pressing vacuum sintering, a dry ultrasonic jet airflow pulverizer is selected to pulverize the material, which does not destroy the particle shape of the material and can effectively disperse the material before preparing the battery silicon-carbon negative electrode slurry based on graphene modification;

[0080] - When implementing coating modification, the particle size of the core material should be more than 30 times larger than the particle size of the coating material to facilitate uniform coating of the coating material. If there is a secondary coating, one can be more than 10 times and the other can be more than 50 times. The sample of the present invention selects a particle size ratio of micron silicon to nano hard carbon of 10 to 20 times, and a particle size ratio of micron silicon to graphene of more than 100 times;

[0081] - The volume percentage of graphene as a primary coating material increases from 0.5% to 2%, which has a significant effect on improving performance. When adding more than 3%, the performance improvement slows down. Due to its high cost, it is not recommended to add more than 2%.

[0082] The graphene-modified battery silicon-carbon negative electrode material prepared by the present invention has the following advantages:

[0083] 1. It basically blocks the ion embedding into the silicon lattice during charging, reducing the volume expansion rate of the material to less than 30%;

[0084] 2. Within the scope disclosed by the present invention, the silicon-carbon ratio can be flexibly adjusted to adapt the material specific capacity to the corresponding battery positive electrode material;

[0085] 3. The electrical conductivity and thermal conductivity are greatly improved, and the oxidation of the electrode surface is curbed;

[0086] 4. The energy density of ion batteries prepared using it is significantly increased;

[0087] 5. The safety and reliability of ion batteries prepared by it far exceed the current similar products, which is very beneficial to the operation of various battery management systems;

[0088] 6. The ion battery prepared by using it has significantly improved charge and discharge cycle life and product life;

[0089] 7. The ion battery prepared by it can be fast charged up to 12C without damaging the internal structure, which is naturally compatible with the 800V charging platform currently respected in the world;

[0090] 8. Since graphene coating modification can be carried out simultaneously with soft / hard carbon coating of large-particle silicon powder, the silicon powder grinding process (or vapor deposition process) is eliminated, which greatly reduces the cost of modified silicon carbon, and the cost can be reduced to less than RMB 60,000 / ton.

[0091] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which are all covered by the protection scope of the present invention.

Claims

1. A method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material, characterized in that: It includes the following steps: S1. Primary coating: Take defect-free original graphene powder, add 1-20 μm micron silicon powder into the coating machine, and add industrial pure alcohol or industrial pure ether solvent for dispersion and primary coating. The resulting slurry is dried to obtain graphene-modified and coated silicon composite material powder, wherein the primary coating time is 6 to 24 hours; S2 secondary coating: 30 ~ 200nm hard carbon powder, step S1 obtained graphene-modified coated silicon composite powder and modifier added to the coating machine for secondary coating, to obtain graphene-modified carbon-coated silicon composite powder; wherein the secondary coating time is 30 ~ 90min; S3 cold pressing: The graphene-modified carbon-coated silicon composite powder prepared in step S2 is cold pressed into a cold pressed block, wherein the cold pressing pressure is 10 to 30 MPa; S4. Hot pressing and sintering: The cold pressed block is placed in a vacuum hot pressing and sintering furnace for hot pressing and sintering. The sintering temperature is 550-750°C and the hot pressing is 80-150kgf / cm 2 , vacuum degree<1.5×10 -2 Pa, the sintering time is 2 to 4 hours, and the sintering is followed by cooling and crushing to obtain the carbon-coated silicon-carbon negative electrode material based on graphene modification.

2. The method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material according to claim 1, characterized in that: In step S1, the weight ratio of the micron silicon powder to the defect-free original graphene powder is 5 to 20:1, and the volume ratio of the total weight of the defect-free original graphene powder and the micron silicon powder to the industrial pure alcohol or industrial pure ether solvent is 1 mg:1 ml.

3. The method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material according to claim 1, characterized in that: The primary coating in step S1 is performed using an ultrasonic dispersion coating machine, and the power of the coating machine is ≥1500W.

4. The method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material according to claim 1, characterized in that: The slurry drying in step S1 is carried out in a vacuum drying oven at a drying temperature of 90 to 110° C. and a drying time of 60 to 90 minutes.

5. The method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material according to claim 1, characterized in that: In step S2, the weight ratio of nano hard carbon powder to micron silicon powder is 3 to 19:

1.

6. The method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material according to claim 1, characterized in that: The modifier in step S2 is at least one of an organic dry modifier or an inorganic dry modifier, and the weight ratio of the modifier to the mixed powder in step S2 is 1:90-110.

7. The method for preparing a graphene-modified carbon-coated silicon-carbon negative electrode material according to claim 1, characterized in that: The secondary coating in step S2 is performed by a continuous powder surface coating and modification machine, and the rotation speed of the coating machine is set to 2000-7000 rpm.