Ultrahigh-nickel polycrystalline positive electrode material as well as preparation method and application thereof
By doping the lithium-ion battery cathode material with large ion radius A elements and high-priced B elements, and using multi-material co-coating technology, the structural instability and electrical performance problems of high-nickel cathode materials have been solved, and high capacity has been achieved. And the rate performance is improved, the process is simplified and the side reactions are reduced.
Patent Information
- Application Number
- CN202410860921.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
AI Technical Summary
Existing high-nickel lithium-ion battery cathode materials have structural instability, cycle life and safety problems under high nickel content, and the washing process is complicated and difficult to control, resulting in aggravated side reactions and poor electrical performance.
The main body of the cathode material is doped with A element, which has a large ion radius and has a strong interaction with oxygen, and high-priced B elements are introduced to suppress polarization. Multi-material co-coating technology is used to reduce the residual alkali content and internal resistance, and reduce side reactions. Improve structural stability and electrochemical performance.
It achieves the structural stability and high capacity performance of ultra-high nickel cathode materials, reduces side reactions and internal resistance, improves capacity and rate performance, and avoids the complexity of the water washing process.
Smart Images

Figure CN118841558A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to an ultra-high nickel polycrystalline positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy, high power density, high energy efficiency, long cycle life and high safety, making them widely used in electric vehicles, portable electronic devices and energy storage fields. With the rapid development of electric vehicles, people's demand for the energy density, cycle life and safety performance of lithium-ion batteries is also increasing. High-nickel ternary positive electrode materials can provide high energy density, long cycle life and low cost and have been widely used. The increase in Ni content is conducive to improving the gram capacity of the material. Coupled with high compaction material design, the energy density of the material can be further improved. At present, the market generally adopts the method of mixing large and small particles to improve the compaction design, that is, filling small-particle single crystals or polycrystals with a D50 of 2-5μm into the gaps between medium and large particles with a D50 of 9-17μm to effectively improve the compaction of the mixed material. Among them, the grain size of small-particle polycrystalline materials is relatively small, Li + The short ion diffusion path is conducive to the occurrence of reactions, and usually has higher capacity and cycle performance, making it suitable for applications with higher energy density requirements.
[0003] However, the increase in Ni content inevitably leads to more complicated synthesis and some structural instability issues that limit battery cycle life and safety, namely, Li + / Ni 2+ Problems include ion mixing, phase transition from layered to inactive rock salt NiO, microcrack formation during cycling, dissolution of transition metals and subsequent deposition at the negative electrode, higher sensitivity to moisture, and more difficult to control water washing process.
[0004] For ultra-high nickel materials, the higher the nickel content, the worse the material stability. Currently, metal cation doping is often used. After washing to reduce residual alkali, a coating method is added to improve the material structure stability and thermal stability. However, while metal cation doping stabilizes the structure, it will inevitably cause capacity loss. In addition, traditional technologies use a one-time lithium addition method for sintering. However, during the high-temperature roasting process, Li + The volatilization of the material puts the material in a lithium-free state, causing a phase change and causing serious degradation of electrical performance. In addition, the water washing process in the existing high-nickel technology is complex and difficult to control. The high sensitivity of ultra-high nickel materials to water exacerbates the side reactions on the surface of the material during the water washing process. Even if the coating is applied after water washing, the effect is not good, and the capacity and rate performance are both poor.
[0005] Therefore, how to effectively improve the structural stability of ultra-high nickel positive electrode materials while also exerting high capacity performance and reducing the occurrence of side reactions is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide an ultra-high nickel polycrystalline positive electrode material and its preparation method and application. The present invention suppresses the polarization of the material in the electrochemical process by doping the A element with a large ion radius and a force with oxygen greater than that of the transition metal in the main body of the positive electrode material, thereby improving the structural stability, and at the same time introduces a high-valent B element to suppress grain growth. The high-valent B element can not only strengthen the crystal structure of the positive electrode material, but also strengthen its microstructure, thereby maximizing the electrochemical performance and exerting a higher capacity. In addition, the present invention adopts the technology of co-coating of multiple materials, which further improves the structural stability of the material, effectively repairs the surface structure of the material, reduces the residual alkali content, does not require water washing, reduces side reactions, and the high conductivity coating also reduces the internal resistance of the material. The ultra-high nickel polycrystalline positive electrode material has excellent capacity and rate performance.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides an ultra-high nickel polycrystalline positive electrode material, the ultra-high nickel positive electrode material comprising a positive electrode material body, and a coating layer coated on the surface of the positive electrode material body;
[0009] The chemical formula of the positive electrode material is LiNi x Co y Mn 1-x-y O2, where 0.9≤x<1, 0<y≤0.06;
[0010] The positive electrode material body is doped with an A element and a B element, wherein the A element includes any one of Zr, Sr, Ce, La, Al, Mg, Na, Ca, Y or Sn or a combination of at least two thereof, and the B element includes any one of Sb, W, Nb, Mo, Ti or P or a combination of at least two thereof;
[0011] The materials in the coating layer include Li-containing material, Co-containing material and solid electrolyte.
[0012] The present invention improves the structural stability by doping the A element with a large ion radius and a greater interaction force with oxygen than the transition metal into the main body of the positive electrode material to inhibit the polarization of the material during the electrochemical process, while introducing a high-valent B element to inhibit grain growth. The high-valent B element can not only strengthen the crystal structure of the positive electrode material, but also strengthen its microstructure, thereby maximizing the electrochemical performance and exerting a higher capacity. In addition, the present invention adopts the technology of multiple material co-coating, which further improves the structural stability of the material, effectively repairs the surface structure of the material, reduces the residual alkali content, does not require water washing, reduces side reactions, and the high conductivity coating also reduces the internal resistance of the material. The ultra-high nickel polycrystalline positive electrode material has excellent capacity and rate performance.
[0013] In the present invention, the introduction of Li-containing materials into the coating layer can provide additional lithium ion replenishment materials to reduce the active lithium ion consumption during the charge and discharge process, so as to improve the energy density; the introduction of Co-containing materials plays a key role in reducing the residual alkali content and improving the surface structure stability. Co will react with the residual alkali (such as LiOH and Li2CO3) on the surface of the material to generate Li x CoO2 and Co3O4 compounds, electrochemical passivation of spinel Co3O4 can stabilize the surface structure of the material, Li x CoO2 can produce high conductivity due to its low energy gap, thereby improving capacity and rate; the introduction of solid electrolyte further improves ionic conductivity and reduces charge exchange impedance. The co-coating of the above materials can also effectively prevent direct contact between the positive electrode material and the electrolyte, prevent the generation of microcracks, and further improve the structural stability of the material.
[0014] In the present invention, 0.9≤x<1, for example, it can be 0.9, 0.92, 0.94, 0.96 or 0.98, etc., 0<y≤0.06, for example, it can be 0.01, 0.02, 0.03, 0.04 or 0.05, etc.,
[0015] Preferably, the particle size D50 of the main body of the positive electrode material is 2-5 μm, for example, it can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm.
[0016] Preferably, the coating layer has a thickness of 10-100 nm, for example, 10 nm, 30 nm, 50 nm, 70 nm or 90 nm.
[0017] Preferably, the surface residual alkali compounds of the ultra-high nickel polycrystalline positive electrode material include LiOH and Li2CO3, the content of LiOH is ≤5500ppm, for example, it can be 5500ppm, 5000ppm or 4000ppm, etc., and the content of Li2CO3 is ≤3500ppm, for example, it can be 3500ppm, 3000ppm or 2000ppm, etc.
[0018] Preferably, the Li-containing material includes any one of Li3N, Li2S, LiF, Li2NiO2, Li2O or Li2O2, or a combination of at least two thereof.
[0019] Preferably, the Co-containing material includes any one of Co(OH)2, CoOOH, CoF2 or CoO, or a combination of at least two thereof.
[0020] Preferably, the solid electrolyte includes any one of LLZO, LLZTO, LATP or LASTP, or a combination of at least two of them.
[0021] It should be noted that LLZO refers to Li7La3Zr2O 12 LLZTO refers to Li 6.4 LqCy 1.4 Ta 0.6 O 12 , LATP refers to Li 1.3 Al 0.3 Ti 1.7 (PO4)3, LASTP refers to Li 1.3 Al 0.3 Si 0.1 Ti 16 (PO4)3.
[0022] Preferably, the mass ratio of the Li-containing material, the Co-containing material and the solid electrolyte is (1-4):(1-4):(1-6), wherein the selection range of the Li-containing material "1-4" can be, for example, 1, 2, 3 or 4, etc., the selection range of the Co-containing material "1-4" can be, for example, 1, 2, 3 or 4, etc., and the selection range of the solid electrolyte "1-6" can be, for example, 1, 2, 3, 4, 5 or 6, etc.
[0023] In the present invention, if the mass ratio of the Co-containing material to the solid electrolyte is too small, that is, the amount of the Co-containing material is too small or the amount of the solid electrolyte is too large, the residual lithium is too high, and the capacity and cycle deviations are; if the mass ratio of the Co-containing material to the solid electrolyte is too large, that is, the amount of the Co-containing material is too large or the amount of the solid electrolyte is too small, the capacity is low and the safety deviations are.
[0024] In a second aspect, the present invention provides a method for preparing the ultra-high nickel polycrystalline positive electrode material as described in the first aspect, the preparation method comprising the following steps:
[0025] (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, a compound containing element A, and a compound containing element B, and then calcining the mixture to obtain a calcined product;
[0026] (2) mixing the calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent, and performing secondary calcination to obtain the ultra-high nickel polycrystalline positive electrode material;
[0027] Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y (OH)2, wherein 0.9≤x<1, 0<y≤0.06.
[0028] Preferably, the lithium source in step (1) includes any one of LiOH, Li2CO3, LiNO3, Li3N, Li2S, LiF, Li2NiO2, Li2O or Li2O2, or a combination of at least two thereof.
[0029] Preferably, the compound containing element A in step (1) comprises any one of carbonate, nitrate, sulfate, chloride or oxide containing element A, or a combination of at least two thereof.
[0030] Preferably, the B-containing compound in step (1) comprises any one of carbonates, nitrates, sulfates, chlorides or oxides containing the B element, or a combination of at least two of them.
[0031] Preferably, the mass of element A in the element A-containing compound in step (1) is 0.05-0.3wt% of the mass of the ultra-high nickel positive electrode material precursor, for example, it can be 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt% or 0.3wt%, etc.
[0032] In the present invention, if the doping amount of element A is too small, the cycle performance of the material will decrease; if the doping amount of element A is too large, the capacity performance of the material will decrease.
[0033] Preferably, the mass of the B element in the B-containing compound in step (1) is 0.1-0.5wt% of the mass of the ultra-high nickel positive electrode material precursor, for example, it can be 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt% or 0.5wt%, etc.
[0034] In the present invention, if the doping amount of the B element is too small, the cycle performance of the material will be reduced; if the doping amount of the B element is too large, the cycle performance of the material will be reduced.
[0035] Preferably, the primary calcination in step (1) is carried out in an oxygen-containing atmosphere.
[0036] Preferably, the oxygen-containing atmosphere is an air atmosphere or a pure oxygen atmosphere.
[0037] Preferably, the primary roasting in step (1) is performed in a multi-stage roasting manner, including a primary roasting and a secondary roasting.
[0038] The present invention adopts a multi-stage calcination method, wherein the first stage of calcination is mainly for the dehydration of the precursor and the lithium salt. This stage of sintering is more conducive to the melting of the Li salt and its penetration into the interior of the precursor, which is conducive to the subsequent homogenization reaction, making the particles more uniform and the residual lithium lower.
[0039] Preferably, the temperature of the first stage roasting is 450-550°C, such as 450°C, 500°C or 550°C, and the time is 3-10h, such as 3h, 5h, 7h or 9h.
[0040] Preferably, the temperature of the second stage calcination is 700-800°C, such as 700°C, 750°C or 800°C, and the time is 6-15h, such as 6h, 8h, 10h, 12h or 15h.
[0041] Preferably, the secondary calcination in step (2) is carried out in an oxygen-containing atmosphere, and the oxygen-containing atmosphere is an air atmosphere or a pure oxygen atmosphere.
[0042] Preferably, the temperature of the secondary calcination in step (2) is 600-800°C, for example, 600°C, 700°C or 800°C, and the time is 5-10h, for example, 5h, 6h, 7h, 8h or 9h.
[0043] Preferably, based on the mass of the calcined product in step (2), the content of the Li-containing coating agent is 0.5-2wt%, for example, 0.5wt%, 1wt%, 1.5wt% or 2wt%, etc., the content of the Co-containing coating agent is 0.5-2wt%, for example, 0.5wt%, 1wt%, 1.5wt% or 2wt%, etc., and the content of the solid electrolyte coating agent is 0.5-3wt%, for example, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%, etc.
[0044] Preferably, the preparation method comprises the following steps:
[0045] (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, a compound containing element A and a compound containing element B to obtain a primary mixture, and then calcining the primary mixture in an oxygen-containing atmosphere, that is, first heating the temperature to 450-550° C. at a heating rate of 3-5° C. / min for a first-stage calcination, keeping the temperature for 3-10 hours, then heating the temperature to 700-800° C. at a heating rate of 1-3° C. / min for a second-stage calcination, keeping the temperature for 6-15 hours, and finally cooling the temperature to room temperature at a rate of 3-5° C. / min, and obtaining a calcined product after pulverization;
[0046] Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y (OH)2, where 0.9≤x<1, 0<y≤0.06;
[0047] (2) The calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent are stirred and mixed to obtain a secondary mixture, and then the secondary mixture is secondary calcined in an oxygen-containing atmosphere, that is, the temperature is increased to 600-800°C at a heating rate of 3-5°C / min, kept warm for 5-10h, and then cooled to room temperature at a rate of 3-5°C / min to obtain the ultra-high nickel polycrystalline positive electrode material.
[0048] In a third aspect, the present invention provides a lithium-ion battery, wherein the positive electrode of the lithium-ion battery comprises the ultra-high nickel polycrystalline positive electrode material as described in the first aspect.
[0049] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] The present invention improves the structural stability by doping the A element with a large ion radius and a greater interaction force with oxygen than the transition metal in the main body of the positive electrode material to inhibit the polarization of the material during the electrochemical process, while introducing a high-valent B element to inhibit grain growth. The high-valent B element can not only strengthen the crystal structure of the positive electrode material, but also strengthen its microstructure, thereby maximizing the electrochemical performance and exerting a higher capacity. In addition, the present invention adopts the technology of co-coating multiple materials to further improve the structural stability of the material, and effectively repair the surface structure of the material, reduce the residual alkali content, and it does not need to be washed with water, and the side reactions are reduced. At the same time, the high conductivity coating also reduces the internal resistance of the material. The ultra-high nickel polycrystalline positive electrode material has excellent capacity and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is a SEM image of the ultra-high nickel polycrystalline positive electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] It should be noted that the room temperature below refers to 25°C.
[0055] Example 1
[0056] This embodiment provides an ultra-high nickel polycrystalline positive electrode material, the ultra-high nickel positive electrode material comprising a positive electrode material body, and a coating layer coated on the surface of the positive electrode material body;
[0057] The chemical formula of the positive electrode material is LiNi x Co y Mn 1-x-y O2, wherein x=0.96, y=0.03, the positive electrode material is doped with element A and element B, element A is Sr, and element B is Sb;
[0058] The particle size D50 of the positive electrode material body is 3.5 μm;
[0059] The materials in the coating layer include a Li-containing material, a Co-containing material and a solid electrolyte, the thickness of the coating layer is 100 nm, the Li-containing material is Li3N, the Co-containing material is Co(OH)2, the solid electrolyte is LLZO, and the mass ratio of the Li-containing material, the Co-containing material and the solid electrolyte is 2:2:4;
[0060] This embodiment also provides a method for preparing the above-mentioned ultra-high nickel polycrystalline positive electrode material, and the preparation method comprises the following steps:
[0061] (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, a carbonate containing an Sr element, and a carbonate containing an Sb element to obtain a primary mixture, and then calcining the primary mixture in a pure oxygen atmosphere, that is, first heating the temperature to 500° C. at a heating rate of 4° C. / min for a first-stage calcination, keeping the temperature for 7 hours, then heating the temperature to 750° C. at a heating rate of 2° C. / min for a second-stage calcination, keeping the temperature for 10 hours, and finally cooling the temperature to room temperature at a rate of 4° C. / min, and obtaining a calcined product after pulverization;
[0062] Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y(OH)2, wherein x=0.96, y=0.03, the lithium source is lithium hydroxide, the mass of the Sr element in the Sr-containing carbonate is 0.15wt% of the mass of the ultra-high nickel positive electrode material precursor, and the mass of the Sb element in the Sb-containing compound is 0.35wt% of the mass of the ultra-high nickel positive electrode material precursor;
[0063] (2) stirring and mixing the calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent to obtain a secondary mixture, and then performing a secondary calcination on the secondary mixture in a pure oxygen atmosphere, i.e., heating the mixture to 700° C. at a heating rate of 4° C. / min, keeping the temperature for 7 hours, and then cooling the temperature to room temperature at a rate of 4° C. / min, to obtain the ultra-high nickel polycrystalline positive electrode material;
[0064] Among them, the Li-containing coating agent is Li3N, the Co-containing coating agent is Co(OH)2, and the solid electrolyte coating agent is LLZO. Based on the mass of the calcined product, the content of the Li-containing coating agent is 1wt%, the content of the Co-containing coating agent is 1wt%, and the content of the solid electrolyte coating agent is 2wt%.
[0065] Figure 1 The SEM image of the ultra-high nickel polycrystalline positive electrode material prepared in this embodiment is shown. It can be seen from the image that the sphericity is good and the primary particles are uniform.
[0066] Example 2
[0067] This embodiment provides an ultra-high nickel polycrystalline positive electrode material, the ultra-high nickel positive electrode material comprising a positive electrode material body, and a coating layer coated on the surface of the positive electrode material body;
[0068] The chemical formula of the positive electrode material is LiNi x Co y Mn 1-x-y O2, wherein x=0.95, y=0.04, the positive electrode material body is doped with element A and element B, the element A is La, and the element B is W; the particle size D50 of the positive electrode material body is 2 μm;
[0069] The materials in the coating layer include a Li-containing material, a Co-containing material and a solid electrolyte, the coating layer has a thickness of 50 nm, the Li-containing material is Li2S, the Co-containing material is CoOOH, the solid electrolyte is LLZTO, and the mass ratio of the Li-containing material, the Co-containing material and the solid electrolyte is 1:1:6;
[0070] This embodiment also provides a method for preparing the above-mentioned ultra-high nickel polycrystalline positive electrode material, and the preparation method comprises the following steps:
[0071] (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, an oxide containing La and an oxide containing W to obtain a primary mixture, and then calcining the primary mixture in a pure oxygen atmosphere, that is, first heating the temperature to 450° C. at a heating rate of 3° C. / min for a first-stage calcination, keeping the temperature for 10 h, then heating the temperature to 700° C. at a heating rate of 1° C. / min for a second-stage calcination, keeping the temperature for 15 h, and finally cooling the temperature to room temperature at a rate of 3° C. / min, and obtaining a calcined product after pulverization;
[0072] Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y (OH)2, wherein x=0.95, y=0.04, the lithium source is lithium hydroxide, the mass of the La element in the La-containing oxide is 0.05wt% of the mass of the ultra-high nickel positive electrode material precursor, and the mass of the W element in the W-containing oxide is 0.5wt% of the mass of the ultra-high nickel positive electrode material precursor;
[0073] (2) stirring and mixing the calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent to obtain a secondary mixture, and then performing a secondary calcination on the secondary mixture in a pure oxygen atmosphere, i.e., heating the mixture to 600° C. at a heating rate of 1.0° C. / min, keeping the temperature for 10 h, and then cooling the temperature to room temperature at a rate of 3° C. / min, to obtain the ultra-high nickel polycrystalline positive electrode material;
[0074] Among them, the Li-containing coating agent is Li2S, the Co-containing coating agent is CoOOH, and the solid electrolyte coating agent is LLZTO. Based on the mass of the calcined product, the content of the Li-containing coating agent is 0.5wt%, the content of the Co-containing coating agent is 0.5wt%, and the content of the solid electrolyte coating agent is 3wt%.
[0075] Example 3
[0076] This embodiment provides an ultra-high nickel polycrystalline positive electrode material, the ultra-high nickel positive electrode material comprising a positive electrode material body, and a coating layer coated on the surface of the positive electrode material body;
[0077] The chemical formula of the positive electrode material is LiNi x Co y Mn 1-x-y O2, wherein x=0.96, y=0.01, the positive electrode material is doped with element A and element B, the element A is Na, and the element B is P;
[0078] The particle size D50 of the positive electrode material body is 5 μm;
[0079] The materials in the coating layer include a Li-containing material, a Co-containing material and a solid electrolyte, the coating layer has a thickness of 10 nm, the Li-containing material is LiF, the Co-containing material is CoF2, the solid electrolyte is LATP, and the mass ratio of the Li-containing material, the Co-containing material and the solid electrolyte is 4:4:1;
[0080] This embodiment also provides a method for preparing the above-mentioned ultra-high nickel polycrystalline positive electrode material, and the preparation method comprises the following steps:
[0081] (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, a carbonate containing a Na element, and a carbonate containing a P element to obtain a primary mixture, and then calcining the primary mixture in a pure oxygen atmosphere, that is, first heating the temperature to 550° C. at a heating rate of 5° C. / min for a first-stage calcination, keeping the temperature for 3 h, then heating the temperature to 800° C. at a heating rate of 3° C. / min for a second-stage calcination, keeping the temperature for 6 h, and finally cooling the temperature to room temperature at a rate of 5° C. / min, and obtaining a calcined product after pulverization;
[0082] Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y (OH)2, wherein x=0.96, y=0.01, the lithium source is lithium hydroxide, the mass of the Sr element in the carbonate containing the Na element is 0.3wt% of the mass of the ultra-high nickel positive electrode material precursor, and the mass of the Sb element in the compound containing the P element is 0.2wt% of the mass of the ultra-high nickel positive electrode material precursor;
[0083] (2) stirring and mixing the calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent to obtain a secondary mixture, and then performing a secondary calcination on the secondary mixture in a pure oxygen atmosphere, i.e., heating the mixture to 800° C. at a heating rate of 5° C. / min, keeping the temperature for 5 h, and then cooling the temperature to room temperature at a rate of 5° C. / min, to obtain the ultra-high nickel polycrystalline positive electrode material;
[0084] Among them, the Li-containing coating agent is LiF, the Co-containing coating agent is CoF2, and the solid electrolyte coating agent is LATP. Based on the mass of the calcined product, the content of the Li-containing coating agent is 2wt%, the content of the Co-containing coating agent is 2wt%, and the content of the solid electrolyte coating agent is 0.5wt%.
[0085] Example 4
[0086] The difference between this embodiment and embodiment 1 is that no primary roasting is performed in step (1).
[0087] The rest of the preparation methods and parameters were the same as those in Example 1.
[0088] Example 5
[0089] The difference between this embodiment and embodiment 1 is that no two-stage roasting is performed in step (1).
[0090] The rest of the preparation methods and parameters were the same as those in Example 1.
[0091] Example 6
[0092] The difference between this embodiment and embodiment 1 is that the mass ratio of the Co-containing material to the solid electrolyte is 1:7 by adjusting the amount of the Co-containing coating agent added in step (2).
[0093] The rest of the preparation methods and parameters were the same as those in Example 1.
[0094] Example 7
[0095] The difference between this embodiment and embodiment 1 is that the mass ratio of the Co-containing material to the solid electrolyte is 5:1 by adjusting the amount of the Co-containing coating agent added in step (2).
[0096] The rest of the preparation methods and parameters were the same as those in Example 1.
[0097] Example 8
[0098] The difference between this embodiment and embodiment 1 is that the amount of the carbonate containing the Sr element added in step (1) is adjusted so that the mass of the Sr element is 0.02 wt % of the mass of the ultra-high nickel positive electrode material precursor.
[0099] The rest of the preparation methods and parameters were the same as those in Example 1.
[0100] Example 9
[0101] The difference between this embodiment and embodiment 1 is that the amount of the carbonate containing the Sr element added in step (1) is adjusted so that the mass of the Sr element is 0.5wt% of the mass of the ultra-high nickel positive electrode material precursor. The rest of the preparation method and parameters are the same as those in embodiment 1.
[0102] Example 10
[0103] The difference between this embodiment and embodiment 1 is that the amount of the carbonate containing the Sb element added in step (1) is adjusted so that the mass of the Sb element is 0.05wt% of the mass of the ultra-high nickel positive electrode material precursor. The rest of the preparation method and parameters are the same as those in embodiment 1.
[0104] Embodiment 11
[0105] The difference between this embodiment and embodiment 1 is that the amount of the carbonate containing the Sb element added in step (1) is adjusted so that the mass of the Sb element is 0.6 wt % of the mass of the ultra-high nickel positive electrode material precursor.
[0106] The rest of the preparation methods and parameters were the same as those in Example 1.
[0107] Comparative Example 1
[0108] The difference between this comparative example and Example 1 is that there is no Li-containing material in the coating layer.
[0109] The rest of the preparation methods and parameters were the same as those in Example 1.
[0110] Comparative Example 2
[0111] The difference between this comparative example and Example 1 is that there is no Co-containing material in the coating layer.
[0112] The rest of the preparation methods and parameters were the same as those in Example 1.
[0113] Comparative Example 3
[0114] The difference between this comparative example and Example 1 is that there is no solid electrolyte in the coating layer.
[0115] The rest of the preparation methods and parameters were the same as those in Example 1.
[0116] Performance Testing
[0117] The ultra-high nickel polycrystalline positive electrode materials prepared in the above embodiments and comparative examples were made into positive electrode plates, which were assembled with negative electrode plates, separators and electrolytes into lithium-ion batteries, and then capacity performance tests, cycle performance tests and rate performance tests were carried out.
[0118] The specific assembly steps include: grinding and mixing the above-prepared positive electrode material with conductive carbon black and polyvinylidene fluoride (PVDF) in a mass ratio of 90:5:5, adding appropriate N-methylpyrrolidone (NMP) and stirring and dispersing, uniformly coating on aluminum foil, and drying to obtain a positive electrode sheet. Subsequently, the positive electrode sheet is dried at 120°C for 4 hours, and then rolled and punched into a circular sheet with a diameter of 12 mm. In the glove box, the positive electrode sheet is assembled into a CR2032 button cell together with a metal lithium sheet, a diaphragm (Celgard2400) and an A007 electrolyte. The assembled button cell is left to stand at 25°C for 12 hours before the electrochemical performance test.
[0119] The test conditions for capacity performance are: 2.8-4.3V, 0.1C@25℃.
[0120] The test conditions for cycle performance are: 3.0-4.5V, 0.5C / 1C@25℃.
[0121] The test conditions for rate performance are: 2.8-4.3V, 0.33C@25℃.
[0122] The test results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] analyze:
[0127] It can be seen from the above table that the ultra-high nickel polycrystalline positive electrode material provided by the present invention has good structural stability and low surface residual alkali content, eliminating the defects of complex and difficult to control water washing process and low electrical performance, and has excellent capacity, cycle and rate performance.
[0128] It can be seen from Example 1 and Examples 4-5 that if the first stage of calcination is not performed in step (1), the primary particles are uneven and the residual alkali is high; if the second stage of calcination is not performed in step (1), the primary particles are small and the residual alkali is very high, and a jelly phenomenon will occur in the later battery production.
[0129] It can be seen from Examples 1 and 6-7 that if the mass ratio of the Co-containing material to the solid electrolyte is too small, the residual lithium is too high, and the capacity and cycle deviations are; if the mass ratio of the Co-containing material to the solid electrolyte is too large, the capacity is reduced and the safety deviations are.
[0130] It can be seen from Example 1 and Examples 8-9 that if the doping amount of the Sr element is too small, the cycle performance of the material will deteriorate; if the doping amount of the Sr element is too large, the capacity performance of the material will deteriorate.
[0131] It can be seen from Example 1 and Examples 10-11 that if the doping amount of the Sb element is too small, the capacity performance of the material will be reduced; if the doping amount of the Sb element is too large, the cycle performance of the material will deteriorate.
[0132] It can be seen from Example 1 and Comparative Examples 1-3 that if there is no Li-containing material in the coating layer, the capacity performance of the material will be reduced; if there is no Co-containing material in the coating layer, the residual alkali on the surface of the material will increase and the cycle performance will deteriorate; if there is no solid electrolyte in the coating layer, the ionic conductivity of the material will deteriorate.
[0133] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An ultra-high nickel polycrystalline positive electrode material, characterized in that: The ultra-high nickel positive electrode material comprises a positive electrode material body and a coating layer coated on the surface of the positive electrode material body; The chemical formula of the positive electrode material is LiNi x Co y Mn 1-x-y O2, where 0.9≤x<1, 0<y≤0.06; The positive electrode material body is doped with an A element and a B element, wherein the A element includes any one of Zr, Sr, Ce, La, Al, Mg, Na, Ca, Y or Sn or a combination of at least two thereof, and the B element includes any one of Sb, W, Nb, Mo, Ti or P or a combination of at least two thereof; The materials in the coating layer include Li-containing material, Co-containing material and solid electrolyte.
2. The ultra-high nickel polycrystalline positive electrode material according to claim 1, characterized in that: The particle size D50 of the positive electrode material body is 2-5 μm; Preferably, the coating layer has a thickness of 10-100 nm; Preferably, the surface residual alkali compounds of the ultra-high nickel polycrystalline positive electrode material include LiOH and Li2CO3, the content of LiOH is ≤5500ppm, and the content of Li2CO3 is ≤3500ppm.
3. The ultra-high nickel polycrystalline positive electrode material according to claim 1 or 2, characterized in that: The Li-containing material includes any one or a combination of at least two of Li3N, Li2S, LiF, Li2NiO2, Li2O or Li2O2; Preferably, the Co-containing material includes any one or a combination of at least two of Co(OH)2, CoOOH, CoF2 or CoO; Preferably, the solid electrolyte comprises any one of LLZO, LLZTO, LATP or LASTP, or a combination of at least two thereof; Preferably, the mass ratio of the Li-containing material, the Co-containing material and the solid electrolyte is (1-4):(1-4):(1-6).
4. A method for preparing the ultra-high nickel polycrystalline positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, a compound containing element A, and a compound containing element B, and then calcining the mixture to obtain a calcined product; (2) mixing the calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent, and performing secondary calcination to obtain the ultra-high nickel polycrystalline positive electrode material; Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y (OH)2, wherein 0.9≤x<1, 0<y≤0.
06.
5. The preparation method according to claim 4, characterized in that: The lithium source in step (1) comprises any one of LiOH, Li2CO3, LiNO3, Li3N, Li2S, LiF, Li2NiO2, Li2O or Li2O2, or a combination of at least two thereof; Preferably, the compound containing element A in step (1) comprises any one or a combination of at least two of carbonate, nitrate, sulfate, chloride or oxide containing element A; Preferably, the compound containing element B in step (1) comprises any one or a combination of at least two of carbonate, nitrate, sulfate, chloride or oxide containing element B; Preferably, the mass of the element A in the element A-containing compound in step (1) is 0.05-0.3wt% of the mass of the ultra-high nickel positive electrode material precursor; Preferably, the mass of the B element in the B-containing compound in step (1) is 0.1-0.5wt% of the mass of the ultra-high nickel positive electrode material precursor.
6. The preparation method according to claim 4 or 5, characterized in that: The primary calcination in step (1) is carried out in an oxygen-containing atmosphere; Preferably, the oxygen-containing atmosphere is an air atmosphere or a pure oxygen atmosphere; Preferably, the primary roasting in step (1) is carried out in a multi-stage roasting manner, including a primary roasting and a secondary roasting; Preferably, the temperature of the first stage calcination is 450-550°C and the time is 3-10h; Preferably, the temperature of the second stage calcination is 700-800°C and the time is 6-15h.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The secondary calcination in step (2) is carried out in an oxygen-containing atmosphere, wherein the oxygen-containing atmosphere is an air atmosphere or a pure oxygen atmosphere; Preferably, the temperature of the secondary calcination in step (2) is 600-800° C. and the time is 5-10 h.
8. The preparation method according to any one of claims 4 to 7, characterized in that: Based on the mass of the calcined product in step (2), the content of the Li-containing coating agent is 0.5-2wt%, the content of the Co-containing coating agent is 0.5-2wt%, and the content of the solid electrolyte coating agent is 0.5-3wt%.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: (1) mixing an ultra-high nickel positive electrode material precursor, a lithium source, a compound containing element A and a compound containing element B to obtain a primary mixture, and then calcining the primary mixture in an oxygen-containing atmosphere, that is, first heating the temperature to 450-550° C. at a heating rate of 3-5° C. / min for a first-stage calcination, keeping the temperature for 3-10 hours, then heating the temperature to 700-800° C. at a heating rate of 1-3° C. / min for a second-stage calcination, keeping the temperature for 6-15 hours, and finally cooling the temperature to room temperature at a rate of 3-5° C. / min, and obtaining a calcined product after pulverization; Among them, the chemical formula of the ultra-high nickel cathode material precursor is Ni x Co y Mn 1-x-y (OH)2, where 0.9≤x<1, 0<y≤0.06; (2) The calcined product, the Li-containing coating agent, the Co-containing coating agent and the solid electrolyte coating agent are stirred and mixed to obtain a secondary mixture, and then the secondary mixture is secondary calcined in an oxygen-containing atmosphere, that is, the temperature is increased to 600-800°C at a heating rate of 3-5°C / min, kept warm for 5-10h, and then cooled to room temperature at a rate of 3-5°C / min to obtain the ultra-high nickel polycrystalline positive electrode material.
10. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery includes the ultra-high nickel polycrystalline positive electrode material as described in any one of claims 1 to 3.
Citation Information
Cited By
Composite positive electrode material and preparation method and application thereof
CN119092696A
A composite positive electrode material and its preparation method and application
CN119092696B
Ultrahigh-nickel single-crystal positive electrode material as well as preparation method and application thereof
CN119581549A